A method for synthesizing di-(2-hydroxy-2-propyl)benzene

By using Pd catalyst for hydroreduction in BIPB production, the particle size and dispersion are regulated, the problem of large amount of wastewater in the prior art is solved, efficient and environmentally friendly BIPB production is achieved, and conversion rate and selectivity are improved.

CN113880687BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010636263.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-03
Publication Date
2024-11-01
Estimated Expiration
2040-07-03

AI Technical Summary

Technical Problem

During the existing BIPB production process, the reducing agent reduction process produces a large amount of unbiochemically-treated wastewater and high-salt wastewater, and the reaction safety is insufficient and there are many by-products, which affects environmental protection and production efficiency.

Method used

The hydroreduction process is carried out using Pd catalyst to regulate the average particle size, dispersion and layer thickness of Pd, the conversion rate and selectivity of the reaction are improved, and wastewater discharge is reduced.

Benefits of technology

The high conversion rate of BIPB (up to 97%) and high selectivity (up to 92%) were achieved, reducing high-salt wastewater discharge, reducing pollution, and improving reaction safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113880687B_ABST
    Figure CN113880687B_ABST
Patent Text Reader

Abstract

The invention provides a method for synthesizing di-(2-hydroxy-2-propyl)benzene, comprising reacting a mixture of 2-hydroxy-2-propyl-cumyl hydroperoxide and diisopropylbenzene hydroperoxide in a reducing atmosphere in the presence of a catalyst, wherein the catalyst comprises a carrier and a Pd layer loaded on the surface of the carrier, wherein the average particle size of Pd in ​​the Pd layer is 5-10 nm. The method can replace the current Na2SO3 reduction method, greatly reduce the discharge of high-salt wastewater, and reduce pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing di-(2-hydroxy-2-propyl)benzene. Background Art

[0002] BIPB is the abbreviation of di-(tert-butylperoxyisopropyl)benzene, which is an upgraded product of diisopropylbenzene peroxide (DCP), commonly known as "odorless DCP", and is an organic peroxide crosslinking agent second only to DCP in terms of usage. The BIPB market has great potential. Since BIPB has been in short supply in the domestic and foreign markets for a long time, it can be predicted that with the development of the globalization of the international market, the enhancement of people's environmental awareness and the improvement of their quality of life, the demand for BIPB from domestic and foreign users will increase.

[0003] The reduction process is an important part of the BIPB production process, that is, the diisopropylbenzene (DIPB) oxidation liquid (obtained from the oxidation of diisopropylbenzene) is reduced with a reducing agent, and the reduced liquid is purified to obtain a mixture of the intermediate 2-hydroxy-2-propyl-hydroperoxyisopropylbenzene (HHP) and diisopropylbenzene dihydroperoxide (DHP), and the intermediate is further reduced to produce di-(2-hydroxy-isopropyl)benzene (abbreviated as DC). The reduction process in the production of BIPB is essentially to convert the hydroperoxy group (-OOH) into a hydroxyl group (-OH), specifically: a mixture of 2-hydroxy-2-propyl-hydroperoxyisopropylbenzene (HHP) and diisopropylbenzene dihydroperoxide (DHP) is reduced to di-(2-hydroxy-2-propyl)benzene (DC), of which isopropyldimethylbenzyl alcohol (MC) is a by-product. The reaction formula is as follows:

[0004]

[0005] The existing reduction methods mainly use Na2SO3 and Na2S as reducing agents, oxidizing liquid plus alkali decomposition, etc. Hydroperoxide reduction usually uses a reducing agent reduction process, which is quite mature at present, but the fatal disadvantage of this reaction is that it will produce an equivalent amount of sulfate wastewater, which contains a large amount of toxic substances to bacteria and cannot be biochemically treated. The process of oxidizing liquid plus alkali decomposition is characterized by a high DC yield, but the disadvantages are insufficient reaction safety, more by-products, and the waste alkali produced cannot be biochemically treated. Summary of the invention

[0006] In order to solve the problem of large amount of wastewater in the above-mentioned reducing agent reduction process, the present invention provides a method for synthesizing di-(2-hydroxy-2-propyl)benzene. The method adopts a hydrogenation reduction process and uses a specific Pd catalyst to greatly improve the conversion rate and selectivity of the reaction and reduce the discharge of wastewater.

