Radio wave absorber

By using an electric wave absorber composed of magnetic powder with a volume filling rate of less than 35% in the radar system, the problem of insufficient recognition accuracy of the radar system is solved, and the effect of improving radar direction and removing unnecessary radio wave components is achieved, which is enhanced. Reliability of autonomous driving control.

CN113875327BActive Publication Date: 2024-11-29FUJIFILM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080035479.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-08
Publication Date
2024-11-29
Estimated Expiration
2040-05-08

AI Technical Summary

Technical Problem

The existing radar systems have the problem of insufficient recognition accuracy when identifying objects, especially in vehicle-mounted radars, which are difficult to effectively improve the directionality of the radar and remove unnecessary radio wave components, affecting the reliability of autonomous driving control.

Method used

An electric wave absorber consisting of magnetic powder with a volume filling rate of less than 35%, including hexagonal ferrite and ε-ferrous oxide powder. The transmission attenuation amount and reflection attenuation amount are both higher than 8.0dB, and are used for radar radio waves. The front side of the transceiver unit is installed to improve the radar recognition accuracy.

Benefits of technology

By increasing the transmission and reflection attenuation of the radar, the directionality of the radar and the ability to selectively receive radio waves of the object are enhanced, the recognition accuracy of the radar is improved, unnecessary radio wave interference is reduced, and the reliability of autonomous driving control is enhanced. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003350833300000341
    Figure BDA0003350833300000341
Patent Text Reader

Abstract

The present invention provides a radio wave absorber comprising magnetic powder and a binder, wherein the volume filling rate of the magnetic powder in the radio wave absorber is 35 volume % or less, the transmission attenuation is 8.0 dB or more, and the reflection attenuation is 8.0 dB or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electromagnetic wave absorber. Background Art

[0002] As a radio wave absorber, there is known a radio wave absorber containing magnetic powder as a radio wave absorbing material. In addition, as a radio wave absorber containing magnetic powder, there is a radio wave absorber in which magnetic powder and a binder are mixed (see Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-56492 Summary of the invention

[0006] Technical issues to be solved by the invention

[0007] In recent years, radars for identifying objects by transmitting and receiving radio waves have attracted attention as electronic devices that use radio waves. For example, vehicle-mounted radars can identify the existence of objects, the distance to objects, etc. by transmitting radio waves and receiving radio waves reflected by objects (pedestrians, vehicles, etc.). In order to prevent collisions with objects, the car's automatic driving control system can automatically brake to stop the car as needed based on the results of radar identification of the object, or can automatically control the speed to maintain the distance from the object.

[0008] As described above, in order to improve the reliability of the system that performs various controls based on the results of radar recognition, it is expected to improve the performance of the radar. Therefore, in recent years, research has begun on providing a radio wave absorber on the front side (the incident side of the radio wave incident from the outside) of the radar's radio wave transceiver unit to improve the recognition accuracy.

[0009] In view of the above, an object of one aspect of the present invention is to provide a radio wave absorber that can contribute to improving the recognition accuracy of radar.

[0010] Means for solving technical problems

[0011] One aspect of the present invention relates to a radio wave absorber comprising magnetic powder and a binder, wherein:

[0012] The volume filling rate of the magnetic powder in the radio wave absorber is 35 volume % or less,

[0013] The transmission attenuation is 8.0dB or more, and

[0014] The reflection loss is 8.0dB or more.

[0015] In one embodiment, the volume filling rate of the magnetic powder may be 15 volume % or more and 35 volume % or less.

[0016] In one embodiment, the radio wave absorber may be a molded product obtained by molding a composition containing magnetic powder and a binder.

[0017] In one embodiment, the radio wave absorber may have a thickness of 2.0 mm to 10.0 mm.

[0018] In one embodiment, the magnetic powder may include hexagonal ferrite powder.

[0019] In one embodiment, the hexagonal ferrite may have a composition represented by Formula 1 below.

[0020] [Chemical formula 1]

[0021] Formula 1

[0022] AFe(12-x)Al x O 19

[0023] (In Formula 1, A represents at least one atom selected from the group consisting of Sr, Ba, Ca and Pb, and x satisfies 1.50≤x≤8.00.)

[0024] In one embodiment, in Formula 1, the atom represented by A may include Sr.

[0025] In one embodiment, the magnetic powder may include ε-iron oxide powder.

[0026] In one embodiment, the ε-iron oxide is ε-iron oxide containing one or more atoms selected from the group consisting of gallium atoms, titanium atoms, and cobalt atoms.

[0027] Effects of the Invention

[0028] According to one aspect of the present invention, it is possible to provide a radio wave absorber that can contribute to improving the recognition accuracy of radar. DETAILED DESCRIPTION

[0029] One aspect of the present invention relates to a radio wave absorber including magnetic powder and a binder, wherein the volume filling rate of the magnetic powder in the radio wave absorber is 35 volume % or less, the transmission attenuation is 8.0 dB or more, and the reflection attenuation is 8.0 dB or more.

[0030] In the present invention and this specification, "radio waves" refer to electromagnetic waves with a frequency of 3 MHz (THz) or less. A radio wave absorber has radio wave absorptivity. Radio wave absorptivity can be evaluated, for example, by transmission attenuation and / or reflection attenuation. It can be said that the higher the transmission attenuation value, the higher the reflection attenuation value, or the higher the transmission attenuation value and the reflection attenuation value, the better the radio wave absorptivity.

[0031] In order to improve the recognition accuracy of the radar, it is expected to improve the directivity of the radar. In addition, it is expected to improve the selectivity of the radar to selectively receive radio waves from the object by removing or reducing unnecessary radio wave components. Since the transmission attenuation and the reflection attenuation are respectively within the above ranges, the above-mentioned radio wave absorber can help improve the directivity of the radar and remove or reduce unnecessary radio wave components. For example, a vehicle-mounted radar, which has received attention in recent years, is a radar that uses radio waves in the millimeter wave frequency band. Millimeter waves are electromagnetic waves with a frequency of 30 GHz to 300 GHz. The above-mentioned radio wave absorber is a radio wave absorber that shows a transmission attenuation of 8.0 dB or more and a reflection attenuation of 8.0 dB or more for the frequency band of the radio wave, that is, for one or more frequencies in the frequency band below 3 MHz (THz). From the perspective of usefulness for improving the recognition accuracy of vehicle-mounted radar, the frequency representing the transmission attenuation of 8.0 dB or more and the reflection attenuation of 8.0 dB or more is preferably in the frequency band of millimeter waves, that is, one or more frequencies in the frequency band of 30 GHz to 300 GHz, more preferably one or more frequencies in the frequency band of 60 GHz to 90 GHz, and further preferably one or more frequencies in the frequency band of 75 GHz to 85 GHz. As an example, the above-mentioned radio wave absorber can be a radio wave absorber with a transmission attenuation of 8.0 dB or more in a frequency of 76.5 GHz and a reflection attenuation of 8.0 dB or more in a frequency of 76.5 GHz. This radio wave absorber is suitable as a radio wave absorber installed on the front side (the incident side of the radio wave incident from the outside) of the radio wave transceiver unit of the vehicle-mounted radar in order to reduce the side lobes of the vehicle-mounted millimeter wave radar.

[0032] In the present invention and this specification, "powder" refers to a collection of a plurality of particles. The so-called "collection" is not limited to a state in which the particles constituting the collection are in direct contact, but also includes a state in which a binder or the like is interposed between the particles.

[0033] [Transmission attenuation, reflection attenuation]

[0034] The transmission attenuation of the above-mentioned radio wave absorber is 8.0 dB or more. In order to improve the recognition accuracy of the radar, it is desired to improve the directivity of the radar. The transmission attenuation of 8.0 dB or more can help improve the directivity of the radar. From the viewpoint of further improving the directivity of the radar, the transmission attenuation of the above-mentioned radio wave absorber is preferably 8.5 dB or more, more preferably 9.0 dB or more, more preferably 10.0 dB or more, more preferably 10.5 dB or more, and more preferably 11.0 dB or more. In addition, the transmission attenuation of the above-mentioned radio wave absorber can be, for example, 15.0 dB or less, 14.5 dB or less, 14.0 dB or less, 13.5 dB or less, 13.0 dB or less, 12.5 dB or less, or 12.0 dB or less. However, from the viewpoint of improving the directivity of the radar, it is preferred that the transmission attenuation of the radio wave absorber is high. Therefore, the transmission attenuation of the above-mentioned radio wave absorber can exceed the value exemplified above.

[0035] In addition, the reflection attenuation of the above-mentioned radio wave absorber is 8.0dB or more. In order to improve the recognition accuracy of the radar, it is expected that the selectivity of the radar to selectively receive radio waves from the object is improved by removing or reducing unnecessary radio wave components with the radio wave absorber. The reflection attenuation of more than 8.0dB can help to remove or reduce unnecessary radio wave components. From this point of view, the reflection attenuation of the above-mentioned radio wave absorber is preferably more than 8.5dB, more preferably more than 9.0dB, more preferably more than 10.0dB, more preferably more than 10.5dB, and more preferably more than 11.0dB. And, the reflection attenuation of the above-mentioned radio wave absorber can be, for example, less than 18.0dB, less than 17.5dB, less than 17.0dB, less than 16.5dB, less than 16.0dB, less than 15.5dB or less than 15.0dB. However, from the viewpoint of removing or reducing unnecessary radio wave components, the reflection attenuation of the preferred radio wave absorber is high. Therefore, the reflection attenuation of the above-mentioned radio wave absorber can exceed the value exemplified above.

[0036] The "transmission attenuation" in the present invention and this specification is the value obtained by setting the incident angle to 0° and measuring the S parameter under the measurement environment of the ambient temperature of 15 to 35°C by the free space method, as the S21 of the S parameter. The "reflection attenuation" is the value obtained by the same measurement as the S11 of the S parameter. The measurement can be performed using a known vector network analyzer and a horn antenna. As a specific example of the measurement method, the method described in the embodiments described later can be cited.

[0037] For radio wave absorbers, a metal layer is sometimes stacked on the surface opposite to the surface on which radio waves are incident on the radio wave absorber (the so-called back surface). This type of radio wave absorber is called a matching type radio wave absorber. The matching type radio wave absorber can improve the reflection attenuation characteristics by setting a metal layer and utilizing phase difference absorption. In contrast, in the above-mentioned radio wave absorber, the radio wave absorber itself has excellent reflection attenuation characteristics. In detail, it is possible to show a reflection attenuation of more than 8.0 dB without relying on a metal layer. Radio wave absorbers used without stacking a metal layer on the back are generally called transmission type radio wave absorbers. In the previous transmission type radio wave absorbers containing magnetic powder and adhesive, usually, when trying to increase the transmission attenuation, the reflection attenuation tends to decrease. In contrast, the above-mentioned radio wave absorber can show a reflection attenuation of more than 8.0 dB without relying on a metal layer, and can show a transmission attenuation of more than 8.0 dB.

