A doped diamond particle sensor and its preparation method and application

By depositing a polycrystalline boron-doped diamond film on the surface of single-crystal structure boron-containing diamond particles or diamond particles and combining it with metal modification, the problems of uneven resistance and impurities in boron-doped diamond electrodes are solved, and the conductive performance and detection sensitivity are improved, achieving for efficient electrochemical detection.

CN113804734BActive Publication Date: 2024-10-01HU-NAN NEW FRONTIER SCI & TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111078508.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-15
Publication Date
2024-10-01
Estimated Expiration
2041-09-15

AI Technical Summary

Technical Problem

Existing boron-doped diamond electrodes have problems such as uneven resistance, high metal impurities, low electrocatalytic activity, poor selectivity and sensitivity, and difficulty in mass production, which limits their application.

Method used

Boron-containing diamond particles or diamond particles with a single crystal structure are used as carrier particles, and a boron-doped diamond film with a polycrystalline structure is deposited on the surface and prepared by high temperature and high pressure method and chemical vapor deposition technology. The doping concentration and film thickness are controlled, combined with metal modification. layer to improve electrocatalytic activity.

Benefits of technology

It significantly improves the conductive performance and specific surface area, reduces the adsorption of substances by the electrode, improves the detection sensitivity and signal-to-noise ratio, and achieves efficient electrochemical detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113804734B_ABST
    Figure CN113804734B_ABST
Patent Text Reader

Abstract

The invention discloses a doped diamond particle sensor and a preparation method and application thereof. The doped diamond particle sensor comprises a working electrode, a counter electrode and a reference electrode. The working electrode is composed of a glass tube, a copper wire encapsulated in the glass tube, and doped diamond particles connected to the copper wire and exposed to the outside. The doped diamond particles comprise carrier particles and a coating layer. The carrier particles are boron-containing diamond particles or pure diamond particles. The coating layer is a doped diamond film, wherein the doping elements are selected from one or more of boron, nitrogen and phosphorus. The invention uses single-crystal structure diamond particles or boron-containing diamond particles synthesized under high temperature and high pressure as carrier particles, and grows a polycrystalline doped diamond film on the surface thereof. The doped diamond particles finally obtained have excellent electrical conductivity. The manufactured sensor has good linear response and high detection sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diamond electrode preparation, and in particular relates to a doped diamond particle sensor and a preparation method and application thereof. Background Art

[0002] Artificial diamond is a superhard material, but it has very few applications in other areas. After boron doping, the resistance of diamond can be greatly reduced. At present, the boron-doped diamond mainly includes single crystal and polycrystalline boron-containing diamond particles, as well as boron-doped diamond films. Among them, boron-containing gold diamond particles are mainly prepared by high temperature and high pressure method. The particles prepared by this method are mainly single crystal diamond, which has the problems of uneven B concentration distribution and low B concentration. In addition, because metals such as Ni and Fe are needed as catalysts in the preparation process, the prepared particle electrodes contain more metal impurities, which to some extent affects the quality of BDD particles.

[0003] Although the existing BDD materials are mostly based on metal or silicon wafers, they have some fatal defects as BDD substrate materials, due to their wide potential window, good chemical stability and weak surface adsorption. The metal matrix has the advantages of high strength, good toughness and strong plasticity, but as the matrix of the electrode, it has the problems of poor corrosion resistance and high thermal expansion coefficient. In addition, the existing BDD electrodes have the disadvantages of low electrocatalytic activity, poor selectivity and sensitivity, and difficulty in large-scale production, which limits their application. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention aims to provide a doped diamond particle sensor and a preparation method and application thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solution.

[0006] The present invention discloses a doped diamond particle sensor, comprising a working electrode, a counter electrode and a reference electrode, wherein the working electrode is composed of a glass tube, a copper wire encapsulated in the glass tube, and doped diamond particles connected to the copper wire and exposed to the outside; the doped diamond particles include carrier particles and a coating layer, wherein the carrier particles are boron-containing diamond particles or pure diamond particles, and the coating layer is a doped diamond film, wherein the doping element is selected from one or more of boron, nitrogen and phosphorus, preferably boron.