[0007] A first aspect of the present invention provides a method for synthesizing di-(2-hydroxy-2-propyl)benzene, the method comprising reacting a mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide and diisopropylbenzene hydroperoxide in a reducing atmosphere in the presence of a catalyst, the catalyst comprising a carrier and a Pd layer supported on the surface of the carrier, wherein the average particle size of Pd in ​​the Pd layer is 5-10 nm.

[0008] According to some embodiments of the present invention, the average particle size of Pd is 5.5-8 nm, for example, 5.7 nm, 5.9 nm, 6.1 nm, 6.2 nm, 6.3 nm, 6.4 nm, 6.5 nm, 6.6 nm, 6.7 nm, 6.8 nm, 6.9 nm, 7.1 nm, 7.3 nm, 7.5 nm, 7.7 nm, 7.9 nm and any value therebetween.

[0009] In some advantageous embodiments of the present invention, the average particle size of Pd is 6-7 nm.

[0010] According to some embodiments of the present invention, the dispersion of Pd is 15-30%, for example 16%, 17%, 19%, 21%, 22%, 23%, 24%, 26%, 28%, 29% and any value therebetween.

[0011] According to some embodiments of the present invention, the dispersion degree of Pd is 20-25%.

[0012] According to some embodiments of the invention, the Pd layer has an average thickness of 1-10 μm, for example, 1.5 μm, 2.0 μm, 2.5 μm, 3.2 μm, 3.5 μm, 3.7 μm, 3.9 μm, 4.0 μm, 4.2 μm, 4.5 μm, 4.7 μm, 4.9 μm, 5.1 μm, 5.5 μm, 6.0 μm, 6.5 μm, 7.0 μm, 7.5 μm, 8.0 μm, 8.9 μm, 9.0 μm, 9.5 μm and any value therebetween.

[0013] According to some embodiments of the present invention, the average thickness of the Pd layer is 2-7 μm.

[0014] In some preferred embodiments of the present invention, the average thickness of the Pd layer is 3-5 μm.

[0015] In the present invention, the thickness of the Pd layer is preferably controlled within the above range. Too high a thickness will result in poor hydrogenation effect, while too low a thickness will easily result in over-hydrogenation.

[0016] The inventor of the present application found in the research process that the hydrogenation reduction of a mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide (HHP) and diisopropylbenzene dihydroperoxide (DHP) to generate di-(2-hydroxy-isopropyl) benzene (DC) is a coupling of two steps of dehydration and hydrogenation reaction. Studies have found that dehydration is the controlling step of the reaction, so the first thing to improve in the regulation of the catalyst is the dehydration activity of the catalyst, thereby increasing the reaction rate of the entire reaction. The dispersity of metal palladium has a certain relationship with its grain size, and generally the larger the grain, the smaller the dispersity. Studies have also found that the Pd dispersity is not linearly related to the size of the grains, because TEM analysis found that the size of the Pd grains on the catalyst with a reduced dispersity did not significantly increase. In addition, the appropriate grain growth of the Pd catalyst helps to improve the reaction selectivity. Therefore, it is necessary to keep the particle size and its dispersity within a reasonable range.

[0017] According to some embodiments of the present invention, the carrier is not particularly limited, and a catalyst carrier commonly used in the art may be used.

[0018] According to some embodiments of the present invention, the carrier is selected from one or more of alumina, silica, activated carbon and alumina-silica.

[0019] According to some embodiments of the present invention, the average pore size of the carrier is 10-25 nm, preferably 12-18 nm.

[0020] According to some embodiments of the present invention, the specific surface area of ​​the carrier is 150-300m 2 / g.