[0038] The "metal layer" described in this specification refers to a layer containing metal and substantially reflecting radio waves. However, when the above-mentioned radio wave absorber containing magnetic powder and adhesive contains metal, such radio wave absorber does not correspond to the above-mentioned metal layer. Here, the so-called "substantially reflecting radio waves" means, for example, reflecting more than 90% of the incident radio waves when radio waves are incident on the radio wave absorber in a state where the metal layer is stacked on the back of the radio wave absorber. As the form of the metal layer, metal plates, metal foils, etc. can be listed. For example, a metal layer formed on the back of the radio wave absorber by vapor deposition can be listed. The above-mentioned radio wave absorber can be used without a metal layer on the back. From the perspective of recycling and cost of the radio wave absorber, it is preferred to be able to use it without a metal layer. In addition, due to the deterioration of the metal layer, the peeling of the metal layer and the radio wave absorber, etc., the quality of the radio wave absorber used by stacking a metal layer on the back may be reduced. From the perspective of not causing such quality degradation, it is also preferred to be able to use it without a metal layer on the back.

[0039] [Volume filling rate of magnetic powder]

[0040] The above-mentioned radio wave absorber contains magnetic powder and adhesive. For the proportion of magnetic powder in the radio wave absorber, the volume filling rate is 35 volume % or less. The case where the volume filling rate of magnetic powder in the above-mentioned radio wave absorber is 35 volume % or less can mainly help to set the reflection attenuation of the radio wave absorber to 8.0 dB or more without relying on the metal layer. From the viewpoint of further improving the reflection attenuation characteristics of the radio wave absorber, the volume filling rate of the above-mentioned magnetic powder is preferably 33 volume % or less, more preferably 30 volume % or less, further preferably 28 volume % or less, and further preferably 25 volume % or less. On the other hand, the transmission attenuation can be controlled according to the proportion of magnetic powder in the radio wave absorber, the thickness of the radio wave absorber, the type of magnetic powder, etc. From the viewpoint of controlling the transmission attenuation, the volume filling rate of the above-mentioned magnetic powder is preferably 10 volume % or more, more preferably 12 volume % or more, and further preferably 15 volume % or more.

[0041] The volume filling rate is a volume-based content relative to 100 volume % of the total volume of the radio wave absorber. The volume filling rate of the magnetic powder in the radio wave absorber can be determined by the following method using a cross-sectional SEM image obtained using a scanning electron microscope (SEM).

[0042] A measurement sample having a square plane with a side of 5 mm is cut out from a randomly set position of the radio wave absorber to be measured. A sample for cross-sectional observation is prepared from the cut sample. The preparation of the sample for cross-sectional observation is performed by FIB (Focused Ion Beam) processing. The prepared sample for cross-sectional observation is observed by SEM, and a cross-sectional image (SEM image) is taken. As the SEM, a field emission scanning electron microscope (FE (Field Emission)-SEM) is used. Using FE-SEM, the sample for cross-sectional observation is set on the workbench in such a way that the cross section processed by FIB faces upward, and a cross-sectional SEM image with a field of view of 30μm×40μm is obtained under the conditions of an acceleration voltage of 15kV and an observation magnification of 3,000 times. The obtained cross-sectional SEM image is binarized, and the proportion of the magnetic powder (area basis) is calculated.

[0043] The above operation is performed on five measurement samples cut from different positions of the radio wave absorber to be measured, and the volume filling rate of the magnetic powder can be calculated as the arithmetic average of the five values ​​obtained. In addition, the element analysis of the cross-sectional observation sample can be performed as needed to determine the part of the magnetic powder in the cross-sectional SEM image.

[0044] Furthermore, the volume filling rate of the magnetic material in the radio wave absorber can be obtained, for example, by collecting magnetic powder from the radio wave absorber by a known method and calculating "(volume of collected magnetic powder / total volume of radio wave absorber) × 100". Here, the total volume of the radio wave absorber and the volume of the magnetic powder can be obtained by a known method. Alternatively, when the composition of the radio wave absorber-forming composition used to produce the radio wave absorber is known, the volume filling rate of the magnetic powder in the radio wave absorber can also be obtained from the known composition.

[0045] The volume filling rates of other components described in this specification can also be calculated in the same manner as above.

[0046] [Magnetic powder]

[0047] As the magnetic powder contained in the above-mentioned radio wave absorber, for example, powders of various magnetic materials such as ferrite, iron oxide, cobalt, and chromium oxide can be listed. The above-mentioned radio wave absorber may contain only one kind of magnetic powder, or may contain two or more different kinds of magnetic powders in any proportion. From the viewpoint of radio wave absorption performance, the magnetic powder is preferably a powder of hexagonal ferrite and a powder of ε-iron oxide. The type of magnetic material constituting the magnetic powder contained in the radio wave absorber can be confirmed by taking out the magnetic powder from the radio wave absorber by a known method and performing an X-ray diffraction analysis on the taken out magnetic powder. Alternatively, for example, it can also be confirmed by the following method. Cut a part or all of the radio wave absorber into small pieces, immerse it in a solvent (for example, acetone) for 1 to 2 days, and then dry it. The radio wave absorber after drying is further finely ground and subjected to X-ray diffraction analysis.

[0048] <Hexagonal ferrite powder>

[0049] In the present invention and this specification, "hexagonal ferrite powder" refers to a magnetic powder in which a hexagonal ferrite type crystal structure is detected as the main phase by X-ray diffraction analysis. The main phase refers to the structure to which the diffraction peak with the highest intensity in the X-ray diffraction spectrum obtained by X-ray diffraction analysis belongs. For example, when the diffraction peak with the highest intensity in the X-ray diffraction spectrum obtained by X-ray diffraction analysis belongs to the hexagonal ferrite type crystal structure, it is judged that the hexagonal ferrite type crystal structure is detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is taken as the main phase. The hexagonal ferrite type crystal structure contains at least iron atoms, divalent metal atoms and oxygen atoms as constituent atoms. Divalent metal atoms are metal atoms that can become divalent cations as ions, and examples thereof include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms. In the present invention and this specification, the powder of hexagonal strontium ferrite means that the main divalent metal atoms contained in the powder are strontium atoms, and the powder of hexagonal barium ferrite means that the main divalent metal atoms contained in the powder are barium atoms. The main divalent metal atoms refer to the divalent metal atoms that account for the largest proportion on an atomic % basis among the divalent metal atoms contained in the powder. However, the above-mentioned divalent metal atoms do not include rare earth atoms. The "rare earth atoms" in the present invention and this specification are selected from the group including scandium atoms (Sc), yttrium atoms (Y) and lanthanide atoms. The lanthanide atom is selected from the group consisting of lanthanum atom (La), cerium atom (Ce), praseodymium atom (Pr), neodymium atom (Nd), promethium atom (Pm), samarium atom (Sm), europium atom (Eu), gadolinium atom (Gd), terbium atom (Tb), dysprosium atom (Dy), holmium atom (Ho), erbium atom (Er), thulium atom (Tm), ytterbium atom (Yb) and lutetium atom (Lu).

[0050] In one embodiment, the hexagonal ferrite powder contained in the radio wave absorber may be a powder of a magnetoplumbite type (generally referred to as "M type") hexagonal ferrite. The magnetoplumbite type hexagonal ferrite has a composition formula of: AFe 12 O 19 Here, A can represent at least one atom selected from the group consisting of Sr, Ba, Ca and Pb, and also includes an embodiment in which two or more of these atoms are contained in any ratio.

[0051] As a preferred hexagonal ferrite from the viewpoint of radio wave absorption performance, a substituted magnetoplumbite hexagonal ferrite in which a part of the iron atoms of the magnetoplumbite hexagonal ferrite is substituted by aluminum atoms can be listed. As one form of such hexagonal ferrite, a hexagonal ferrite having a composition represented by the following formula 1 can be listed.

[0052] [Chemical formula 2]

[0053] Formula 1

[0054] AFe (12-x) Al x O 19

[0055] In Formula 1, A represents at least one atom selected from the group consisting of Sr, Ba, Ca and Pb (hereinafter also referred to as "A atom"). There may be only one atom or two or more atom in any proportion. From the viewpoint of improving the uniformity of the composition between the particles constituting the powder, it is preferably only one atom.

[0056] From the viewpoint of radio wave absorption in a high frequency band, A in Formula 1 is preferably at least one atom selected from the group consisting of Sr, Ba, and Ca, and more preferably Sr.

[0057] In Formula 1, x satisfies 1.50≤x≤8.00. From the viewpoint of radio wave absorption in the high frequency band, x is 1.50 or more, more preferably greater than 1.50, further preferably 2.00 or more, and further preferably greater than 2.00. Furthermore, from the viewpoint of magnetic properties, x is 8.00 or less, preferably less than 8.00, more preferably 6.00 or less, and more preferably less than 6.00.

[0058] Specific examples of the magnetoplumbite type hexagonal ferrite represented by Formula 1 include SrFe (9.58) Al (2.42) O 19 、SrFe (9.37) Al (2.63) O 19 、SrFe (9.27) Al (2.73) O 19 、SrFe (9.85) Al (2.15) O 19 、SrFe (10.00) Al (2.00) O 19 、SrFe (9.74) Al (2.26) O 19 、SrFe (10.44) Al (1.56) O 19 、SrFe (9.79) Al (2.21) O 19 、SrFe (9.33) Al (2.67) O 19 、SrFe (7.88) Al (4.12) O 19 、SrFe (7.04) Al(4.96) O 19 、SrFe (7.37) Al (4.63) O 19 、SrFe (6.25) Al (5.75) O 19 、SrFe (7.71) Al (4.29) O 19 , Sr (0.80) Ba (0.10) Ca (0.10) Fe (9.83) Al (2.17) O 19 ,BaFe (9.50) Al (2.50) O 19 , CaFe (10.00) Al (2.00) O 19 、PbFe (9.00) Al (3.00) O 19 The composition of the hexagonal ferrite can be confirmed by high-frequency inductively coupled plasma emission spectrometry. As a specific example of the confirmation method, the method described in the embodiments described below can be cited. Alternatively, after the radio wave absorber is cut to expose the cross section, the composition of the magnetic powder contained in the radio wave absorber can be confirmed by performing energy dispersive X-ray analysis on the exposed cross section, for example.

[0059] In one embodiment, the hexagonal ferrite powder contained in the above-mentioned radio wave absorber can be a powder with a single crystal phase or a powder containing multiple crystal phases. Preferably, it is a powder of magnetoplumbite-type hexagonal ferrite with a single crystal phase, and more preferably, it is a powder of magnetoplumbite-type hexagonal ferrite with a single crystal phase.

[0060] The case where "the crystal phase is a single phase" refers to the case where only one diffraction pattern showing an arbitrary crystal structure is observed in the X-ray diffraction analysis. The X-ray diffraction analysis can be performed, for example, by the method described in the embodiments described later. When multiple crystal phases are included, in the X-ray diffraction analysis, two or more diffraction patterns showing an arbitrary crystal structure are observed. For the attribution of the diffraction pattern, for example, the database of the International Center for Diffraction Data (ICDD: International Centre for Diffraction Data (registered trademark)) can be referenced. For example, for the diffraction pattern of the magnetoplumbite-type hexagonal ferrite containing Sr, "00-033-1340" of the International Center for Diffraction Data (ICDD) can be referenced. However, if a part of the iron atoms is substituted by substitution atoms such as aluminum atoms, the peak position is offset from the peak position when the substitution atoms are not included.

[0061] (Method for producing hexagonal ferrite powder)

[0062] As a method for producing hexagonal ferrite powder, a solid phase method and a liquid phase method can be cited. The solid phase method is a method for producing hexagonal ferrite powder by calcining a mixture obtained by dry mixing a plurality of solid raw materials. In contrast, the liquid phase method includes a process using a solution. Below, one method for producing hexagonal ferrite powder by a liquid phase method is described. However, when the above-mentioned radio wave absorber includes hexagonal ferrite powder, its production method is not limited to the following method.