[0007] In a preferred embodiment, the carrier particles are of a single crystal structure, and the doped diamond film is of a polycrystalline structure.

[0008] The inventors have found that using single-crystal boron-containing diamond particles or diamond particles as carrier particles and then depositing a polycrystalline boron-doped diamond film on their surface can greatly improve the conductivity of the boron-containing diamond particles or diamond particles.

[0009] In the present invention, the carrier particles used can be natural or artificially synthesized, and are preferably prepared by high temperature and high pressure to reduce costs.

[0010] In a preferred embodiment, the concentration of the doping element in the doped diamond film is greater than 10 21 cm -3 , preferably 10 21 cm -3~ 10 22 cm -3 .

[0011] When the content of the doped diamond film is controlled within the above range, the performance of the finally obtained doped diamond particles is optimal. This is because when the doping concentration is greater than 10 18 cm -3 When the insulating diamond has semiconductor properties, when it is greater than 10 21 cm -3 When the doping element is too high, metal-like properties can be obtained. However, due to the different lattice coefficients of the doping element and diamond, excessive doping will cause the diamond lattice to be destroyed and produce impurity phases (such as sp 2 )), resulting in the loss of some excellent properties of diamond such as high hardness, high strength and inert surface. Controlling the doping concentration in the doped diamond film within the above range will achieve optimal performance in collaboration with the carrier particles.

[0012] In a preferred solution, the particle size of the carrier particles is 100 nm-500 μm, preferably 100 nm-300 μm, and more preferably 100 nm-100 μm, and the thickness of the doped diamond film is 5 μm-20 μm.

[0013] The inventors found that when the size of the carrier particles is less than 100 μm, the microelectrode effect can be achieved, which has a higher detection sensitivity. However, when the electrode size is greater than 100 μm and less than 300 μm, the preparation method can be simplified to a certain extent while having better detection performance. Therefore, the size can be selected according to the actual application.

[0014] The inventors have found that by setting the thickness of the doped diamond film within the above range, completely uniformly coated doped diamond particles with the best performance can be obtained.

[0015] Preferably, the doping method of the doped diamond film includes one or more combinations of constant doping, multi-layer variable doping, and gradient doping.

[0016] In a preferred solution, the diameter of the copper wire is 100 μm-300 μm. The inventors have found that controlling the diameter of the copper wire within the above range is convenient for installation with doped diamond particles and has high detection sensitivity.

[0017] In a preferred embodiment, the doped diamond film is a doped diamond film with a porous structure, and the diameter of the holes in the doped diamond film is 10 nm-200 nm.

[0018] Providing micropores on the surface of the doped diamond film can further increase the specific surface area of ​​the particles and improve their performance.

[0019] In a preferred embodiment, a modification layer is disposed on the surface of the coating layer, and the modification layer is selected from one or more combinations of metal modification layer, organic modification, and end group modification.

[0020] By providing a modification layer on the surface of the coating layer, the electrocatalytic activity of the modified layer particles can be further improved.

[0021] Further preferably, a metal modification layer is provided on the surface of the coating layer, and the metal in the metal modification layer is selected from at least one of iron, copper, platinum, silver and gold.

[0022] The inventors found that the introduction of metal modification can not only further improve the electrochemical catalytic performance, but also different metals have different electrochemical activities for different substances. Therefore, different metal modifications can be selected according to different applications, such as Au detection of -DA molecules, such as modified Ni detection of glucose.

[0023] The present invention provides a method for preparing a doped diamond particle sensor, comprising the following steps:

[0024] Step 1 Preparation of doped diamond particles

[0025] First, nano-diamond seed crystals are planted on the surface of carrier particles, and then the carrier particles planted with diamond seed crystals are subjected to chemical vapor deposition to grow doped diamond films to obtain doped diamond particles. During the chemical vapor deposition, the mass flow ratio of the gas is hydrogen: methane: doping gas source = 98:2:0.3-0.6, the growth pressure is 2-5Kpa, the growth temperature is 800-850°C, the growth times are 2-6 times, preferably 5 times, each time the growth is performed, the carrier particles are taken out, the carrier particles are shaken, and then the growth is continued. The single growth time is 3-6h, and the doping gas source is selected from at least one of ammonia, phosphine, and boron.

