Nickel-platinum alloy target and its preparation method
By controlling the platinum content and process conditions of the nickel-platinum alloy target, ensuring that its hardness is within a specific range, the problems of high deformation and cracks of the nickel-platinum alloy target are solved, and its processability and quality are improved.
Patent Information
- Application Number
- CN202010629763.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-07-03
AI Technical Summary
Existing nickel-platinum alloy targets are prone to excessive deformation during plastic forming and heat treatment, resulting in target cracks, affecting their quality and processability.
By controlling the platinum content, average grain size and grain size variation of nickel-platinum alloy targets, ensuring that the hardness index is within the range of 100 to 150, and specific process conditions such as smelting, plastic forming and heat treatment temperature are used to reduce the temperature. Deformation and avoid cracks.
The low deformation and high machiningability of the nickel-platinum alloy target is achieved, which avoids cracks in the target after processing, and improves its quality and process performance.
Smart Images

Figure BDA0002568079790000051 
Figure BDA0002568079790000061 
Figure BDA0002568079790000071
Abstract
Description
Technical Field
[0001] The invention relates to a target material used in semiconductor technology and a preparation method thereof, in particular to a nickel-platinum alloy target material and a preparation method thereof. Background Art
[0002] Metal silicide has been widely used in semiconductor technology due to its excellent high-temperature oxidation resistance and good electrical and thermal conductivity. Specifically, metal silicide can reduce the contact resistance of transistors at the gate, source and drain, thereby increasing the driving current, response time or circuit operation speed of the entire component.
[0003] As semiconductor components develop towards smaller sizes, they are more significantly affected by resistance, so the research on metal silicide has attracted attention. Generally speaking, titanium silicide or cobalt silicide is usually used as the main material in complementary metal-oxide-semiconductor (CMOS) above 90 nanometers; when the CMOS process develops to below 65 nanometers, nickel silicide with better properties is used instead. In particular, when the CMOS process is below 45 nanometers, in order to improve the adverse effects of the short-channel effects that occur, oxide materials with high dielectric constants (such as hafnium dioxide) are usually selected to replace the silicon dioxide insulating layer, and nickel silicide with characteristics such as low resistance, low silicon consumption and low process temperature is used. However, nickel silicide has poor thermal stability and needs to be improved by adding platinum elements. Therefore, nickel-platinum alloy targets are one of the important sources for making nickel silicide.
[0004] In the prior art, research has been conducted on nickel-platinum alloy targets. For example, CN1926254A mentions that the nickel-platinum alloy after melting and casting is often too brittle and hard to be further processed into a target. In this regard, the patent case discloses that the problem of the nickel-platinum alloy after melting and casting being too brittle and hard to be further processed can be solved by increasing the purity of the nickel-platinum alloy raw material to more than 99.99%. However, during the further plastic forming and heat treatment of the nickel-platinum alloy ingot to obtain the nickel-platinum alloy target and the subsequent processing, the target material often has cracks due to excessive deformation, which affects its quality, but there is no corresponding solution yet.
[0005] Based on this, there is still a need to develop relevant research on reducing target deformation and avoiding target cracks in order to obtain high-quality nickel-platinum alloy targets. Summary of the invention
[0006] In view of the defects of the prior art, the purpose of the present invention is to control the hardness of the nickel-platinum alloy target within a specific range, so that the nickel-platinum alloy ingot can obtain a nickel-platinum alloy target with low deformation after plastic forming and heat treatment steps, and will not produce cracks after processing, that is, it has good machinability and maintains excellent quality.