[0063] One method of the liquid phase method can include:

[0064] Step 1, obtaining a precipitate from a solution containing an iron atom, at least one atom selected from the group consisting of Sr, Ba, Ca and Pb, and at least one substituent atom substituting for the iron atom as required;

[0065] Step 2, calcining the precipitate obtained in step 1 to obtain a calcined body; and

[0066] Hereinafter, each step will be described in detail.

[0067] Process 1

[0068] In step 1, a precursor of hexagonal ferrite can be obtained as a precipitate. For example, in order to obtain a powder of hexagonal ferrite in which an aluminum atom is included as a substituent atom that replaces a part of an iron atom, an iron atom, an A atom, and an aluminum atom can be mixed in a solution. In this case, it is estimated that the precipitate obtained by step 1 is iron hydroxide, aluminum hydroxide, a composite hydroxide of an iron atom, an aluminum atom, and an A atom, or the like.

[0069] The solution used to obtain the precipitate in step 1 is preferably a solution containing at least water, and more preferably an aqueous solution. For example, the precipitate can be generated by mixing an aqueous solution containing various atoms (hereinafter also referred to as "raw material aqueous solution") with an alkaline aqueous solution. In addition, step 1 can include a step of solid-liquid separation of the precipitate.

[0070] The raw material aqueous solution may be, for example, an aqueous solution containing a salt of an Fe salt, an Al salt, and an A atom. These salts may be, for example, water-soluble inorganic acid salts such as nitrates, sulfates, and chlorides.

[0071] Specific examples of the Fe salt include iron (III) chloride hexahydrate [FeCl 3 ·6H 2 O], iron (III) nitrate nonahydrate [Fe(NO 3 ) 3 ·9H 2 O], and the like.

[0072] Specific examples of Al salts include aluminum chloride hexahydrate [AlCl 3 ·6H 2 O], aluminum nitrate nonahydrate [Al(NO 3 ) 3 ·9H 2 O], and the like.

[0073] The salt of the A atom may be one or more selected from the group consisting of Sr salts, Ba salts, Ca salts, and Pb salts.

[0074] Specific examples of Sr salts include strontium chloride hexahydrate [SrCl2.6H2O], strontium nitrate [Sr(NO3)2], and strontium acetate 0.5 hydrate [Sr(CH3COO)2.0.5H2O].

[0075] Specific examples of the Ba salt include barium chloride dihydrate [BaCl2.2H2O], barium nitrate [Ba(NO3)2], and barium acetate [(CH3COO)2Ba].

[0076] Specific examples of the Ca salt include calcium chloride dihydrate [CaCl2.2H2O], calcium nitrate tetrahydrate [Ca(NO3)2.4H2O], and calcium acetate monohydrate [(CH3COO)2Ca.H2O].

[0077] Specific examples of Pb salts include lead (II) chloride [PbCl 2 ], lead (II) nitrate [Pb(NO 3 ) 2 ], and the like.

[0078] However, the above is an example, and other salts may be used. The mixing ratio of various salts used for preparing the raw material aqueous solution may be determined according to the desired hexagonal ferrite composition.

[0079] Examples of the alkaline aqueous solution include sodium hydroxide aqueous solution and potassium hydroxide aqueous solution. The concentration of the alkaline aqueous solution can be, for example, 0.1 mol / L to 10 mol / L. However, the type and concentration of the alkaline aqueous solution are not limited to the above examples as long as a precipitate can be generated.

[0080] The raw aqueous solution and the alkaline aqueous solution only need to be mixed. The raw aqueous solution and the alkaline aqueous solution may be mixed in total at once, or the raw aqueous solution and the alkaline aqueous solution may be slowly mixed. Furthermore, the other may be slowly added to either the raw aqueous solution or the alkaline aqueous solution and mixed. The method of mixing the raw aqueous solution and the alkaline aqueous solution is not particularly limited, and an example of mixing by stirring may be cited. The stirring mechanism is also not particularly limited, and a general stirring mechanism can be used. The stirring time can be set to a time in which a precipitate can be generated, and can be appropriately set according to the composition of the raw aqueous solution, the type of stirring mechanism used, etc.

[0081] For example, from the viewpoint of preventing sudden boiling, the temperature (liquid temperature) when mixing the raw aqueous solution and the alkaline aqueous solution is preferably 100°C or less, and from the viewpoint of performing the formation reaction of the precipitate well, it is more preferably 95°C or less, and further preferably 15°C or more and 92°C or less. As a mechanism for adjusting the temperature, a general heating device, a cooling device, etc. can be used. The pH of the aqueous solution obtained by mixing the raw aqueous solution and the alkaline aqueous solution at a liquid temperature of 25°C is preferably in the range of 5 to 13, and more preferably in the range of 6 to 12, for example, from the viewpoint of more easily obtaining a precipitate.

[0082] After the precipitate is generated, when the obtained precipitate is subjected to solid-liquid separation, the method is not particularly limited, and examples thereof include decantation, centrifugal separation, filtration (suction filtration, pressure filtration, etc.), etc. For example, when the solid-liquid separation is performed by centrifugal separation, the conditions of the centrifugal separation are not particularly limited, and for example, the centrifugal separation can be performed at a rotation speed of 2000 rpm (revolutions per minute) or more for 3 minutes to 30 minutes. Furthermore, the centrifugal separation can be performed multiple times.

[0083] Process 2

[0084] Step 2 is a step of calcining the precipitate obtained in step 1.

[0085] In step 2, the precursor of hexagonal ferrite can be converted into hexagonal ferrite by calcining the precipitate obtained in step 1. Calcination can be performed using a heating device. The heating device is not particularly limited, and a known heating device such as an electric furnace, a calcination device made according to a production line, etc. can be used. Calcination can be performed, for example, in an atmospheric environment. The calcination temperature and calcination time can be set to a range that can convert the precursor of hexagonal ferrite into hexagonal ferrite. The calcination temperature is preferably 900°C or more, more preferably in the range of 900°C to 1400°C, and further preferably in the range of 1000°C to 1200°C. The calcination time is preferably in the range of 1 hour to 10 hours, and more preferably in the range of 2 hours to 6 hours. In addition, the precipitate obtained by step 1 can also be dried before calcination. The drying mechanism is not particularly limited, and examples thereof include dryers such as ovens. The drying temperature is preferably in the range of 50°C to 200°C, and more preferably in the range of 70°C to 150°C. The drying time is preferably in the range of 2 hours to 50 hours, and more preferably in the range of 5 hours to 30 hours. The calcination temperature and drying temperature may be the internal environment temperature of the device for calcination or drying.

[0086] The calcined body obtained by the above-mentioned step 2 can be a block-shaped calcined body or a powder-shaped calcined body which is a precursor of hexagonal ferrite and shows the crystal structure of hexagonal ferrite. In addition, the step of crushing the calcined body can also be implemented. The crushing can be carried out by a known crushing mechanism such as a mortar and pestle, a grinder (cutter, ball mill, bead mill, roller mill, jet mill, hammer mill, grinder, etc.). For example, when a medium is used for crushing, the particle size of the medium (so-called medium diameter) is, for example, preferably in the range of 0.1 mm to 5.0 mm, and more preferably in the range of 0.5 mm to 3.0 mm. "Medium diameter" in the case of spherical media refers to the arithmetic average of the diameters of a plurality of randomly selected media (e.g., beads). In the case of non-spherical media (e.g., non-spherical beads), it refers to the arithmetic mean of the circle equivalent diameters of a plurality of randomly selected media obtained from the observation image of a transmission electron microscope (TEM; Transmission Electron Microscope) or a scanning electron microscope (SEM; Scanning Electron Microscope). As the material of the medium, for example, glass, alumina, steel, zirconia, ceramics, etc. can be listed. In addition, when a shredder is used for pulverization, the pulverization conditions can be determined according to the amount of the calcined body to be pulverized, the size of the shredder used, etc. For example, in one embodiment, the rotation speed of the shredder can be set to about 5000 to 25000 rpm.

[0087] <ε-Iron Oxide Powder>

[0088] In the present invention and this specification, "ε-iron oxide powder" refers to a powder of a magnetic material in which an ε-iron oxide type crystal structure is detected as a main phase by X-ray diffraction analysis. For example, when the diffraction peak with the highest intensity in the X-ray diffraction spectrum obtained by X-ray diffraction analysis belongs to the ε-iron oxide type crystal structure, it is determined that the ε-iron oxide type crystal structure is detected as the main phase. The ε-iron oxide powder in the present invention and this specification includes a so-called unsubstituted ε-iron oxide powder composed of iron atoms and oxygen atoms and a so-called substituted ε-iron oxide powder containing one or more substituent atoms replacing iron atoms.

[0089] (Method for producing ε-iron oxide powder)

[0090] As a method for producing a powder of ε-iron oxide, a method of producing from goethite, a reverse micelle method, etc. are known. The above production methods are all known. In addition, for a method of producing a powder of ε-iron oxide in which a part of Fe is substituted by substitution atoms such as Ga, Co, Ti, Al, and Rh, for example, reference can be made to J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp. 5200-5206, etc.

[0091] As an example, for example, the ε-iron oxide powder can be obtained by a method for producing the ε-iron oxide powder through the following steps, that is,

[0092] A step of preparing a precursor of ε-iron oxide (hereinafter also referred to as a "precursor preparation step");

[0093] A step of subjecting the precursor to a film-forming treatment (hereinafter also referred to as a "film-forming step");

[0094] a step of converting the precursor into ε-iron oxide by subjecting the precursor after the film forming process to a heat treatment (hereinafter also referred to as a "heat treatment step"); and

[0095] A step of subjecting the ε-iron oxide to a film removal treatment (hereinafter also referred to as a "film removal step").

[0096] The production method will be further described below. However, the production method described below is for illustrative purposes, and when the radio wave absorber includes ε-iron oxide powder, the powder is not limited to powder produced by the production method described below.

[0097] (Precursor preparation process)

[0098] The precursor of ε-iron oxide refers to a substance that contains a crystalline structure of ε-iron oxide type as the main phase by heating. The precursor can be, for example, a hydroxide, an oxyhydroxide (oxyhydroxide), etc., which contain atoms that can replace a part of iron in iron and the crystalline structure. The precursor preparation process can be carried out using a coprecipitation method, a reverse micelle method, etc. The preparation method of the above-mentioned precursor is well known, and the precursor preparation process in the above-mentioned manufacturing method can be carried out by a known method.

[0099] ε-iron oxide containing no substituent atom that replaces a part of the iron atoms can be represented by the composition formula: Fe2O3. On the other hand, ε-iron oxide in which a part of the iron atoms is replaced by, for example, one to three kinds of atoms can be represented by the composition formula: A 1 x A 2y A 3 z Fe (2-x-y-z) O3 means. 1 , A 2 and A 3 Each independently represents a substituent atom that replaces the iron atom, and x, y and z are independently greater than 0 and less than 1, wherein at least one exceeds 0, and x+y+z is less than 2. The above-mentioned ε-iron oxide powder may not contain or contain substituent atoms that replace iron atoms. The magnetic properties of the ε-iron oxide powder can be adjusted by the type and amount of the substituent atoms. When substituent atoms are included, as the substituent atoms, one or more of Ga, Co, Ti, Al, Rh, etc. can be listed, preferably one or more of Ga, Co and Ti. When manufacturing a powder of ε-iron oxide containing substituent atoms that replace iron atoms, a part of the compound that will become the source of Fe in the ε-iron oxide can be replaced by a compound of the substituent atom. The composition of the obtained ε-iron oxide powder can be controlled by its substitution amount. As compounds that become the source of iron atoms and various substituent atoms, for example, inorganic salts such as nitrates, sulfates, chlorides (which may be hydrates), organic salts such as penta(hydrogen oxalate) salts (which may also be hydrates), hydroxides, hydroxy oxides, etc. can be listed.