[0021] According to some embodiments of the present invention, the pore volume of the carrier is 0.4-0.6 mL / g.

[0022] According to some embodiments of the present invention, the mass content of Pd is 0.01-5%, for example 0.3%, 0.6%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 4.0%, 4.5% and any value therebetween, based on the mass of the carrier.

[0023] According to some embodiments of the present invention, the mass content of Pd is 0.05-2%.

[0024] According to some embodiments of the present invention, the method for preparing the catalyst comprises the following steps:

[0025] S1, mixing a palladium source with a solvent to form a solution;

[0026] S2, adjusting the pH of the solution in S1 to 1-6, preferably to 2-4;

[0027] S3, mixing the carrier with the solution after adjusting the pH, drying, calcining and reducing to obtain the catalyst.

[0028] According to some embodiments of the present invention, in S3, the mixing temperature is 50-90°C, such as 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C and any value therebetween.

[0029] According to some embodiments of the present invention, in S3, the mixing temperature is 60-80°C.

[0030] According to some embodiments of the present invention, in S3, the mixing time is 10-60 min, such as 15 min, 25 min or 30 min.

[0031] According to some embodiments of the present invention, in S3, the mixing time is 20-40 min.

[0032] According to some embodiments of the present invention, during the mixed impregnation process, the impregnation temperature is adjusted to 60-90°C; and the impregnation time is adjusted, preferably to 10-40 minutes, so that the Pd layer thickness and dispersion of the final catalyst meet the requirements of the present invention.

[0033] According to some embodiments of the present invention, the calcination temperature is 400-600°C.

[0034] According to some embodiments of the present invention, the reducing atmosphere is a hydrogen-nitrogen mixed gas with a hydrogen content of 30-100% and an air velocity of 100-4000h -1 , the time is at least 5h and the pressure is below 2MPa.

[0035] According to some embodiments of the present invention, the palladium source is selected from one or more of chloropalladic acid, palladium nitrate and palladium sulfate.

[0036] According to some embodiments of the present invention, the solvent is selected from one or more of water and C1-C4 alkyl alcohol.

[0037] According to some embodiments of the present invention, the solvent is selected from one or more of water, methanol and ethanol.

[0038] According to some embodiments of the present invention, an acidic compound is used to adjust the pH of the solution in S1.

[0039] According to some embodiments of the present invention, the acidic compound is selected from one or more of phosphoric acid, sulfuric acid, citric acid, nitric acid, acetic acid and hydrochloric acid.

[0040] In the present invention, the activity and selectivity of the prepared catalyst are appropriately regulated by adjusting the pH of the impregnation solution, and preferably the pH of the impregnation solution is adjusted to 2-4.

[0041] According to some embodiments of the present invention, the reaction pressure is 0.1-4.0 MPa, such as 0.5 MPa, 0.9 MPa, 1.5 MPa, 2.5 MPa, 3.5 MPa and any value therebetween.

[0042] According to some embodiments of the present invention, the reaction pressure is 1-3.0 MPa.

[0043] According to some embodiments of the present invention, the reaction temperature is 30-100°C, such as 40°C, 60°C, 70°C or 90°C.

[0044] According to some embodiments of the present invention, the volume space velocity of the mixture is 1-20h -1 , for example 2h -1 、 3h -1 , 4h -1 , 8h -1 , 10h -1 , 14h -1 , 16h -1 、18h -1 and any values ​​in between.

[0045] According to some embodiments of the present invention, the volume space velocity of the mixture is 1-5h -1 .

[0046] According to some embodiments of the present invention, the reducing atmosphere is a hydrogen atmosphere, and preferably the molar ratio of hydrogen to diisopropylbenzene hydroperoxide is >4.

[0047] According to some embodiments of the present invention, the molar ratio of hydrogen to diisopropylbenzene hydroperoxide is 5-7.

[0048] The second aspect of the present invention provides di-(2-hydroxy-2-propyl)benzene prepared by the method described in the first aspect.