[0026] Step 2: Packaging of working electrode

[0027] The doped diamond particles prepared in step 1 are connected to the metal wire using conductive silver glue. After drying, the copper wire is inserted into the glass tube, and the glass tube is thinned using a microelectrode pulling instrument. The copper wire and the conductive silver glue are partially sealed into the obtained glass tube, leaving only the doped diamond particles exposed outside the glass tube. Finally, an adhesive is dripped into the glass tube to fill the front section of the glass tube, and dried to obtain a working electrode.

[0028] Step 3

[0029] The doped diamond particle sensor is obtained by combining the working electrode, the reference electrode and the counter electrode.

[0030] In the step 1 of the present invention, during the preparation of the doped diamond particles, since the carrier particles and the doped diamond film have similar structures and are easy to nucleate, conventional chemical vapor deposition methods can be used to grow excellent doped diamond films. However, the inventors have found that the carrier particles can be better coated by cooling down every 3-6 hours of growth, taking out the carrier particles, and then heating up to the target temperature and growing them in multiple times, and the performance of the boron-doped diamond particles finally obtained is optimal.

[0031] In a preferred embodiment, in step 1, the process of planting nano-diamond seed crystals on the surface of the carrier particles is as follows: immersing the carrier particles in a suspension containing nano-diamonds and ultrasonically vibrating for ≥30 minutes, and finally washing and drying. The mass fraction of nano-diamonds in the suspension containing nano-diamonds is 0.01-0.1wt%.

[0032] In a preferred embodiment, in step one, the chemical vapor deposition is hot wire chemical vapor deposition, and the temperature of the hot wire is 2500-2700°C.

[0033] In a preferred solution, in step 1, the doped diamond particles are etched to obtain a doped diamond film with a porous structure; the etching process is: firstly sputtering metal nickel on the surface of the doped diamond film by magnetron sputtering, and then performing heat treatment.

[0034] In addition, according to the actual application situation, after the heat treatment, boiling nitric acid solution can be used to remove the nickel particles in the pores.

[0035] Further preferably, the process parameters of sputtering metal nickel are: the gas pressure is adjusted to 1-3 Pa by introducing argon gas, the sputtering current is 250-350 mA, and the sputtering time is 10-30 s; the thickness of the sputtered Ni layer is 5-10 nm, and the gas pressure is maintained at 7-15 kPa.

[0036] Further preferably, the temperature of the heat treatment is 800-900° C., the time of the heat treatment is 3-5 hours, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5.

[0037] Further preferably, the nitric acid solution is a mixture of concentrated nitric acid and water in a volume ratio of 1 to 4:4.

[0038] In step 2 of the present invention, the secondary drying temperature is 60°C for 3 hours.

[0039] In step 2 of the present invention, the adhesive used is preferably 502 glue, and the 502 glue is dripped into the glass tube to fill the front part of the glass tube to prevent the exposure of the conductive silver glue and make the particles and the glass tube more tightly connected.

[0040] In a preferred embodiment, in step 2, metal particles are modified on the surface of the doped diamond particles exposed in the obtained working electrode.

[0041] Further preferably, when the modified metal particles are selected from Au, a sodium acetate buffer solution with a pH value of 4.5-5.5 and containing 5-50 mM chloroauric acid is used as the deposition solution, and an electrochemical workstation is used to select a pulse multi-potential deposition method to deposit the particle electrode. The on-time is 0.6-0.8s, the on-potential is -0.5V--1V, the off-time is 0.4-0.2s, and the off-voltage is 0V, so as to obtain Au nanoparticles of 10-500nm on the surface of the doped diamond particles.

[0042] In a preferred embodiment, in step 2, end group modification is performed on the surface of the doped diamond particles exposed at the obtained working electrode. The modification process is to place the doped diamond particles exposed at the obtained working electrode in a 0.1-1MH2SO4 solution, apply a voltage of -3--3.5V, and react for 2-10min to obtain H end group modification.

[0043] In a preferred embodiment, in step 2, end group modification is performed on the surface of the doped diamond particles exposed at the obtained working electrode. The modification process is to place the doped diamond particles exposed at the obtained working electrode in a 0.1-1MH2SO4 solution, apply a voltage of 3-3.5V, react for 2-10min, and perform O end group modification.