[0100] (Film Forming Step)

[0101] If the precursor is heated after the film formation treatment, the reaction of the precursor being converted into ε-iron oxide can be carried out under the film. In addition, it is believed that the film can also prevent sintering during heating. From the perspective of the ease of film formation, the film formation treatment is preferably carried out in a solution, and more preferably by adding a film forming agent (a compound for film formation) to a solution containing a precursor. For example, when the film formation treatment is continued in the same solution after the precursor is prepared, a film forming agent is added to the solution after the precursor is prepared and stirred, so that a film can be formed on the precursor. As a preferred film from the perspective of easily forming a film on a precursor in a solution, a silicon-containing film can be listed. As a film forming agent for forming a silicon-containing film, for example, silane compounds such as alkoxysilane can be listed. By hydrolyzing the silane compound, it is preferably possible to form a silicon-containing film on the precursor using a sol-gel method. As specific examples of silane compounds, tetraethoxysilane (TEOS; Tetraethyl orthosilicate), tetramethoxysilane and various silane coupling agents can be exemplified. For example, the film formation treatment can be performed by stirring a solution containing the precursor and the film forming agent at a temperature of 50 to 90° C. for about 5 to 36 hours. The film may cover the entire surface of the precursor, or a portion of the precursor surface may not be covered by the film.

[0102] (Heat treatment process)

[0103] By subjecting the precursor to heat treatment after the above-mentioned film forming treatment, the precursor can be converted into ε-iron oxide. The heat treatment can be performed, for example, on a powder collected from a solution subjected to the film forming treatment (powder of the precursor having the film). The heat treatment step can be performed, for example, in a heat treatment furnace at a furnace temperature of 900 to 1200° C. for about 3 to 6 hours.

[0104] (Film removal process)

[0105] By performing the above-mentioned heat treatment step, the precursor with a coating is converted into ε-iron oxide. Since the coating remains in the ε-iron oxide obtained in this way, it is preferable to perform a coating removal treatment. The coating removal treatment can be performed, for example, by stirring the ε-iron oxide with a coating in a sodium hydroxide aqueous solution with a concentration of about 4 mol / L and a liquid temperature of about 60 to 90°C for 5 to 36 hours. However, the powder of ε-iron oxide can also be manufactured without undergoing a coating removal treatment, that is, a powder with a coating. In addition, it can also be a treatment in which the coating is not completely removed in the coating removal treatment, and a part of the coating remains.

[0106] It is also possible to arbitrarily implement known steps before and / or after the various steps described above. As such steps, various known steps such as filtration, washing, and drying can be cited.

[0107] The shape of the particles constituting the magnetic powder is not particularly limited, and examples thereof include spherical, rod-shaped, needle-shaped, plate-shaped, irregular shapes, etc. For example, the shape of the particles constituting the powder of magnetoplumbite-type hexagonal ferrite may include plate-shaped, irregular shapes, etc., and the shape of the particles constituting the powder of ε-iron oxide may include spherical shapes, etc.

[0108] <Various physical properties of magnetic powders can be obtained>

[0109] The size of the magnetic powder particles included in the radio wave absorber is not particularly limited. In the particle size distribution of the magnetic powder measured by laser diffraction scattering method, the mode value is defined as the mode diameter and the cumulative 10% diameter is defined as D 10 And the cumulative 90% diameter is set as D 90 When the mode diameter is preferably 5 μm or more and less than 10 μm. 90 -D 10 ) / mode diameter ≤3.0, more preferably (D 90 -D 10 ) / mode diameter ≤ 2.5, more preferably (D 90 -D 10 ) / mode diameter ≤ 2.0, more preferably (D90 -D 10 ) / mode diameter ≤ 1.5, more preferably (D 90 -D 10 ) / mode diameter ≤ 1.0. The mode diameter is 5 μm or more and (D 90 -D 10 ) / mode diameter ≤3.0, there is a tendency that a radio wave absorber with better radio wave absorption performance can be manufactured by using such magnetic powders because of the relatively small number of fine particles. 90 -D 10 ) / mode diameter ≤3.0, there is a tendency that a radio wave absorber with higher strength can be manufactured by using such magnetic powder because there are relatively few coarse particles.

[0110] The particle size of magnetic powder (i.e., mode diameter, D 10 and D 90 ) can be controlled by classification using a sieve, a centrifuge, or the like, or by pulverization using a mortar and pestle, an ultrasonic disperser, or the like. For example, when the particle size of the magnetic powder is controlled by pulverization, the particle size can be adjusted by selecting a pulverization mechanism, pulverization time, a medium material, a medium diameter, or the like. For example, the longer the pulverization time, the smaller the particle size of the magnetic powder. And, for example, the smaller the medium diameter, the smaller the particle size of the magnetic powder. "(D 90 -D 10 The value of ") / mode diameter" can be adjusted by classifying the particles after pulverization, for example, by using a sieve, a centrifuge, or the like.

[0111] The particle size of the magnetic powder is a value obtained from a number-based particle size distribution measured by a laser diffraction scattering method. Specifically, it can be measured by the following method.

[0112] After adding 500 mL of cyclohexanone to 10 mg of magnetic powder for dilution, the mixture was stirred for 30 seconds using an oscillator, and the obtained liquid was used as a sample for particle size distribution measurement. Next, the sample for particle size distribution measurement was used to measure the particle size distribution by a laser diffraction scattering method. A laser diffraction / scattering particle size distribution measuring device was used in the measuring device.

[0113] The particle size of the magnetic powder contained in the radio wave absorber can be confirmed by the following method, for example.

[0114] After the radio wave absorber is finely cut, it is dispersed in a solvent (for example, acetone) by ultrasonic wave, and the obtained dispersion is used as a sample and measured by laser diffraction scattering method to confirm the particle size of the magnetic powder.

[0115] Furthermore, from the viewpoint of radio wave absorption performance, regarding the magnetic properties of the magnetic powder contained in the above-mentioned radio wave absorber, the magnetic field intensity Hα that becomes 90% of the magnetization amount when an external magnetic field of 50kOe is applied is preferably 19.0kOe or more and 28.0kOe or less. From the viewpoint of further improving the radio wave absorption performance, the above-mentioned magnetic field intensity Hα is more preferably 20.0kOe or more, more preferably 21.0kOe or more, and further preferably 22.0kOe or more. Furthermore, from the same viewpoint, the above-mentioned magnetic field intensity Hα is more preferably 27.0kOe or less, more preferably 26.0kOe or less, and further preferably 25.0kOe or less. The above-mentioned magnetic field intensity Hα of the magnetic powder can be adjusted by the composition of the magnetic body constituting the magnetic powder, the manufacturing method, etc.

[0116] The above-mentioned magnetic field intensity Hα is a value obtained by the following method.

[0117] Using a vibrating sample magnetometer, the magnetization intensity of the magnetic powder relative to the applied magnetic field is measured at an ambient temperature of 23°C, with a maximum applied magnetic field of 50kOe and a magnetic field scanning speed of 25Oe / s ("s" means "seconds"). Then, the magnetic field (H)-magnetization (M) curve of the powder is obtained based on the measurement results. Based on the obtained magnetic field (H)-magnetization (M) curve, the magnetic field intensity that is 90% of the magnetization amount under the applied magnetic field of 50kOe is calculated, and this magnetic field intensity is set to Hα. Regarding units, 1kOe=(10 6 / 4π)A / m.

[0118] The coercive force (Hc) of the magnetic powder contained in the above-mentioned radio wave absorber is not particularly limited. From the perspective of radio wave absorption performance, the coercive force (Hc) of the magnetic powder is preferably 2.5 kOe or more, more preferably 4.0 kOe or more, and further preferably 5.0 kOe or more. The upper limit of the coercive force (Hc) of the magnetic powder is not particularly limited, and can be, for example, 18.0 kOe or less.

[0119] The saturation magnetization (δs) per unit mass of the magnetic powder contained in the above-mentioned radio wave absorber is not particularly limited. From the perspective of radio wave absorption performance, the saturation magnetization (δs) of the magnetic powder is preferably 10.0 emu / g or more, more preferably 20.0 emu / g or more, and further preferably 30.0 emu / g or more. Regarding the unit, 1 emu / g = 1 A·m 2 / kg.

[0120] The upper limit of the saturation magnetization (δs) per unit mass of the magnetic powder is not particularly limited, and may be, for example, 60.0 emu / g or less.

[0121] The coercive force (Hc) and saturation magnetization per unit mass (δs) of the magnetic powder are measured using a vibrating sample magnetometer at an ambient temperature of 23°C, with a maximum applied magnetic field of 50 kOe and a magnetic field scanning speed of 25 Oe / s.

[0122] In one embodiment, the magnetic powder contained in the radio wave absorber is preferably surface-treated.

[0123] The surface-treated powder can realize a radio wave absorber having excellent radio wave absorption performance, especially a balance between reflection attenuation and transmission attenuation. The surface-treated magnetic powder can particularly increase the peak attenuation of reflection of the radio wave absorber.

[0124] Furthermore, if the magnetic powder is surface treated, even if a composition for forming a radio wave absorber (so-called radio wave absorber-forming composition) contains a large amount of magnetic powder, the handling and processing properties are unlikely to be impaired.

[0125] Furthermore, when the composition for forming a radio wave absorber contains surface-treated magnetic powder, the mechanical strength of the formed radio wave absorber can be improved.

[0126] The reason why the surface-treated magnetic powder can exert the above-mentioned effects is not clear, but the present inventors speculate as follows.

[0127] If the magnetic powder is subjected to surface treatment, the cohesive force between the particles constituting the magnetic powder can be weakened, and the aggregation of the particles can be suppressed. If the aggregation of the particles is suppressed, the viscosity of the composition for forming a radio wave absorber is difficult to increase. Therefore, it is believed that the composition for forming a radio wave absorber shows sufficient fluidity even when a large amount of magnetic powder is included, and the operability and processability are not easily impaired.

[0128] Furthermore, if the magnetic powder is subjected to surface treatment, the affinity between the magnetic powder and the adhesive can be improved. By weakening the cohesive force between the particles constituting the magnetic powder and / or by improving the affinity between the magnetic powder and the adhesive, the powder can be more evenly dispersed in the adhesive. Therefore, it is believed that a radio wave absorber that is not prone to causing deviations in radio wave absorption performance and has excellent mechanical strength can be formed.

[0129] When the magnetic powder included in the radio wave absorber is subjected to surface treatment, a known surface treatment technique can be applied to the surface treatment.