[0049] Compared with the prior art, the present invention uses a Pd catalyst to hydrogenate a mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide (HHP) and diisopropylbenzene dihydroperoxide (DHP) to generate di-(2-hydroxy-2-propyl)benzene (DC), with a conversion rate of 97% and a selectivity of up to 92%. The method can replace the current Na2SO3 reduction method, greatly reduce the discharge of high-salt wastewater, and reduce pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1is a Pd distribution diagram of the catalyst obtained according to Example 1 of the present invention.

[0051] Figure 2 is a TEM image of the catalyst obtained according to Example 1 of the present invention. DETAILED DESCRIPTION

[0052] In order to make the present invention easy to understand, the present invention will be described in detail below with reference to embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.

[0053] Unless otherwise specified, the raw materials or components used in the present invention can be obtained through commercial routes or conventional methods.

[0054] Test Method

[0055] 1) The Pd metal dispersion is determined by hydrogen-oxygen titration. The specific analysis steps are: the catalyst is heated to 120°C (heating rate 10°C / min) under a certain hydrogen flow, kept constant for 2 hours, then heated to 145°C and purged with argon for 1 hour before cooling to room temperature (under argon atmosphere). Chemical adsorption of oxygen: at room temperature, pulse oxygen into the sample tube until saturated, then purge with argon for 40 minutes. Determination of hydrogen titration: use a six-way injection valve to make a quantitative pulse of hydrogen (quantitative tube volume 0.3mL). The difference in the area of ​​the front and rear peaks on the chromatograph can be used to calculate the amount of hydrogen consumed, and thus the dispersion of metal Pd on the catalyst can be calculated.

[0056] 2) Particle size distribution of Pd: The particle size distribution of Pd on the catalyst was measured and analyzed using transmission electron microscopy (TEM).

[0057] 3) Pd layer thickness: The catalyst shell thickness was measured qualitatively and quantitatively by cutting the catalyst in half and using a scanning electron microscope-energy dispersive spectrometer (SEM-EDS).

[0058] Example 1

[0059] 1. Preparation of silica-alumina carrier

[0060] 300g of a mixture of pseudo-boehmite and silica powder (where the mass ratio of pseudo-boehmite to silica powder is 4:1) was mixed evenly and formed into a clover shape by kneading and extrusion. After drying and calcination at 900℃ for 4h, the carrier with a specific surface area of ​​190m 2 ·g -1 , pore volume is 0.59 mL·g -1 , the average pore size is 12.06nm.

[0061] 2. Preparation of catalyst

[0062] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 2.5. The impregnation time was 30 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 1. The Pd content in catalyst 1 was 0.5%, the dispersion was 22%, the average particle size was 6.0 nm, and the catalyst Pd layer thickness was 3.35 μm.

[0063] Example 2

[0064] 1. Preparation of silica-alumina carrier

[0065] Same as Example 1.

[0066] 2. Preparation of catalyst

[0067] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 70°C, and the pH was adjusted to 2.5. The impregnation time was 30 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 2. The Pd content in catalyst 2 was 0.5%, the dispersion was 30%, the average particle size was 7.0 nm, and the catalyst Pd layer thickness was 5.57 μm.

[0068] Example 3

[0069] 1. Preparation of silica-alumina carrier

[0070] Same as Example 1.

[0071] 2. Preparation of catalyst

[0072] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 50°C, and the pH was adjusted to 2.5, and the impregnation time was 30 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours, and the calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain Catalyst 3. The Pd content in Catalyst 3 was 0.5%, the dispersion was 27%, the average particle size was 10.0 nm, and the thickness of the catalyst Pd layer was 6.56 μm.

[0073] Example 4

[0074] 1. Preparation of silica-alumina carrier

[0075] Same as Example 1.

[0076] 2. Preparation of catalyst

[0077] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 2.5. The impregnation time was 20 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 4. The Pd content in catalyst 1 was 0.5%, the dispersion was 25%, the average particle size was 8.5 nm, and the thickness of the catalyst Pd layer was 5.01 μm.