[0007] To achieve the above-mentioned object, the present invention provides a nickel-platinum alloy target material, which comprises nickel and platinum; wherein the nickel-platinum alloy target material has the following characteristics:
[0008] a content of platinum atoms, based on the total number of atoms of the nickel-platinum alloy target, the content of platinum atoms (platinum content) is greater than or equal to 1 percent (%) and less than or equal to 20%, and its value when expressed in percentage is X;
[0009] an average grain size, the value of which is Y when expressed in micrometers;
[0010] 1. Grain size variation, the value of which is expressed in percentage as Z;
[0011] A hardness index, wherein the value of the hardness index is represented by H;
[0012] Wherein, H, X, Y and Z satisfy the following formula (I):
[0013] Formula (I): H = 10000 × (X ÷ Z) 1 / 10 ÷Y, and H is greater than or equal to 100 and less than or equal to 150.
[0014] By means of the above-mentioned technical means, the platinum content in the nickel-platinum alloy target is controlled within a specific range, and the values of the platinum content, the average grain size and the grain size variation of the nickel-platinum alloy target are further controlled to satisfy a specific relationship, so that the hardness index is greater than or equal to 100 and less than or equal to 150, thereby ensuring that the Vickers hardness of the nickel-platinum alloy target is within an appropriate range, thereby reducing the deformation of the nickel-platinum alloy target and avoiding the generation of cracks after processing, that is, improving its machinability to obtain a nickel-platinum alloy target of excellent quality.
[0015] According to the present invention, "X", "Y" and "Z" in formula (I) are respectively the values when the platinum content is expressed in percentage, the average grain size is expressed in micrometers, and the grain size variation is expressed in percentage. For example, if the platinum content of the nickel-platinum alloy target is 1%, the average grain size is 75 micrometers, and the grain size variation is 13%, then "X", "Y" and "Z" in formula (I) are respectively substituted into the calculation with "1", "75" and "13".
[0016] According to the present invention, the hardness index represents the specific relationship between the platinum content, average grain size and grain size variation of the nickel-platinum alloy target, but is not substantially equivalent to the real hardness of the nickel-platinum alloy target.
[0017] Preferably, the variation of the grain size of the nickel-platinum alloy target is less than 15%. More preferably, the variation of the grain size of the nickel-platinum alloy target is greater than or equal to 7% and less than 15%. Even more preferably, the variation of the grain size of the nickel-platinum alloy target is greater than or equal to 7% and less than or equal to 13%.
[0018] Preferably, the average grain size of the nickel-platinum alloy target is greater than or equal to 55 microns and less than or equal to 110 microns. More preferably, the average grain size of the nickel-platinum alloy target is greater than or equal to 60 microns and less than or equal to 100 microns. Even more preferably, the average grain size of the nickel-platinum alloy target is greater than or equal to 68 microns and less than or equal to 100 microns.
[0019] Preferably, based on the total number of atoms of the nickel-platinum alloy target, the platinum content is greater than or equal to 1% and less than or equal to 18%. More preferably, based on the total number of atoms of the nickel-platinum alloy target, the platinum content is greater than or equal to 1% and less than or equal to 17%.
[0020] Preferably, the Vickers hardness of the nickel-platinum alloy target is greater than or equal to 110 HV and less than or equal to 150 HV. More preferably, the Vickers hardness of the nickel-platinum alloy target is greater than or equal to 120 HV and less than or equal to 150 HV. When the nickel-platinum alloy target has the aforementioned hardness range, the deformation of the nickel-platinum alloy target can be further reduced and cracks in the target after processing can be avoided, thereby improving its machinability. In this specification, the Vickers hardness measured for the nickel-platinum alloy target refers to the Vickers hardness of the nickel-platinum alloy target after plastic forming.
[0021] To achieve the aforementioned object, the present invention further provides a method for preparing a nickel-platinum alloy target, which comprises the following steps:
[0022] Step (a): smelting and casting nickel and platinum to obtain a nickel-platinum alloy ingot, wherein the amount of platinum atoms added is greater than or equal to 1% and less than or equal to 20% based on the total number of nickel and platinum atoms;
[0023] Step (b): plastically forming the nickel-platinum alloy ingot, wherein the maximum temperature of the plastic forming is greater than or equal to 800° C. and less than or equal to 1200° C., and the total plastic forming amount of the nickel-platinum alloy ingot is greater than or equal to 90% and less than or equal to 95%; and
[0024] Step (c): performing heat treatment at 700° C. to 1000° C. to obtain the nickel-platinum alloy target.