[0130] Types of surface treatment include oil treatment using hydrocarbon oil, ester oil, lanolin, etc.; silicone treatment using dimethylpolysiloxane, methylhydrogenpolysiloxane, methylphenylpolysiloxane, etc.; fluorine compound treatment using esters containing perfluoroalkyl groups, perfluoroalkyl silanes, perfluoropolyethers, and polymers having perfluoroalkyl groups; silane coupling agent treatment using 3-methacryloxypropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, etc.; titanium coupling agent treatment using isopropyl triisostearoyl titanate, isopropyl tri(dioctyl pyrophosphate) titanate, etc.; metal soap treatment; amino acid treatment using acylglutamic acid, etc.; lecithin treatment using hydrogenated egg yolk lecithin, etc.; polyethylene treatment; mechanochemical treatment; phosphoric acid compound treatment using phosphoric acid, phosphorous acid, phosphate, phosphite, etc.; and the like.

[0131] Among them, as the type of surface treatment, phosphoric acid compound treatment is preferred.

[0132] When the magnetic powder is treated with a phosphoric acid compound, a thick layer with high polarity can be formed on the surface of the particles constituting the magnetic powder.

[0133] If a high polarity layer is formed on the surface of the particles, the aggregation caused by the hydrophobic interaction between the particles is suppressed, so the viscosity increase of the radio wave absorber-forming composition can be more effectively suppressed. Therefore, in the case of magnetic powder treated with a phosphate compound, the fluidity of the radio wave absorber-forming composition is less likely to decrease due to the inclusion of a large amount of magnetic powder, and there is a tendency that the handleability and processability are less likely to be impaired.

[0134] Furthermore, if a high polarity layer is formed on the surface of the particles, not only can the aggregation of the particles be suppressed, but also the affinity between the magnetic powder and the binder can be further improved, so that the magnetic powder can be dispersed more uniformly in the binder. Therefore, the radio wave absorber formed by the radio wave absorber-forming composition containing the magnetic powder treated with the phosphate compound tends to be less likely to have a deviation in radio wave absorption performance and has a better mechanical strength.

[0135] The phosphoric acid compound includes phosphorous acid, hypophosphorous acid, pyrophosphoric acid, linear polyphosphoric acid, cyclic metaphosphoric acid, and salts thereof in addition to phosphoric acid.

[0136] When the phosphoric acid compound is in the form of a salt, the phosphoric acid compound is preferably a metal salt.

[0137] The metal salt is not particularly limited, and examples thereof include alkali metal salts and alkaline earth metal salts.

[0138] Also, the phosphoric acid compound may be an ammonium salt.

[0139] In the phosphoric acid compound treatment, only one phosphoric acid compound may be used, or two or more phosphoric acid compounds may be used.

[0140] In the phosphoric acid compound treatment, the phosphoric acid compound is usually mixed with a chelating agent, a neutralizing agent, etc. as a surface treatment agent.

[0141] In the phosphoric acid compound treatment, an aqueous solution containing a generally commercially available phosphoric acid compound can be used as a surface treatment agent.

[0142] The phosphoric acid compound treatment of the magnetic powder can be carried out, for example, by mixing the magnetic powder and a surface treatment agent containing a phosphoric acid compound. The mixing time, temperature and other conditions can be appropriately set according to the purpose. In the phosphoric acid compound treatment, the dissociation (equilibrium) reaction of the phosphoric acid compound can be used to precipitate the insoluble phosphoric acid compound on the surface of the particles constituting the magnetic powder.

[0143] For the phosphoric acid compound treatment, for example, reference can be made to the description in “Surface Technology”, Vol. 61, No. 3, p. 216, 2010, or “Surface Technology”, Vol. 64, No. 12, p. 640, 2013.

[0144] Furthermore, as the type of surface treatment, treatment with a silane coupling agent is also preferred.

[0145] As the silane coupling agent, a silane coupling agent having a hydrolyzable group is preferred.

[0146] In the silane coupling agent treatment using a silane coupling agent having a hydrolyzable group, the hydrolyzable group in the silane coupling agent is hydrolyzed by water to form a hydroxyl group, which undergoes a dehydration condensation reaction with a hydroxyl group on the surface of the silica particles, thereby modifying the surface of the particles.

[0147] Examples of the hydrolyzable group include an alkoxy group, an acyloxy group, and a halide group.

[0148] The silane coupling agent may have a hydrophobic group as a functional group.

[0149] Examples of the silane coupling agent having a hydrophobic group as a functional group include alkoxysilanes such as methyltrimethoxysilane (MTMS), dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, methyltriethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, and decyltrimethoxysilane; trichlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, and phenyltrichlorosilane; hexamethyldisilazane (HMDS); and the like.

[0150] Furthermore, the silane coupling agent may have a vinyl group as a functional group.

[0151] Examples of the silane coupling agent having a vinyl group in its functional group include alkoxysilanes such as methacryloxypropyltriethoxysilane, methacryloxypropyltrimethoxysilane, methacryloxypropylmethyldiethoxysilane, methacryloxypropylmethyldimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, and vinylmethyldimethoxysilane; chlorosilanes such as vinyltrichlorosilane and vinylmethyldichlorosilane; divinyltetramethyldisilazane; and the like.

[0152] In the silane coupling agent treatment, only one type of silane coupling agent may be used, or two or more types may be used.

[0153] The surface treatment method is not particularly limited, and a known method can be applied.

[0154] Examples of the surface treatment method include a method of mixing magnetic powder and a surface treatment agent using a mixer such as a Henschel mixer, a method of spraying a surface treatment agent on particles constituting the magnetic powder, and a method of mixing a liquid containing a surface treatment agent obtained by dissolving or dispersing the surface treatment agent in an appropriate solvent with the magnetic powder and then removing the solvent.

[0155] [Adhesive]

[0156] The radio wave absorber includes magnetic powder and a binder. The binder may be, for example, a resin, and examples of the resin include thermoplastic resins and thermosetting resins.

[0157] Examples of the thermoplastic resin include acrylic resins, polyacetals, polyamides, polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polystyrene, polyphenylene sulfide, polyvinyl chloride, ABS (acrylonitrile butadiene styrene) resins obtained by copolymerizing acrylonitrile, butadiene and styrene; and AS (acrylonitrile styrene) resins obtained by copolymerizing acrylonitrile and styrene.

[0158] Examples of the thermosetting resin include phenol resin, epoxy resin, melamine resin, urea resin, unsaturated polyester, diallyl phthalate resin, polyurethane resin, and silicone resin.

[0159] The adhesive may also be rubber. As the rubber, for example, from the viewpoint of being able to manufacture a radio wave absorber having good miscibility with magnetic powder and having better durability, weather resistance and impact resistance, synthetic rubbers such as butadiene rubber, isoprene rubber, chloroprene rubber, halogenated butyl rubber, fluororubber, polyurethane rubber, acrylic rubber (abbreviated as ACM) obtained by copolymerizing polyacrylates (e.g., ethyl acrylate, butyl acrylate and 2-ethylhexyl acrylate) and other monomers, ethylene-propylene rubber obtained by coordination polymerization of ethylene and propylene using a Ziegler catalyst, butyl rubber (abbreviated as IIR) obtained by copolymerizing isobutylene and isoprene, styrene butadiene rubber (abbreviated as SBR) obtained by copolymerizing butadiene and styrene, acrylonitrile butadiene rubber (abbreviated as NBR) obtained by copolymerizing polyacrylonitrile and butadiene, and silicone rubber can also be cited.

[0160] When the radio wave absorber contains rubber as a binder, it may contain various additives such as a vulcanizing agent, a vulcanizing accelerator, a softener, a plasticizer, etc. in addition to the rubber. Examples of the vulcanizing agent include sulfur, organic sulfur compounds, and metal oxides.

[0161] As the binder, for example, thermoplastic elastomer (TPE; Thermoplastic Elastomer) can also be cited. As the thermoplastic elastomer, olefin-based thermoplastic elastomer (TPO; Thermoplastic Olefinic Elastomer), styrene-based thermoplastic elastomer (TPS; Thermoplastic Styrenic Elastomer), amide-based thermoplastic elastomer (TPA; Thermoplastic Polyamide Elastomer), polyester-based thermoplastic elastomer (TPC; Thermoplastic Copolyester) and the like can be cited.

[0162] The radio wave absorber may contain only one adhesive or two or more adhesives. The volume filling rate of the adhesive in the radio wave absorber is not particularly limited, but, for example, is preferably 65 volume % or more, more preferably 65 volume % or more and 92 volume % or less, and further preferably 65 volume % or more and 85 volume % or less. When the radio wave absorber contains two or more adhesives, the volume filling rate refers to the total volume filling rate of the two or more adhesives. This is also the same for the volume filling rates related to other components.

[0163] [additive]

[0164] The above-mentioned radio wave absorber contains magnetic powder and adhesive, and may also contain one or more additives at will. Other additives include antioxidants, light stabilizers, dispersants, dispersing aids, mildew inhibitors, antistatic agents, plasticizers, impact resistance improvers, crystal nucleating agents, lubricants, surfactants, pigments, dyes, fillers, release agents (fatty acids, fatty acid metal salts, hydroxy fatty acids, fatty acid esters, aliphatic partially saponified esters, paraffin, low molecular weight polyolefins, fatty acid amides, alkylene bis fatty acid amides, aliphatic ketones, fatty acid lower alcohol esters, fatty acid polyol esters, fatty acid polyethylene glycol esters, modified silicones, etc.), processing aids, antifogging agents, anti-drip agents, antibacterial agents, etc. The additive may be an additive in which one component performs two or more functions. The above-mentioned radio wave absorber may contain commercially available products or products manufactured by known methods at any filling rate as additives. In addition, the research results of the inventors show that if carbon components such as graphite are used as additives, there is a tendency to degrade the reflection attenuation of the radio wave absorber. Therefore, when using carbon components as additives, it is preferred that the amount of carbon components used is small, and it is also preferred not to use carbon components as additives. In addition, carbon components are mixed in commercial products that can be used as adhesives for color adjustment, etc. From the viewpoint of increasing the reflection attenuation, for adhesives containing carbon components, it is preferred to use an adhesive in which the proportion of carbon components is small. In addition, as an adhesive, it is also preferred to use an adhesive that does not contain carbon components. Here, "carbon component" refers to a component in which carbon atoms account for 90 atomic% to 100 atomic% of all atoms constituting the component. In one embodiment, in the above-mentioned radio wave absorber, the volume filling rate of the carbon component is preferably in the range of 0 to 2.0 volume%, more preferably in the range of 0 to 1.5 volume%, and further preferably in the range of 0 to 1.0 volume%.

[0165] <Antioxidants>

[0166] In one embodiment, the radio wave absorber preferably contains an antioxidant.

[0167] The antioxidant is not particularly limited, and a known antioxidant can be used.

[0168] Examples of antioxidants are described in, for example, "Comprehensive Technology for Polymer Stabilization - Mechanism and Application Development" published by CMC and supervised by Yasukazu Ohkatsu, which is incorporated herein by reference.

[0169] Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants.

[0170] The antioxidant is preferably used together with a phenolic antioxidant and / or an amine antioxidant and a phosphorus antioxidant and / or a sulfur antioxidant.

[0171] Examples of the phenolic antioxidant include Adekastab AO-20, Adekastab AO-30, Adekastab AO-40, Adekastab AO-50, Adekastab AO-60, Adekastab AO-80, and Adekastab AO-330 manufactured by Adeka Corporation, and IRGANOX 1010, IRGANOX 1035, IRGANOX 1076, IRGANOX 1098, IRGANOX 1135, IRGANOX 1330, IRGANOX 1726, IRGANOX 245, IRGANOX 259, IRGANOX 3114, and IRGANOX 565 manufactured by BASF Japan Ltd. In addition, both of the above-mentioned "Adekastab" and "IRGANOX" are registered trademarks.