[0044] The present invention also provides an application of a doped diamond particle sensor, which uses the doped diamond particle sensor for electrochemical detection.

[0045] Beneficial Effects

[0046] The present invention is the first to use diamond particles or boron-containing diamond particles synthesized at high temperature and high pressure as carrier particles, and grow polycrystalline doped diamond films on their surfaces. The resulting doped diamond particles have excellent conductivity, high specific surface area, and are non-toxic to the environment and have a high signal-to-noise ratio. In addition, because commercial particle electrodes contain impurities such as Fe and Ni, they are easy to adsorb substances. The polycrystalline film produced is mainly composed of sp 3The diamond phase of the saturated structure has a chemically inert surface and is not easy to adsorb other substances. The surface of the BDD particle microelectrode is a polycrystalline BDD film, which does not contain metal impurity phases, has low capacitance, high signal-to-noise ratio, and the sensor has good linear response and high detection sensitivity.

[0047] The present invention adopts a vapor deposition method in the growth process. Taking a boron-doped diamond film as an example, vapor deposition is used to prepare polycrystalline diamond by introducing hydrocarbons such as methane (CH4), acetylene, hydrogen (H2) and borane into a reaction chamber. The gas concentration is adjustable and the ratio is uniform. Therefore, the boron-doped diamond film prepared by the vapor deposition method has high B doping uniformity and is easy to prepare a highly doped film. The present invention adopts a multiple growth method and effectively controls the crystal structure, the thickness of the film, and the doping amount, so that the performance of the obtained doped diamond particles is ultimately the best.

[0048] The preparation method of the invention is simple and controllable, and the carrier particles used are diamond particles or boron-containing diamond particles with a single crystal structure synthesized under high temperature and high pressure, which are commercially available, and are inexpensive and low in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 The microstructure of the boron-doped diamond particles prepared in Example 1, wherein Figure 1 (a) is a SEM image of a single-crystal boron-containing diamond coated with a polycrystalline B-doped diamond film. (b) is a magnified image of a polycrystalline boron-doped diamond film. (c) is a Raman spectrum of a polycrystalline diamond film.

[0050] Figure 2 The microstructure of the boron-doped diamond particles prepared in Example 2, wherein Figure 1 (a) is a SEM image of a single-crystal boron-containing diamond coated with a polycrystalline B-doped diamond film. (b) is a magnified image of a polycrystalline boron-doped diamond film. (c) is a Raman spectrum of a polycrystalline diamond film.

[0051] Figure 3 The microstructure of the boron-doped diamond particles prepared in the comparative example.

[0052] Figure 4 Schematic diagram of the doped diamond particle sensor in the present invention, in which: 1, carrier particles; 2, doped diamond film; 3, copper wire; 4, glass tube; 5, copper wire. DETAILED DESCRIPTION

[0053] Example 1

[0054] Preparation of Boron-doped Diamond Particles

[0055] (1) First, the boron-containing diamond particles with an average particle size of 150 μm are cleaned.

[0056] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. The nano-diamonds are placed in the suspension containing nano-diamonds, and the mass fraction of the nano-diamonds is 0.01 wt%.

[0057] (3) A boron-doped diamond film was deposited by hot-wire CVD, and the deposition process parameters were as follows: hot-wire distance 6 mm, growth temperature 800-850°C, hot-wire temperature 2200°C, deposition pressure 3 KPa, and a diamond film thickness of 50 μm was obtained by controlling the deposition time; during the chemical vapor deposition, the mass flow ratio of the gas was hydrogen: methane: borane = 98:2:0.3, the growth pressure was 2 KPa, and the number of growths was 2 times. After each growth, the carrier particles were taken out, and the carrier particles were shaken before continuing to grow. The single growth time was 6 hours.

[0058] Figure 1 (a) is the SEM image of a single crystal B-doped diamond coated with a polycrystalline B-doped diamond film. (b) is the magnified image of the polycrystalline film. (c) is the Raman peak of the polycrystalline diamond film with a high B-doping degree, showing a typical B peak (479 cm -1 and 1200cm -1 ), less graphite phase (G peak: 1530cm -1 ), and the concentration of B is greater than 10 21 cm -1 , indicating that it is a heavily B-doped material.