[0025] By adding a specific content of platinum to the metal raw material and controlling the maximum temperature during plastic forming in the aforementioned process, the total plastic forming amount of the nickel-platinum alloy ingot and the temperature of the subsequent heat treatment within a specific range, the obtained nickel-platinum alloy target material can have a suitable hardness range, and thus has good machinability, low deformation and no cracking characteristics.
[0026] In step (a), the purity of platinum applicable to the present invention may be greater than 4N5, and the purity of nickel applicable to the present invention may be greater than 5N, that is, the purity of the selected platinum may be greater than 99.995%, and the purity of the selected nickel may be greater than 99.999%. Preferably, the purity of the prepared nickel-platinum alloy target may be greater than 5N (99.999%).
[0027] According to the present invention, the melting step may be performed by any conventional melting method. For example, the melting method may be vacuum induction melting (VIM), electron beam melting (EBM), vacuum arc remelting (VAR) or water-cooled copper crucible melting, but is not limited thereto.
[0028] According to the present invention, the plastic forming step can be performed by any conventional plastic forming method. For example, the plastic forming step can be performed by forging or rolling, and is not limited to hot forming or cold forming.
[0029] In step (c), after the heat treatment step, a processing step may be further included to obtain the nickel-platinum alloy target. The processing step may be any conventional target material processing method, for example, the processing step may be a turning process or a grinding process, but is not limited thereto.
[0030] Preferably, the maximum temperature of the plastic molding is greater than or equal to 850° C. and less than or equal to 1150° C. More preferably, the maximum temperature of the plastic molding is greater than or equal to 850° C. and less than or equal to 1000° C.
[0031] Preferably, the total plastic forming amount of the nickel-platinum alloy ingot is greater than or equal to 90% and less than or equal to 94%. More preferably, the total plastic forming amount of the nickel-platinum alloy ingot is greater than or equal to 90% and less than or equal to 93%.
[0032] Preferably, the temperature of the heat treatment is greater than or equal to 800° C. and less than or equal to 1000° C. More preferably, the temperature of the heat treatment is greater than or equal to 850° C. and less than or equal to 1000° C. DETAILED DESCRIPTION
[0033] In order to verify the influence of the specific relationship between the platinum content, average grain size and grain size variation of the nickel-platinum alloy target of the present invention on its hardness and machinability caused by controlling specific conditions in the process, several embodiments are listed below to illustrate the implementation mode of the present invention, and the difference in characteristics between each embodiment and the comparative example is explained; those skilled in the art can easily understand the advantages and effects that can be achieved by the present invention through the contents of this specification, and make various modifications and changes without departing from the spirit of the present invention to implement or apply the contents of the present invention.
[0034] Examples 1 to 6: Nickel-platinum alloy target
[0035] According to the conditions of different platinum contents listed in Table 1, a metal raw material containing nickel with a purity greater than 5N and platinum with a purity greater than 4N5 is prepared, the metal raw material is smelted to form a high-purity nickel-platinum alloy, and cast into a block-shaped nickel-platinum alloy ingot, and then the nickel-platinum alloy ingot is plastically formed, and the maximum temperature and the total plastic forming amount of the nickel-platinum alloy ingot are controlled within a specific range during the process, and then heat treatment is performed under a specific temperature range, and finally processed to a target size to obtain the nickel-platinum alloy target materials of Examples 1 to 6. The maximum temperature measured during plastic forming, the total plastic forming amount of the nickel-platinum alloy ingot, and the temperature conditions of the heat treatment of Examples 1 to 6 are respectively listed in the following Table 1.