[0172] Examples of the amine antioxidant include Sanole LS-770, Sanole LS-765, and Sanole LS-2626 manufactured by Sankyo Lifetech Co., Ltd., Adekastab LA-77, Adekastab LA-57, Adekastab LA-52, Adekastab LA-62, Adekastab LA-63, Adekastab LA-67, Adekastab LA-68, and Adekastab LA-72 manufactured by ADEKA Corporation, and TINUVIN 123, TINUVIN 144, TINUVIN 622, TINUVIN 765, and TINUVIN 944 manufactured by BASF Japan Ltd. In addition, both of the above-mentioned "Adekastab" and "TINUVIN" are registered trademarks.

[0173] Furthermore, the above-mentioned radio wave absorber can also contain an amine compound capable of quenching free radicals as an antioxidant. Examples of such amine compounds include polyethylene glycol bis-TEMPO (Sigma-Aldrich Co. LLC.), sebacic acid bis-TEMPO, etc. In addition, "TEMPO" is an abbreviation for tetramethylpiperidin-1-oxyl.

[0174] Examples of the phosphorus-based antioxidant include Adekastab PEP-8, Adekastab PEP-36, Adekastab HP-10, and Adekastab 2112 manufactured by ADEKA Corporation and IRGAFOS 168 manufactured by BASF Japan Ltd. In addition, both of the above-mentioned "Adekastab" and "IRGAFOS" are registered trademarks.

[0175] Examples of the sulfur-based antioxidant include Adekastab AO-412S and Adekastab AO-503S manufactured by ADEKA Corporation. In addition, the above-mentioned "Adekastab" is a registered trademark.

[0176] Among the above, as a phenol-based antioxidant, at least one selected from the group consisting of Adekastab AO-20, Adekastab AO-60, Adekastab AO-80 and IRGANOX 1010 is preferred, as an amine-based antioxidant, Adekastab LA-52 is preferred, as a phosphorus-based antioxidant, Adekastab PEP-36 is preferred, and as a sulfur-based antioxidant, Adekastab AO-412S is preferred.

[0177] When the radio wave absorber contains an antioxidant, it may contain only one antioxidant or two or more antioxidants.

[0178] When the above-mentioned radio wave absorber contains an antioxidant, the content of the antioxidant in the radio wave absorber is not particularly limited. For example, from the viewpoint of simultaneously suppressing the decomposition of the adhesive and the leakage of the antioxidant, it is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the adhesive.

[0179] <Light stabilizer>

[0180] In one embodiment, the radio wave absorber preferably contains a light stabilizer.

[0181] Examples of the light stabilizer include HALS (hindered amine light stabilizer), ultraviolet absorbers, and singlet oxygen quenchers.

[0182] When the radio wave absorber contains a light stabilizer, it may contain only one type of light stabilizer or may contain two or more types.

[0183] HALS may be a high molecular weight HALS, a low molecular weight HALS, or a combination of a high molecular weight HALS and a low molecular weight HALS. In the present invention and this specification, "high molecular weight HALS" refers to a hindered amine light stabilizer having a weight average molecular weight exceeding 1000. In addition, in the present invention and this specification, "low molecular weight HALS" refers to a hindered amine light stabilizer having a molecular weight of 1000 or less (preferably 900 or less, more preferably 600 to 900).

[0184] The weight average molecular weight (Mw) in the present invention and this specification is a value measured by gel permeation chromatography (GPC). In the measurement by gel permeation chromatography (GPC), HLC (registered trademark)-8220GPC (Tosoh Corporation) can be used as a measuring device, TSKgel (registered trademark) Super HZM-M (4.6 mmID (Inner Diameter) × 15 cm, Tosoh Corporation), Super HZ4000 (4.6 mmID × 15 cm, Tosoh Corporation), Super HZ3000 (4.6 mmID × 15 cm, Tosoh Corporation), Super HZ2000 (4.6 mmID × 15 cm, Tosoh Corporation) can be used as a column connected in series, and THF (tetrahydrofuran) can be used as an eluent.

[0185] The measurement can be performed using a differential refractive index (RI) detector with a sample concentration of 0.2 mass %, a flow rate of 0.35 mL / min, a sample injection amount of 10 μL, and a measurement temperature of 40° C.

[0186] The calibration curve can be prepared using “standard samples TSK standard, polystyrene” manufactured by Tosoh Corporation: “F-40”, “F-20”, “F-4”, “F-1”, “A-5000”, “A-2500”, and “A-1000”.

[0187] High molecular weight HALS

[0188] Examples of high molecular weight HALS include oligomer-type HALS, i.e., poly[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino], dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidinyl condensate, and the like.

[0189] Examples of commercially available products of high molecular weight HALS include CHIMASSORB 944LD and TINUVIN 622LD from BASF Japan Ltd. In addition, both of the above-mentioned "CHIMASSORB" and "TINUVIN" are registered trademarks.

[0190] When the radio wave absorber includes a high molecular weight HALS, the content of the high molecular weight HALS in the radio wave absorber is not particularly limited, and is preferably, for example, 0.2% by mass to 10% by mass based on the total mass of the radio wave absorber.

[0191] From the viewpoint of improving weather resistance, the content of the high molecular weight HALS in the radio wave absorber is preferably 0.2 mass % or more relative to the total mass of the radio wave absorber.

[0192] When the content of the high molecular weight HALS in the radio wave absorber is 10 mass % or less relative to the total mass of the radio wave absorber, a decrease in mechanical strength tends to be suppressed, and the occurrence of flocculants tends to be suppressed.

[0193] Low molecular weight HALS

[0194] Examples of low molecular weight HALS include tris(2,2,6,6-tetramethyl-4-piperidinyl)benzene-1,3,5-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidinyl)-2-acetoxypropane-1,2,3-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidinyl)-2-hydroxypropane-1,2,3-tricarboxylate, tris(2,2,6,6-tetramethyl-4-piperidinyl)triazine-2,4,6-tricarboxylate, and tris(2,2,6,6-tetramethyl-4-piperidinyl)-triazine-2,4,6-tricarboxylate. tetrakis(2,2,6,6-tetramethyl-4-piperidyl)propane-1,1,2,3-tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)1,2,3,4-butanetetracarboxylate, 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-n-butylmalonate, and the like.

[0195] Examples of commercially available low-molecular-weight HALS include Adekastab LA-57 and Adekastab LA-52 manufactured by ADEKA Corporation and TINUVIN 144 manufactured by BASF Japan Ltd. In addition, both of the above-mentioned "Adekastab" and "TINUVIN" are registered trademarks.

[0196] When the above-mentioned radio wave absorber contains low molecular weight HALS, the content of the low molecular weight HALS in the radio wave absorber is not particularly limited, and is preferably, for example, 0.2% by mass to 10% by mass based on the total mass of the radio wave absorber.

[0197] From the viewpoint of improving weather resistance, the content of the low molecular weight HALS in the radio wave absorber is preferably 0.2 mass % or more relative to the total mass of the radio wave absorber.

[0198] When the content of the low molecular weight HALS in the radio wave absorber is 10 mass % or less relative to the total mass of the radio wave absorber, a decrease in mechanical strength tends to be suppressed, and the occurrence of flocculants tends to be suppressed.

[0199] UV absorber

[0200] Examples of the ultraviolet absorber include 2-(-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(-(3,5-di-tert-amyl-2-hydroxyphenyl)benzotriazole, 2-(-(2'-hydroxy-5'-methyl-phenyl)benzotriazole, 2-(-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3",4",5",6"-tetrahydro-o-phenyl)benzotriazole, 2-[2-Hydroxy-3,5-bis(a,a-dimethylbenzyl)benzene] Benzotriazole-based ultraviolet absorbers such as benzotriazole-2H-benzotriazole, 2-(-(2-hydroxy-4-octyloxyphenyl)-2H-benzotriazole, 2-(-(2H-benzotriazol-2-yl)-4-methyl-6-(-(3,4,5,6-tetrahydrophthalimidomethyl)phenol, 2-hydroxy-4-methoxybenzophenone, 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2-hydroxy Benzophenone-based ultraviolet absorbers such as 4-n-octyloxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 3,5-di-tert-butyl-4-(hydroxybenzoyl)benzoic acid n-hexadecyl ester, 1,4-bis(4-benzoyl-3-hydroxyphenoxy)butane, 1,6-bis(4-benzoyl-3-hydroxyphenoxy)hexane, and cyanoacrylate-based ultraviolet absorbers represented by ethyl-2-cyano-3,3-diphenylacrylate.

[0201] Examples of commercially available ultraviolet absorbers include TINUVIN 320, TINUVIN 328, TINUVIN 234, TINUVIN 1577, TINUVIN 622, and IRGANOX series manufactured by BASF Japan Ltd., Adekastab LA31 manufactured by ADEKA, and SEESORB 102, SEESORB 103, and SEESORB 501 manufactured by SHIPRO KASEI KAISHA, LTD. In addition, the above-mentioned "TINUVIN", "IRGANOX", "Adekastab", and "SEESORB" are all registered trademarks.

[0202] When the radio wave absorber contains an ultraviolet absorber, the content of the ultraviolet absorber in the radio wave absorber is not particularly limited, and is preferably, for example, 0.2% by mass to 10% by mass based on the total mass of the radio wave absorber.

[0203] From the viewpoint of improving weather resistance, the content of the ultraviolet absorber in the radio wave absorber is preferably 0.2% by mass or more based on the total mass of the radio wave absorber.

[0204] When the content of the ultraviolet absorber in the radio wave absorber is 10 mass % or less relative to the total mass of the radio wave absorber, a decrease in mechanical strength tends to be suppressed, and the occurrence of blisters tends to be suppressed.

[0205] -Singlet oxygen quencher-

[0206] When the radio wave absorber contains a singlet oxygen quencher, the content of the singlet oxygen quencher in the radio wave absorber is not particularly limited, and is preferably, for example, 0.2% by mass to 10% by mass relative to the total mass of the radio wave absorber.

[0207] From the viewpoint of improving weather resistance, the content of the singlet oxygen quencher in the radio wave absorber is preferably 0.2% by mass or more relative to the total mass of the radio wave absorber.

[0208] When the content of the singlet oxygen quencher in the radio wave absorber is 10 mass % or less relative to the total mass of the radio wave absorber, the mechanical strength tends to be reduced and the occurrence of flocculants tends to be suppressed.