[0059] Electrode packaging

[0060] Dip the copper wire (100 μm in diameter) into the conductive silver glue, connect the washed boron-doped diamond particles with the conductive silver glue and the copper wire, put them into the oven, and dry them at 60° for 3 hours. After drying, insert the copper wire into the glass tube, and use a microelectrode puller to thin the glass tube, partially seal the copper wire and the conductive silver glue into the glass tube, and only expose the doped diamond particles outside the glass tube. Drip 502 glue into the glass tube and fill the front part of the glass tube to prevent the exposure of the conductive silver glue and make the particles and the glass tube more tightly connected. Put it in the oven and dry it at 60° for 1 hour.

[0061] Electrode modification

[0062] Nickel nanoparticles were sputtered on the sample by magnetron sputtering on a physical vapor deposition device, with argon gas introduced to adjust the gas pressure to about 1 Pa, the sputtering current to 200 mA, and the sputtering time to 15 s.

[0063] The electrochemical potential window of the Ni-modified boron-doped diamond particle microelectrode obtained in this example is as high as 3.1V; using glucose detection: it has a good linear response in the concentration range of 0.05-15μM, and the detection sensitivity is as high as 140μA·μM-1·cm-2.

[0064] Example 2

[0065] (1) First, the boron-containing diamond particles with an average particle size of 300 μm are cleaned.

[0066] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. Putting into the suspension containing nano-diamonds, the mass fraction of nano-diamonds is 0.1wt%.

[0067] (3) Boron-doped diamond film was deposited by hot wire CVD. The deposition process parameters were as follows: hot wire distance 6 mm, growth temperature 800-850°C, hot wire temperature 2200°C, deposition pressure 4 KPa, gas ratio hydrogen: methane: borane = 98:2:0.5. By controlling the deposition time, the diamond film thickness of 10 μm was obtained. The number of growths was 4 times. After each growth, the carrier particles were taken out and shaken before continuing to grow. The single growth time was 4 hours.

[0068] Figure 2 (a) is the SEM image of a single crystal B-doped diamond coated with a polycrystalline B-doped diamond film. (b) is the magnified image of the polycrystalline film. (c) is the Raman peak of the polycrystalline diamond film, where the typical B peak (479 cm -1 and 1200cm -1 ), the graphite phase is less (G peak: 1530cm-1), and the B concentration is greater than 10 after fitting. 21 cm -1 , indicating that it is a heavily B-doped material.

[0069] Electrode packaging

[0070] Dip the copper wire (200 μm in diameter) into the conductive silver glue, connect the washed boron-doped diamond particles with the conductive silver glue and the copper wire, put them into the oven, and dry them at 60° for 3 hours. After drying, insert the copper wire into the glass tube, and use a microelectrode puller to thin the glass tube, partially seal the copper wire and the conductive silver glue into the glass tube, and only expose the doped diamond particles outside the glass tube. Drip 502 glue into the glass tube and fill the front part of the glass tube to prevent the exposure of the conductive silver glue and make the particles and the glass tube more tightly connected. Put it in the oven and dry it at 60° for 1 hour.

[0071] Au was deposited on the particle electrode using an electrochemical deposition workstation. 0.5 mM chloroauric acid solution was placed in the particle electrode and the electrodeposition was performed at a voltage of -0.5 V for 120 s using a pulsed electro-deposition method.

[0072] The electrochemical potential window of the Au-modified boron-doped diamond particle microelectrode obtained in this example is as high as 3V; using dopamine for detection: it has a good linear response in the concentration range of 0.05-16μM, and the detection sensitivity is as high as 205μA·μM-1·cm-2.

[0073] Example 3

[0074] (1) First, the boron-containing diamond particles with an average particle size of 300 μm are cleaned.

[0075] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. Putting into the suspension containing nano-diamonds, the mass fraction of nano-diamonds is 0.1wt%.