[0036] Comparative Examples 1 to 5: Nickel-platinum alloy target
[0037] The implementation methods of Comparative Examples 1 to 5 are similar to those of Examples 1 to 6, that is, according to the conditions of different platinum contents listed in Table 1, the metal raw materials containing nickel and platinum are sequentially subjected to the steps of melting and casting, plastic forming, heat treatment and processing to obtain the nickel-platinum alloy targets of Comparative Examples 1 to 5. The differences lie in the conditions such as the maximum temperature of plastic forming, the total plastic forming amount of the nickel-platinum alloy ingot and the heat treatment temperature. The above-mentioned different conditions are also listed in Table 1 below.
[0038] Table 1: Platinum content of nickel-platinum alloy targets of Examples 1 to 6 and Comparative Examples 1 to 5, maximum temperature of plastic forming in the process, total plastic forming amount of nickel-platinum alloy ingots, and heat treatment temperature
[0039]
[0040] Test Example 1: Average grain size and grain size variation
[0041] This test example uses the nickel-platinum alloy target materials that have been plastically formed and heat-treated in Examples 1 to 6 and Comparative Examples 1 to 5 as the test samples. Specifically, test pieces of about 10 mm × 10 mm in size are taken from the center, half radius and edge of the target material, respectively. After the samples are prepared by grinding, polishing and etching, they are observed and captured using an optical microscope (model: OLYMPUS BX51M). Then, four cross-sections are drawn on the captured image using Image J Pro analysis software, two of which are diagonal lines of the image, and the other two are respectively the center line parallel to the long side and the center line parallel to the short side. The four cross-sections are arranged in a cross shape on each image.
[0042] Next, the total number of grains on the four sections is counted by sampling, and the length of each section is divided by the total number of grains to obtain the grain size on each section; then, the average grain size and its standard deviation of all sections are calculated using the data of the grain size on each section obtained by the above calculation. The percentage calculated by dividing the standard deviation by the average grain size represents the normalized uniformity of grain size. The larger the percentage of grain size uniformity, the more serious the degree of variation, and the more uneven the grain size of the sample to be tested. The analysis results of the average grain size and grain size variation of the nickel-platinum alloy targets of Examples 1 to 6 and Comparative Examples 1 to 5 are shown in Table 2.
[0043] Test Example 2: Hardness Analysis
[0044] This test example uses the nickel-platinum alloy target materials that have been plastically formed and heat-treated in Examples 1 to 6 and Comparative Examples 1 to 5 as the test samples. Specifically, test pieces of about 10 mm × 10 mm in size are taken from the center, half radius and edge of the target material, respectively. After the samples are prepared through grinding and polishing steps, the hardness is measured using a microhardness tester (model: SHIMADZU HMV-2). After the hardness value of each sample is measured on its polished surface, the hardness values of the above three different positions are averaged to serve as the hardness measurement value of the nickel-platinum alloy target materials of Examples 1 to 6 and Comparative Examples 1 to 5. The results are also listed in Table 2.
[0045] Test Example 3: Evaluation of target deformation and target cracks
[0046] In this test example, the target deformation amount is tested using the nickel-platinum alloy targets after plastic forming and heat treatment in Examples 1 to 6 and Comparative Examples 1 to 5 as the test samples. Specifically, the target is placed on a horizontal plane, and the warping degree of the target surface relative to the horizontal plane is measured with a square ruler, which is the evaluation result of the target deformation amount and is listed in Table 2.
[0047] Next, the evaluation of target cracks was performed by further processing the nickel-platinum alloy targets after plastic forming and heat treatment in the aforementioned Examples 1 to 6 and Comparative Examples 1 to 5 to the same size (φ450×4mm) under the same conditions, and then visually observing whether cracks were generated on their surfaces. The results of the evaluation of target cracks are also listed in Table 2.