[0209] <Method for producing radio wave absorber>

[0210] The manufacturing method of the above-mentioned radio wave absorber is not particularly limited. For example, it can be manufactured by using magnetic powder, adhesive and solvent, additives, etc. as needed and by a known method. For example, the above-mentioned radio wave absorber can be a molded product formed by molding a composition containing magnetic powder and adhesive (hereinafter, also referred to as "radio wave absorber forming composition".). The radio wave absorber forming composition can be made by mixing a mixture of magnetic powder and adhesive, and further mixing solvents, additives, etc. as needed, while heating and kneading to form a mixed product. The mixed product can be obtained in the form of particles, for example. By molding the mixed product into a desired shape by a known molding method such as extrusion molding, stamping molding, injection molding, in-mold molding, etc., a radio wave absorber (molded product) can be obtained. The shape of the radio wave absorber is not particularly limited, and can be any shape such as a plate shape, a wire shape, etc. "Plate shape" includes sheet shape and film shape. Plate-shaped radio wave absorbers can also be called radio wave absorption plates, radio wave absorption sheets, radio wave absorption films, etc. The above-mentioned radio wave absorber may be a radio wave absorber of a single composition (for example, a single-layer radio wave absorbing plate), or may be a combination of two or more parts having different compositions (for example, a laminate). Furthermore, the above-mentioned radio wave absorber may have a planar shape, may have a three-dimensional shape, or may be a combination of a part having a planar shape and a part having a three-dimensional shape. Examples of the planar shape include a sheet shape, a film shape, and the like. Examples of the three-dimensional shape include a cylindrical shape (cylindrical shape, square cylindrical shape, etc.), a trumpet shape, a box shape (for example, at least one surface is open), and the like.

[0211] For example, from the viewpoint of ease of handling, the thickness of the radio wave absorber is preferably 20.0 mm or less, more preferably 10.0 mm or less, and further preferably 5.0 mm or less. From the viewpoint of mechanical properties, the thickness is preferably 1.0 mm or more, more preferably 2.0 mm or more. For example, the transmission attenuation can be controlled by adjusting the thickness of the radio wave absorber. In addition, when the radio wave absorber is a laminate, the thickness refers to the total thickness of the radio wave absorber constituting the laminate. The thickness of the radio wave absorber is a value measured using a digital length measuring machine, specifically the arithmetic average of the measured values ​​measured at 9 randomly selected positions.

[0212] The composition for forming a radio wave absorber may or may not contain a solvent. When the composition for forming a radio wave absorber contains a solvent, the solvent is not particularly limited, and examples thereof include water, an organic solvent, or a mixed solvent of water and an organic solvent.

[0213] As the organic solvent, there can be mentioned alcohols such as methanol, ethanol, n-propanol, isopropanol, methoxypropanol, ketones such as acetone, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, acetonitrile, ethyl acetate, toluene, etc. Among them, as the solvent, from the viewpoint of drying speed, ketones are preferred, and cyclohexanone is more preferred. When the composition for forming the radio wave absorber contains a solvent, the content of the solvent in the composition is not particularly limited, as long as it is determined according to the method for manufacturing the radio wave absorber.

[0214] The composition for forming a radio wave absorber can be prepared by mixing the above-mentioned components. The mixing method is not particularly limited, and for example, a method of mixing by stirring can be cited. As a stirring mechanism, a known stirring device can be used. For example, as a stirring device, a stirrer such as a paddle stirrer and an impeller stirrer can be cited. The stirring time can be set according to the type of stirring device, the composition of the composition for forming a radio wave absorber, etc.

[0215] As one aspect of the method for producing the radio wave absorber, there can be mentioned a method of molding the radio wave absorbing composition into a desired shape by a known molding method as exemplified above.

[0216] In addition, as another method for producing the above-mentioned radio wave absorber, a method of coating the radio wave absorber-forming composition on a support to produce the radio wave absorber as a radio wave absorbing layer can be cited. The support used here may be removed before the radio wave absorber is assembled into an article to be given radio wave absorbency, or may be assembled into the article together with the radio wave absorber without being removed.

[0217] As a support, there is no particular limitation, and a known support can be used. As a support, for example, metal plates (metal plates such as aluminum, zinc, and copper), glass plates, plastic sheets [polyester (polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.), polyethylene (linear low-density polyethylene, low-density polyethylene, high-density polyethylene, etc.), polypropylene, polystyrene, polycarbonate, polyimide, polyamide, polyamide-imide, polysulfone, polyvinyl chloride, polyacrylonitrile, polyphenylene sulfide, polyetherimide, polyethersulfone, polyvinyl acetal, acrylic resin and other sheets], laminated or vapor-deposited plastic sheets exemplified for the above-mentioned metal plates, etc. The plastic sheet is preferably biaxially stretched. The shape, structure, size, etc. of the support can be appropriately selected. As the shape of the support, for example, a plate-like shape can be cited. The structure of the support can be a single-layer structure or a laminated structure of more than two layers. The size of the support can be appropriately selected according to the size of the radio wave absorber, etc. The thickness of the support is generally about 0.01 mm to 10 mm, and for example, preferably 0.02 mm to 3 mm, and more preferably 0.05 mm to 1 mm, from the viewpoint of handling properties.

[0218] The method of coating the composition for forming a radio wave absorber on the support is not particularly limited, and examples thereof include methods using a film coater, a knife coater, an applicator, and the like. The method of coating and drying the composition for forming a radio wave absorber to form a coating film is not particularly limited, and examples thereof include methods using a known heating device such as an oven. The drying temperature and the drying time are not particularly limited. As an example, the drying temperature may be in the range of 70° C. to 90° C., and the drying time may be in the range of 1 hour to 3 hours.

[0219] The above-mentioned radio wave absorber can be assembled into various articles to which radio wave absorbency is desired. For example, a plate-shaped radio wave absorber can be assembled into an article directly or in any form such as by bending it at any part. In addition, it can also be assembled into an article by adjusting it into a desired shape by injection molding or the like.

[0220] Example

[0221] Hereinafter, the present invention will be described based on examples. However, the present invention is not limited to the embodiments shown in the examples. Unless otherwise specified, the steps and evaluations described below were performed in an environment with an ambient temperature of 23°C ± 1°C.

[0222] The “hexagonal ferrite” described below is a powder of hexagonal strontium ferrite produced by the following method, and the “ε-iron oxide” is a powder of ε-iron oxide produced by the following method.

[0223] [Production of magnetic powder]

[0224] <Preparation of magnetic powder 1 (preparation of hexagonal ferrite powder)>

[0225] As the magnetic powder 1, a powder of magnetoplumbite-type hexagonal ferrite was prepared by the following method.

[0226] 400.0 g of water was stirred and maintained at a liquid temperature of 35° C., and all amounts of a raw aqueous solution prepared by dissolving 57.0 g of iron (III) chloride hexahydrate [FeCl3·6H2O], 27.8 g of strontium chloride hexahydrate [SrCl2·6H2O] and 10.2 g of aluminum chloride hexahydrate [AlCl3·6H2O] in 216.0 g of water and a solution prepared by adding 113.0 g of water to 181.3 g of an aqueous sodium hydroxide solution having a concentration of 5 mol / L were added to the stirred water at a flow rate of 10 mL / min at the same addition timing to obtain a first liquid.

[0227] Next, after the liquid temperature of the first liquid was set to 25°C, 39.8 g of a 1 mol / L sodium hydroxide aqueous solution was added while maintaining the liquid temperature to obtain a second liquid. The pH of the obtained second liquid was 10.5±0.5. The pH was measured using a tabletop pH meter (F-71 manufactured by HORIBA, Ltd.).

[0228] Next, the second liquid was stirred for 15 minutes to obtain a liquid containing a precipitate that is a precursor of magnetoplumbite-type hexagonal ferrite (precursor-containing liquid).

[0229] Next, the liquid containing the precursor was subjected to centrifugal separation treatment three times (rotation speed: 2000 rpm, rotation time: 10 minutes), and the obtained precipitate was recovered and washed with water.

[0230] Next, the recovered precipitate was dried in an oven at an internal ambient gas temperature of 95° C. for 12 hours to obtain a precursor powder.

[0231] Next, the precursor powder was placed in a muffle furnace, and the temperature in the furnace was set to 1100° C. in an atmospheric atmosphere, and calcined for 4 hours to obtain a bulk calcined body.

[0232] Next, the obtained calcined body was pulverized for 90 seconds using a chopper (Wonder Crusher WC-3 manufactured by OSAKA CHEMICAL Co., Ltd.) as a pulverizer, with the variable speed dial of the pulverizer set to "5" (rotation speed: about 10,000 to 15,000 rpm).

[0233] In summary, magnetic powder 1 was obtained.

[0234] <Preparation of magnetic powder 2 (preparation of ε-iron oxide powder)>

[0235] As the magnetic powder 2, ε-iron oxide powder was prepared by the following method.

[0236] A liquid prepared by dissolving 8.6 g of iron nitrate (III) 9 hydrate, 1.0 g of gallium (III) nitrate 8 hydrate, 190 mg of cobalt (II) nitrate 6 hydrate, 150 mg of titanium (IV) sulfate and 1.5 g of polyvinyl pyrrolidone (PVP) in 90.0 g of pure water was stirred with a magnetic stirrer, and 4.0 g of ammonia solution with a concentration of 25% was added in an atmospheric environment at an ambient temperature of 25°C, and stirred for 2 hours at an ambient temperature of 25°C. To the obtained solution, a citric acid aqueous solution prepared by dissolving 1 g of citric acid in 9 g of pure water was added and stirred for 1 hour. The powder that precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace at a furnace temperature of 80°C.

[0237] 800 g of pure water was added to the dried powder, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to a liquid temperature of 50°C, and 40 g of a 25% ammonia solution was added dropwise while stirring. After stirring for 1 hour while maintaining a temperature of 50°C, 14 mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 50.0 g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried in a heating furnace at a furnace temperature of 80°C for 24 hours to obtain a precursor of ε-iron oxide.

[0238] The obtained precursor was placed in a heating furnace at a furnace temperature of 1000° C. in an atmospheric environment and subjected to a heating treatment for 4 hours.

[0239] The precursor after the heat treatment was put into a 4 mol / L sodium hydroxide (NaOH) aqueous solution, and the liquid temperature was maintained at 70° C. and stirred for 24 hours, thereby removing the silicic acid compound as an impurity from the precursor after the heat treatment.

[0240] Then, the powder from which the silicate compound was removed was collected by centrifugal separation and washed with pure water, thereby obtaining magnetic powder 2.

[0241] [Confirmation of crystal structure]

[0242] The crystal structure of the magnetic substance constituting each of the magnetic powders was confirmed by X-ray diffraction analysis. As a measuring device, X'Pert Pro manufactured by PANalytical, which is a powder X-ray diffraction analyzer, was used. The measuring conditions are shown below.

[0243] -Measurement conditions-

[0244] X-ray source: CuKα line

[0245] 〔wavelength: (0.154nm), output: 40mA, 45kV〕

[0246] Scanning range: 20°<2θ<70°

[0247] Scanning interval: 0.05°

[0248] Scanning speed: 0.75° / min

[0249] The results of the above X-ray diffraction analysis confirmed that the magnetic powder 1 had a magnetoplumbite type crystal structure and was a single-phase magnetoplumbite type hexagonal ferrite powder that did not contain a crystal structure other than the magnetoplumbite type. In addition, the results of the above X-ray diffraction analysis confirmed that the magnetic powder 2 had a unidirectional crystal structure of the ε phase (ε-iron oxide type crystal structure) that did not contain a crystal structure of the α phase and the γ phase.

[0250] [Confirmation of composition]

[0251] The composition of the magnetic substance constituting each of the magnetic powders was confirmed by high-frequency inductively coupled plasma emission spectrometry. Specifically, the composition was confirmed by the following method.