[0078] Example 5

[0079] 1. Preparation of silica-alumina carrier

[0080] Same as Example 1.

[0081] 2. Preparation of catalyst

[0082] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 2.5. The impregnation time was 40 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 1. The Pd content in catalyst 1 was 0.5%, the dispersion was 22%, the average particle size was 6 nm, and the catalyst Pd layer thickness was 7.03 μm.

[0083] Example 6

[0084] 1. Preparation of silica-alumina carrier

[0085] Same as Example 1.

[0086] 2. Preparation of catalyst

[0087] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 3.0. The impregnation time was 30 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 1. The Pd content in catalyst 1 was 0.5%, the dispersion was 22%, the average particle size was 7nm, and the catalyst Pd layer thickness was 8μm.

[0088] Example 7

[0089] 1. Preparation of silica-alumina carrier

[0090] Same as Example 1.

[0091] 2. Preparation of catalyst

[0092] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 3.0. The impregnation time was 20 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 1. The Pd content in catalyst 1 was 0.5%, the dispersion was 25%, the average particle size was 5 nm, and the catalyst Pd layer thickness was 2.0 μm.

[0093] Example 8

[0094] 1. Preparation of silica-alumina carrier

[0095] Same as Example 1.

[0096] 2. Preparation of catalyst

[0097] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 3.0. The impregnation time was 10 minutes. The impregnated catalyst was dried and calcined at 450°C for 4 hours. The calcined product was reduced with a mixed gas of N2:H2 molar ratio = 0.5:1 at 450°C for 12 hours to obtain catalyst 1. The Pd content in catalyst 1 was 0.5%, the dispersion was 20%, the average particle size was 7nm, and the catalyst Pd layer thickness was 2.5μm.

[0098] Comparative Example 1

[0099] 1. Preparation of silica-alumina carrier

[0100] Same as Example 1.

[0101] 2. Preparation of comparative catalyst 1

[0102] A chloropalladic acid aqueous solution was prepared, and 50 g of the silicon oxide-alumina carrier was impregnated at 80°C, and the pH was adjusted to 3.0, and the impregnation time was 10 minutes. The impregnated catalyst was dried and calcined at 450°C, and the calcined product was reduced at 450°C for 12 hours with a mixed gas of N2:H2 molar ratio = 0.5:1 to obtain comparative catalyst 1. The Pd content in comparative catalyst 1 was 0.5%, the dispersion was 35%, the average particle size was 4.0 nm, and the catalyst Pd layer thickness was 5.52 μm.

[0103] Catalyst performance test

[0104] A mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide (HHP) and diisopropylbenzene diperoxide (DHP) is used as the raw material oil, wherein the mass ratio of HHP to DHP is 6:4, wherein the mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide (HHP) and diisopropylbenzene diperoxide (DHP) is obtained by purifying diisopropylbenzene (DIPB) oxidation liquid (obtained by oxidation of diisopropylbenzene) in the BIPB production process, and the purification process is a conventional process in the art.

[0105] 50 ml of catalyst 1-6 and comparative catalyst 1- were respectively loaded into an adiabatic bed reaction device, the pressure was raised to 2.7 MPa, the hydrogen flow rate was 180 ml / min, and the bed temperature was reduced for 16 hours at 35 ° C. After the reduction was completed, the inlet temperature was cooled to 33 ° C, and the C6-C8 hydrogenation product oil was used to establish a cycle. After the cycle was stable, the inlet temperature was raised to 38 ° C, and the raw oil was introduced. The evaluation conditions were: reaction pressure 2.7 MPa, inlet temperature 38 ° C, fresh raw oil volume space velocity 3.0 h -1 , hydrogen flow rate 180ml / min.

[0106] After 180 hours of reaction, the specific properties are shown in Table 1.