[0048] In addition, based on the target deformation and target crack results obtained in the above-mentioned test example 3, the machinability of the nickel-platinum alloy target can be further evaluated. Specifically, the target deformation is greater than 0.3 mm and the target surface obtained after processing has obvious cracks, which is marked as △; the target deformation is approximately equal to 0.3 mm and the target surface obtained after processing has no cracks, which is marked as ○; the target deformation is less than 0.2 mm and the target surface obtained after processing has no cracks, which is marked as ◎. The results of the above-mentioned evaluation of the target machinability are listed in Table 2.
[0049] Table 2: Platinum content, hardness index, grain size variation, average grain size, Vickers hardness, target deformation, target crack and machinability of nickel-platinum alloy targets of Examples 1 to 6 and Comparative Examples 1 to 5
[0050]
[0051]
[0052] Discussion of experimental results
[0053] According to the contents of Table 1 and Table 2, the nickel-platinum alloy targets of Examples 1 to 6 control the maximum temperature of plastic forming, the total plastic forming amount of the nickel-platinum alloy ingot, and the heat treatment temperature within a specific range, so that the obtained nickel-platinum alloy targets have a specific average grain size and grain size variation under a specific platinum content, so that the hardness index is within a specific range, and thus have an appropriate Vickers hardness range, and have the effects of low target deformation and no cracking after further processing, thereby improving the machinability of the target and maintaining its excellent quality; on the other hand, the nickel-platinum alloy targets of Comparative Examples 1 to 5 do not control at least one of the maximum temperature of plastic forming, the total plastic forming amount of the nickel-platinum alloy ingot, and the heat treatment temperature within a specific range during the process, resulting in no specific relationship between the platinum content, the average grain size, and the grain size variation, resulting in the Vickers hardness of the target not being within a suitable range, not only the target deformation is high, but also the target is prone to cracking after processing, thereby affecting its machinability.
[0054] Further referring to the groups of Example 2, Comparative Example 1 and Example 4, Comparative Example 3, although the platinum content of Example 2 and Comparative Example 1 is 3%; the platinum content of Example 4 and Comparative Example 3 is 7%, the heat treatment temperatures of Comparative Example 1 and Comparative Example 3 are 550°C and 1100°C respectively, and are not in the range of 700°C to 1000°C, wherein 550°C is not higher than the recrystallization temperature of the alloy, and 1100°C is too high a temperature to cause grain growth. Both situations result in the average grain size and grain size variation of the nickel-platinum alloy targets of Comparative Example 1 and Comparative Example 3 being too high, and the hardness index is not in the range of 100 to 150, so that the Vickers hardness of the nickel-platinum alloy targets of Comparative Example 1 and Comparative Example 3 is too low, so a higher target deformation and cracks after processing can be observed, and the targets do not have good machinability.
[0055] Further referring to the groups of Example 3 and Comparative Example 2, although the platinum content is the same, the total plastic forming amount of the nickel-platinum alloy ingot in the process of Comparative Example 2 is less than 90%, resulting in insufficient kinetic energy for grain refinement, and also causing the average grain size and grain size variation of the nickel-platinum alloy target of Comparative Example 2 to be high, so that the hardness index is not in the range of 100 to 150, thereby reducing the Vickers hardness of the nickel-platinum alloy target of Comparative Example 2. Although no cracks are observed in the target after processing, the target still has a high deformation amount, which affects its machinability.
[0056] Further referring to the groups of Example 5 and Comparative Example 4, under the condition of the same platinum content of 10%, since the maximum temperature of the plastic forming in the process of Comparative Example 4 is significantly lower, the total plastic forming amount of the nickel-platinum alloy ingot is also insufficient and there is no significant grain refinement phenomenon, which makes the average grain size and grain size variation of the nickel-platinum alloy target of Comparative Example 4 too high and the hardness index cannot fall within the range of 100 to 150. The Vickers hardness of the nickel-platinum alloy target of Comparative Example 4 is measured to be only 97HV. It can be observed that the deformation of the target is high and cracks are generated after the target is processed, which is not conducive to subsequent processing.