[0252] A beaker containing 12 mg of magnetic powder and 10 mL of 4 mol / L hydrochloric acid aqueous solution was placed on a hot plate set at 120°C for 3 hours to obtain a solution. After adding 30 mL of pure water to the obtained solution, it was filtered using a membrane filter with a pore size of 0.1 μm. The elemental analysis of the filtrate thus obtained was performed using a high-frequency inductively coupled plasma emission spectrometer [ICPS-8100 manufactured by Shimadzu Corporation]. Based on the obtained elemental analysis results, the content of each atom relative to 100 atomic % of iron atoms was calculated. Then, the composition of the magnetic body was confirmed based on the obtained content. As a result, it was confirmed that magnetic powder 1 had SrFe 10.00 Al 2.00 O 19 The powder of hexagonal ferrite (hexagonal strontium ferrite) and the magnetic powder 2 are Ga 0.22 Ti 0.05 Co 0.05 Fe 1.68 Powder of ε-iron oxide composed of O3.

[0253] [Evaluation of magnetic powder]

[0254] <Particle size distribution>

[0255] The number-based particle size distribution of the magnetic powder 1 was measured by a laser diffraction scattering method, and the mode value (so-called mode diameter), the cumulative 10% diameter, and the cumulative 90% diameter were obtained.

[0256] Specifically, 500 mL of cyclohexanone was added to 10 mg of the magnetic powder for dilution, and then the mixture was stirred for 30 seconds using a shaker, and the obtained liquid was used as a sample for particle size distribution measurement.

[0257] Next, the particle size distribution of the particle size distribution measurement sample was measured using a laser diffraction / scattering type particle size distribution measuring apparatus (Partica LA-960 manufactured by HORIBA, Ltd.).

[0258] Then, based on the obtained number-based particle size distribution, the mode diameter (unit: μm) as the mode value and the cumulative 10% diameter D 10 (unit: μm) and D as the cumulative 90% diameter 90(Unit: μm). And, the "(D 90 -D 10 ) / mode diameter” value.

[0259] As a result, the mode diameter of magnetic powder 1 was 6.7 μm, and D 10 4.1μm, D 90 9.5μm, (D 90 -D 10 ) / mode diameter” is 0.81.

[0260] The magnetic field intensity Hα, the coercive force (Hc), and the saturation magnetization (δs) per unit mass of each of the magnetic powders were measured by the following method.

[0261] As a measuring device, a vibrating sample magnetometer (model: TM-TRVSM5050-SMSL) manufactured by TAMAKAWA CO., LTD was used. Under the conditions of a maximum applied magnetic field of 50 kOe and a magnetic field scanning speed of 25 Oe / s, the intensity of the magnetization of the magnetic powder relative to the applied magnetic field was measured at an ambient temperature of 23°C. Based on the measurement results, a magnetic field (H)-magnetization (M) curve of the magnetic powder was obtained. Based on the obtained magnetic field (H)-magnetization (M) curve, the coercive force (Hc) (unit: kOe) and the saturation magnetization (δs) per unit mass (unit: emu / g) of the magnetic powder were calculated. Furthermore, based on the obtained magnetic field (H)-magnetization (M) curve, the magnetic field intensity that is 90% of the magnetization amount under an applied magnetic field of 50 kOe was calculated, and this was set as the magnetic field intensity Hα.

[0262] As a result, the magnetic field strength Hα of magnetic powder 1 was 24.5 kOe, the coercive force (Hc) was 10.5 kOe, and the saturation magnetization (δs) per unit mass was 43.2 emu / g. In addition, the magnetic field strength Hα of magnetic powder 2 was 23.5 kOe, the coercive force (Hc) was 4.6 kOe, and the saturation magnetization (δs) was 18.5 emu / g.

[0263] [Examples 1 to 4, Comparative Examples 1 to 4]

[0264] The magnetic powder and the binder (olefin-based thermoplastic elastomer (TPO) [Mirastomer (registered trademark) 7030NS manufactured by Mitsui Chemicals, Inc.) shown in Table 1 were kneaded for 20 minutes using a kneading machine (Lavoplastmill manufactured by Toyo Seiki Seisaku-sho, Ltd.) with the set temperature of the kneading machine set to 200°C to obtain a composition for forming a radio wave absorber (a granular kneaded product). The above-mentioned binder is a binder that does not contain a carbon component.

[0265] The obtained composition for forming a radio wave absorber was press-molded using a heating press to obtain a radio wave absorber as a plate-shaped molded product having a square plane with a side length of 100 mm. The volume filling rate of the magnetic body in each radio wave absorber was adjusted by changing the mixing ratio of the magnetic powder and the binder when preparing the composition for forming a radio wave absorber. The thickness of each radio wave absorber was adjusted by changing the press conditions during molding.

[0266] [Comparative Example 5]

[0267] When preparing the composition for forming a radio wave absorber, a radio wave absorber was prepared in the same manner as in Example 3 except that no magnetic powder was added and graphite powder (CNP-35 manufactured by Ito Graphite Co., Ltd.) was added as a carbon component in an amount such that the volume filling rate in the radio wave absorber became 30 volume %.

[0268] [Comparative Example 6]

[0269] When preparing a composition for forming a radio wave absorber, a radio wave absorber was obtained by the same method as in Example 2 except that a graphite powder (CNP-35 manufactured by ItoGraphite Co., Ltd.) as a carbon component was mixed with the above-mentioned binder in an amount so that the volume filling rate in the radio wave absorber became 5.0 volume %, and then mixed with the magnetic powder shown in Table 1 and the subsequent steps were carried out.

[0270] [Evaluation of radio wave absorbers]

[0271] <Volume filling rate of magnetic powder>

[0272] Each of the above-mentioned radio wave absorbers was cut into a plate-shaped measurement sample having a square plane with a side length of 5 mm. The thickness of the measurement sample was the same as that of each radio wave absorber.

[0273] After attaching the above-mentioned measurement sample to the workbench, a focused ion beam (FIB) device (MI4050 manufactured by Hitachi, Ltd.) was used to perform FIB processing to expose the thickness direction and form a cross section, thereby preparing a cross-section observation sample. The prepared cross-section observation sample was observed by SEM, and a cross-section image (SEM image) was taken. As an SEM, a field emission scanning electron microscope (SU-8220 manufactured by Hitachi, Ltd.) was used, and the cross-section observation sample was set on the workbench in such a way that the cross section after FIB processing faced upward. Under the conditions of an acceleration voltage of 15 kV and an observation magnification of 3,000 times, a cross-section SEM image with a field of view of 30 μm × 40 μm was obtained. The obtained cross-section SEM image was binarized and the proportion of the magnetic powder (area basis) was calculated. After the brightness distribution of the obtained cross-sectional SEM image was expressed by a histogram, binarization processing was performed using the brightness values ​​of the peak of the bright part (part of the magnetic powder) and the center of the peak of the dark part (part other than the magnetic powder) as thresholds.

[0274] The above operation was performed on five measurement samples cut out from different positions of each radio wave absorber, and the volume filling rate of the magnetic powder in each radio wave absorber was calculated as the arithmetic average of the five values ​​obtained.

[0275] <Thickness of radio wave absorber>

[0276] For each of the above-mentioned radio wave absorbers, the thickness was determined as the arithmetic mean of the measured values ​​at 9 randomly selected locations using a digital length measuring machine [Litematic (registered trademark) VL-50A manufactured by Mitutoyo Corporation].

[0277] <Transmission loss and reflection loss>

[0278] The transmission attenuation (unit: dB) and reflection attenuation (unit: dB) of each of the above-mentioned radio wave absorbers were measured by the following method.

[0279] As measuring devices, a vector network analyzer (product name: N5225B) manufactured by Keysight and a horn antenna (product name: RH12S23) manufactured by KEYCOM Corp. were used. By using the free space method, the incident angle was set to 0° and the scanning frequency was set to 60 GHz to 90 GHz. One plane of each of the above-mentioned radio wave absorbers was directed toward the incident side to measure the S parameters, and the S parameter S21 at a frequency of 76.5 GHz was set as the transmission attenuation, and the S parameter S11 at a frequency of 76.5 GHz was set as the reflection attenuation.

[0280] < Radar Directivity >

[0281] Each of the above-mentioned radio wave absorbers was bent into a trumpet shape and placed in the radio wave transceiver of the evaluation device. Then, a metal plate that reflects radio waves was placed at a position 1m away from the radio wave transceiver (at an angle of 0° and 45° with the front of the radio wave transceiver as the angle), and an evaluation was conducted to determine whether the metal plate was recognized by the radio wave transceiver. The case of clear recognition was set as evaluation result C, the case of slight recognition was set as evaluation result B, and the case of no recognition was set as evaluation result A.

[0282] <Unnecessary reflection components>

[0283] Each of the above-mentioned radio wave absorbers was bent into a trumpet shape and placed in the radio wave transceiver of the evaluation device. Then, a metal plate that reflects radio waves was placed at a position 10m away from the radio wave transceiver (at the front of the radio wave transceiver (at an angle of 0°)), and an evaluation was conducted to determine whether the metal plate was recognized by the radio wave transceiver. The case where normal recognition was possible was set as evaluation result A, the case where normal recognition was almost possible was set as evaluation result B, and the case where no recognition was possible was set as evaluation result C.

[0284] The above results are shown in Table 1.

[0285]

[0286] From the results shown in Table 1, it can be confirmed that the radio wave absorber of the example is a radio wave absorber that can contribute to improving the recognition accuracy of the radar.

[0287] Industrial Applicability

[0288] One aspect of the present invention is useful in the technical field of various automatic driving controls such as automatic driving control of automobiles.

Claims

1. A radio wave absorber comprising magnetic powder and a binder, wherein: The volume filling rate of the magnetic powder in the radio wave absorber is 15 volume % or more and 35 volume % or less, The thickness of the radio wave absorber is not less than 2.0 mm and not more than 10.0 mm, The magnetic powder comprises hexagonal ferrite powder, The mode diameter of the magnetic powder particles is greater than 5 μm and less than 10 μm, (D 90 -D 10 ) / mode diameter ≤ 3.0, The transmission attenuation of the radio wave absorber at a frequency of 76.5 GHz is greater than 8.0 dB, and The reflection attenuation of the radio wave absorber at a frequency of 76.5 GHz is 8.0 dB or more. 2 . The radio wave absorber according to claim 1 , which is a molded product obtained by molding a composition containing magnetic powder and a binder.

3. The radio wave absorber according to claim 1, wherein: The hexagonal ferrite has a composition represented by the following formula 1, Formula 1 AFe (12-x) Al X O 19 In Formula 1, A represents at least one atom selected from the group consisting of Sr, Ba, Ca and Pb, and x satisfies 1.50≤x≤8.

00.

4. The radio wave absorber according to claim 3, wherein: In Formula 1, the atom represented by A includes Sr.

5. The radio wave absorber according to claim 1 or 2, wherein: The magnetic powder includes ε-iron oxide powder.

6. The radio wave absorber according to claim 5, wherein: The epsilon-iron oxide is epsilon-iron oxide containing one or more atoms selected from the group consisting of gallium atoms, titanium atoms, and cobalt atoms.

Citation Information

Patent Citations

  • Radio wave absorption sheet

    JP2018056492A

  • Electromagnetic wave absorption material and electromagnetic wave absorber

    CN108370654A

  • Electromagnetic wave absorber for millimeter

    JP2002118008A

  • Oxide magnetic powder and its manufacturing method

    JP2003282319A

  • Electromagnetic wave absorbing body

    JP2004096084A