[0076] (3) Boron-doped diamond film was deposited by hot-filament CVD. The deposition process parameters were as follows: hot-filament distance 6 mm, growth temperature 800-850°C, hot-filament temperature 2200°C, deposition pressure 4 KPa, gas ratio hydrogen: methane: borane = 98:2:0.6. By controlling the deposition time, a diamond film thickness of 10 μm was obtained. The number of growths was 5 times. After each growth, the carrier particles were taken out and shaken before continuing the growth. The single growth time was 3 h.

[0077] (4) Etching the boron-doped diamond particles to obtain a porous boron-doped diamond film; the etching process is: sputtering metal nickel on the surface of the boron-doped diamond film by magnetron sputtering, the process parameters of sputtering metal nickel are: adjusting the gas pressure to 3Pa by introducing argon gas, sputtering current 350mA, sputtering time 10s; the thickness of the sputtered Ni layer is 7nm, and then heat treatment is performed, the gas pressure is maintained at 12kpa, the heat treatment temperature is 900℃, the heat treatment time is 3h, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.5. After the heat treatment is completed.

[0078] Electrode packaging

[0079] Dip the copper wire (300μm in diameter) into the conductive silver glue, connect the washed boron-doped diamond particles with the conductive silver glue and the copper wire, put them into the oven, and dry them at 60° for 3h. After drying, insert the copper wire into the glass tube, and use a microelectrode puller to thin the glass tube, partially seal the copper wire and the conductive silver glue into the glass tube, and only expose the doped diamond particles outside the glass tube. Drip 502 glue into the glass tube and fill the front part of the glass tube to prevent the exposure of the conductive silver glue and make the particles and the glass tube more tightly connected. Put it in the oven and dry it at 60° for 1h.

[0080] Au was deposited on the particle electrode using an electrochemical deposition workstation. 0.5 mM chloroauric acid solution was placed in the particle electrode and the electrodeposition was performed at a voltage of -0.5 V for 120 s using a pulsed electro-deposition method.

[0081] The electrochemical potential window of the Au-modified boron-doped diamond particle microelectrode obtained in this example is as high as 3V; using dopamine for detection: it has a good linear response in the concentration range of 0.1-1000 μM, and the detection sensitivity is as high as 390 μA·μM-1·cm-2.

[0082] Comparative Example 1

[0083] (1) Diamond particles with an average particle size of 150 μm are cleaned.

[0084] (2) Immersing in a suspension containing nano-diamonds and ultrasonically vibrating for 30 minutes, cleaning and drying. The nano-diamonds are placed in the suspension containing nano-diamonds, and the mass fraction of the nano-diamonds is 0.01 wt%.

[0085] (3) Boron-doped diamond film was deposited by hot-filament CVD. The deposition process parameters were as follows: hot-filament distance 7 mm, growth temperature 800-900°C, hot-filament temperature 2200°C, deposition pressure 3 KPa, gas mass flow ratio of hydrogen:methane:borane = 98:2:0.3, growth pressure 2 KPa, and continuous growth for 6 h.

[0086] Figure 3 This is a SEM image of diamond particles coated with polycrystalline B-doped diamond film. Due to the lack of continuous growth, some areas on the surface are not completely coated.

Claims

1. A method for preparing a doped diamond particle sensor, characterized in that: The steps include: Step 1 Preparation of doped diamond particles First, nano-diamond seed crystals are planted on the surface of carrier particles, and then the carrier particles planted with diamond seed crystals are subjected to chemical vapor deposition to grow doped diamond films to obtain doped diamond particles. During the chemical vapor deposition, the mass flow ratio of the gas is hydrogen: methane: doping gas source = 98:2:0.3-0.6, the growth pressure is 2-5Kpa, the growth temperature is 800-850°C, the growth times are 2-6 times, and after each growth, the carrier particles are taken out, shaken, and then continued to grow. The single growth time is 3-6 hours, and the doping gas source is selected from at least one of ammonia, phosphine, and borane; Step 2: Packaging of working electrode The doped diamond particles prepared in step 1 are connected to the metal wire using conductive silver glue. After drying, the copper wire is inserted into the glass tube, and the glass tube is thinned using a microelectrode pulling instrument. The copper wire and the conductive silver glue are partially sealed into the obtained glass tube, leaving only the doped diamond particles exposed outside the glass tube. Finally, an adhesive is dripped into the glass tube to fill the front section of the glass tube, and dried to obtain a working electrode. Step 3 The doped diamond particle sensor is obtained by combining the working electrode, the reference electrode and the counter electrode; The doped diamond particle sensor comprises a working electrode, a counter electrode and a reference electrode, wherein the working electrode is composed of a glass tube, a copper wire encapsulated in the glass tube, and doped diamond particles connected to the copper wire and exposed to the outside; the doped diamond particles comprise carrier particles and a coating layer, wherein the carrier particles are boron-containing diamond particles, and the coating layer is a doped diamond film, wherein the doping element is selected from one or more of boron, nitrogen and phosphorus; The carrier particles are of a single crystal structure, and the doped diamond film is of a polycrystalline structure; The concentration of the doping element in the doped diamond film is 10 21 cm -3~ 10 22 cm -3 .

2. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: In step 1, the process of planting nano-diamond seed crystals on the surface of the carrier particles is as follows: immersing the carrier particles in a suspension containing nano-diamonds and ultrasonically vibrating for ≥30 minutes, and finally washing and drying. The mass fraction of nano-diamonds in the suspension containing nano-diamonds is 0.01-0.1wt%; In step 1, the chemical vapor deposition is hot wire chemical vapor deposition, and the temperature of the hot wire is 2500-2700°C.

3. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: In step 1, the doped diamond particles are etched to obtain a doped diamond film with a porous structure; the etching process is: firstly sputtering metal nickel on the surface of the doped diamond film by magnetron sputtering method, and then performing heat treatment; The process parameters of the sputtering of metal nickel are: the pressure of argon gas is adjusted to 1-3 Pa, the sputtering current is 250-350 mA, and the sputtering time is 10-30 s; the thickness of the sputtered Ni layer is 5-10 nm, and the pressure is maintained at 7-15 kPa. The heat treatment temperature is 800-900° C., the heat treatment time is 3-5 hours, and the mass flow ratio of the introduced atmosphere is H2:Ar=1.

5.

4. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: In step 2, metal particles are modified on the surface of the doped diamond particles exposed in the obtained working electrode. When the modified metal particles are selected from Au, a sodium acetate buffer solution with a pH value of 4.5-5.5 containing 5-50 mM chloroauric acid is used as a deposition solution, and an electrochemical workstation is used to select a pulse multi-potential deposition method to deposit the particle electrode, with a turn-on time of 0.6-0.8 s, a turn-on potential of -0.5V - -1 V, a turn-off time of 0.4-0.2s, and a turn-off voltage of 0V, that is, 10-500 nm Au nanoparticles are modified on the surface of the doped diamond particles; or In step 2, the exposed surface of the doped diamond particles of the obtained working electrode is subjected to end group modification. The modification process is to place the exposed doped diamond particles of the obtained working electrode in a 0.1-1M H2SO4 solution, apply a voltage of -3- -3.5V, and react for 2-10min to obtain H end group modification; or In step 2, end group modification is performed on the surface of the doped diamond particles exposed in the obtained working electrode. The modification process is to place the doped diamond particles exposed in the obtained working electrode in a 0.1-1M H2SO4 solution, apply a voltage of 3-3.5V, react for 2-10min, and perform O end group modification.

5. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: The particle size of the carrier particles is 100nm-500μm, and the thickness of the doped diamond film is 5μm-20μm; The doping method of the doped diamond film includes one or more combinations of constant doping, multi-layer variable doping, and gradient doping.

6. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: The diameter of the copper wire is 100 μm-300 μm.

7. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: The concentration of the doping element in the doped diamond film is greater than 10 21 cm -3 .

8. The method for preparing a doped diamond particle sensor according to claim 1, characterized in that: The doped diamond film is a doped diamond film with a porous structure, and the pore diameter of the pores in the doped diamond film is 10nm-200nm; The surface of the coating layer is provided with a modification layer, and the modification layer is selected from one or more combinations of metal modification layer, organic modification, and end group modification.

9. Application of a doped diamond particle sensor prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The doped diamond particle sensor was used for electrochemical detection.