[0107] Table 1

[0108] Pd dispersion % Average particle size nm Pd layer thickness μm Conversion Rate % DC selectivity % Example 1 22 6 3.35 100 98 Example 2 30 7 5.57 100 95 Example 3 27 10 6.56 99 92 Example 4 25 8.50 5.01 100 93 Example 5 22 6 7.03 98 94 Example 6 20 7 8.0 97 92 Example 7 25 5 2.0 98 90 Example 8 20 7 2.5 100 88 Comparative Example 1 35 4 5.52 100 90

[0109] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A method for synthesizing di-(2-hydroxy-2-propyl)benzene, comprising reacting a mixture of 2-hydroxy-2-propyl-isopropylbenzene hydroperoxide and diisopropylbenzene dihydroperoxide in a reducing atmosphere in the presence of a catalyst, wherein the catalyst comprises a carrier and a Pd layer supported on the surface of the carrier, wherein the average particle size of Pd in ​​the Pd layer is 5-10 nm; and the dispersion degree of Pd is 15-30%; The average thickness of the Pd layer is 3-6 μm.

2. The method according to claim 1, characterized in that The average particle size of the Pd is 5.5-8 nm.

3. The method according to claim 2, characterized in that The average particle size of the Pd is 6-7 nm.

4. The method according to any one of claims 1 to 3, characterized in that: The dispersion degree of Pd is 20-25%.

5. The method according to any one of claims 1 to 3, characterized in that: The average thickness of the Pd layer is 3-5 μm.

6. The method according to any one of claims 1 to 3, characterized in that: The carrier is selected from one or more of alumina, silica, activated carbon and alumina-silica; And / or the average pore size of the carrier is 10-25nm, the specific surface area is 150-300m 2 / g, pore volume is 0.4-0.6mL / g; The mass content of Pd and / or Pd is 0.01-5%.

7. The method according to claim 6, characterized in that The average pore size of the carrier is 12-18 nm; The mass content of and / or Pd is 0.05-2%.

8. The method according to any one of claims 1 to 3, characterized in that: The preparation method of the catalyst comprises the following steps: S1, mixing a palladium source with a solvent to form a solution; S2, adjusting the pH of the solution in S1 to 1-6; S3, mixing the carrier with the solution after adjusting the pH, drying, calcining and reducing to obtain the catalyst.

9. The method according to claim 8, characterized in that In step S2, the pH of the solution in S1 is adjusted to 2-4.

10. The method according to claim 8, characterized in that In S3, the mixing temperature is 50-90°C; And / or the mixing time is 10-60min; And / or the calcination temperature is 400-600°C; And / or the reducing atmosphere is a hydrogen-nitrogen mixed gas with a hydrogen content of 30-100% and an air velocity of 100-4000h -1 , the time is at least 5h and the pressure is below 2MPa.

11. The method according to claim 10, characterized in that In S3, the mixing temperature is 60-80°C; And / or the mixing time is 20-40 min.

12. The method according to claim 8, characterized in that The palladium source is selected from one or more of chloropalladic acid, palladium nitrate and palladium sulfate; and / or the solvent is selected from one or more of water and C1-C4 alkyl alcohol; and / or in S2, an acidic compound is used to adjust the pH of the solution in S1.

13. The method according to claim 12, characterized in that The solvent is selected from one or more of water, methanol and ethanol; And / or in S2, the acidic compound is selected from one or more of phosphoric acid, sulfuric acid, citric acid, nitric acid, acetic acid and hydrochloric acid.

14. The method according to any one of claims 1 to 3, characterized in that: The reaction pressure is 0.1-4.0MPa; and / or the reaction temperature is 30-100°C; and / or the volume space velocity of the mixture is 1-20h -1 ; And / or the reducing atmosphere is a hydrogen atmosphere.

15. The method according to claim 14, characterized in that The reaction pressure is 1-3.0MPa; and / or the volume space velocity of the mixture is 1-5h -1 ; And / or the molar ratio of hydrogen to diisopropylbenzene hydroperoxide is >4.

16. The method according to claim 15, characterized in that The molar ratio of hydrogen to diisopropylbenzene hydroperoxide is 5-7.