[0057] Further referring to the group of Comparative Example 5, even though only the total plastic forming amount of the nickel-platinum alloy ingot is higher than 95% defined in the present invention, the hardness index of Comparative Example 5 is not in the range of 100 to 150. After measuring the Vickers hardness of the nickel-platinum alloy target of Comparative Example 5, it is 184HV. The excessively high hardness value leads to difficulties in subsequent processing.
[0058] Based on the results of the above test examples, it can be seen that the present invention controls the platinum content, the maximum plastic forming temperature, the total plastic forming amount of the nickel-platinum alloy ingot and the heat treatment temperature in the nickel-platinum alloy target process, so that the prepared nickel-platinum alloy target has a specific range of platinum content, average grain size and grain size variation, thereby obtaining a suitable hardness range, reducing the deformation of the target material and avoiding the generation of cracks in the target material after processing, specifically improving the machinability of the target material and maintaining the quality of the target material.
Claims
1. A nickel-platinum alloy target material, comprising nickel and platinum; wherein the nickel-platinum alloy target material has the following characteristics: A hardness index, wherein the value of the hardness index is represented by H, and H is greater than or equal to 100 and less than or equal to 150; a content of platinum atoms, based on the total number of atoms of the nickel-platinum alloy target, the content of platinum atoms is greater than or equal to 1 percent and less than or equal to 20 percent, and the value when the unit is expressed in percentage is X; an average grain size, whose value is Y when expressed in micrometers; and a grain size variation, wherein the grain size variation is less than 15%, and the value thereof when expressed in percentage is Z, and the grain size variation is a percentage calculated by dividing the standard deviation of the grain size by the average grain size; in, H, X, Y and Z satisfy the following formula (I): Formula (I): H = 10000 × (X ÷ Z) 1 / 10 ÷Y. 2 . The nickel-platinum alloy target material as claimed in claim 1 , wherein an average grain size of the nickel-platinum alloy target material is greater than or equal to 55 μm and less than or equal to 110 μm.
3. The nickel-platinum alloy target material as claimed in claim 1, wherein the content of the platinum atoms is greater than or equal to 1 atomic percent and less than or equal to 18 atomic percent based on the total number of atoms of the nickel-platinum alloy target material. 4 . The nickel-platinum alloy target according to claim 1 , wherein the Vickers hardness of the nickel-platinum alloy target is greater than or equal to 110 HV and less than or equal to 150 HV.
5. A method for preparing a nickel-platinum alloy target, comprising the following steps: Step (a): smelting and casting nickel and platinum to obtain a nickel-platinum alloy ingot, wherein the amount of platinum atoms added is greater than or equal to 1% and less than or equal to 20% based on the total number of nickel and platinum atoms; Step (b): plastically forming the nickel-platinum alloy ingot, wherein the maximum temperature of the plastic forming is greater than or equal to 800° C. and less than or equal to 1200° C., and the total plastic forming amount of the nickel-platinum alloy ingot is greater than or equal to 90% and less than or equal to 95%; as well as Step (c): performing heat treatment at 850° C. to 1000° C. to obtain the nickel-platinum alloy target.
6. The method according to claim 5, wherein the maximum temperature of the plastic forming is greater than or equal to 850°C and less than or equal to 1150°C.
7. The method according to claim 5, wherein the total plastic forming amount of the nickel-platinum alloy ingot is greater than or equal to 90% and less than or equal to 94%.
Citation Information
Patent Citations
Ni-Pt alloy and Ni-Pt alloy target
CN1926254A
Ultra-high purity NiPt alloys and sputtering targets comprising same
CN101353732A
Nickel-platinum alloy target and preparation method thereof
CN104018120A
Nickel-platinum alloy sputtering target material and preparation method thereof
CN104018128A
Ni-pt alloy and target comprising the alloy
US20070098590A1