Film capacitor and film for film capacitor
By using a dielectric resin film with a high glass transition temperature and moderate density in the film capacitor, combined with the design of the metal layer, the problem of reduced voltage resistance of the film capacitor under high temperature conditions is solved, and high-reliability insulation breakdown is achieved. Strength and voltage resistance.
Patent Information
- Application Number
- CN202080039466.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-09
- Filing Date
- 2020-02-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-02-25
AI Technical Summary
The voltage resistance of existing film capacitors drops significantly under high temperature conditions, and the breakdown voltage has large deviations, making it difficult to maintain high reliability in harsh environments.
Using a dielectric resin film with a glass transition temperature of 160°C or higher and a film capacitor with a density of 1.22g/cm3 or more and 1.26g/cm3 or less at 25°C, a metal layer is provided on the dielectric resin film to form a winding type Or laminated structure to improve insulation breakdown strength.
It provides sufficient dielectric breakdown strength and excellent voltage resistance in high temperature environments, ensuring the high reliability of film capacitors.
Smart Images

Figure CN113892153B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a film capacitor and a film for the film capacitor. Background Art
[0002] As one type of capacitor, there is a film capacitor having the following structure, that is, a flexible resin film is used as a dielectric, and a first opposing electrode and a second opposing electrode are arranged opposite to each other through the resin film. The film capacitor is usually in the form of a roughly cylindrical shape formed by winding a resin film as a dielectric, and a first external terminal electrode and a second external terminal electrode are formed on the first end face and the second end face of the cylinder facing each other, respectively. In addition, the first opposing electrode is electrically connected to the first external terminal electrode, and the second opposing electrode is electrically connected to the second external terminal electrode.
[0003] Patent document 1 discloses a capacitor, characterized in that the dielectric is composed of a polymer film, and the conductor is composed of a metal foil or a metal film, wherein the polymer film contains a polyester containing 50 mol % or more of a specific repeating unit, and has a refractive index in the thickness direction of 1.50 to 1.57 and a density of 1.45 to 1.50 g / cm 3 , the amount of extracted low molecular weight components is less than 1.0% by weight.
[0004] Prior Art Literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 60-180008 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Patent Document 1 states that the density of the polyester film constituting the dielectric needs to be 1.45 to 1.50 g / cm 3 The range is preferably 1.46 to 1.48 g / cm 3 According to Patent Document 1, if the density of the film is less than the above range, the deviation of the breakdown voltage of the capacitor becomes larger, and conversely, if the density is greater than the above range, the breakdown voltage of the capacitor becomes smaller and its deviation becomes larger, which is not preferred.
[0009] However, in the invention described in Patent Document 1, the breakdown voltage of the capacitor is evaluated at 25°C, and the withstand voltage significantly decreases under higher temperature conditions. Film capacitors are expected to be used in harsh environments such as in vehicles, so they need to show high reliability even under high temperature conditions.
[0010] The present invention is made to solve the above-mentioned problems, and its object is to provide a film capacitor having a dielectric resin film having sufficient insulation breakdown strength under high temperature environment. The present invention also aims to provide a film for a film capacitor used as the dielectric resin film of the above-mentioned film capacitor.
[0011] Technical solutions to solve problems
[0012] The film capacitor of the present invention is a film capacitor comprising a dielectric resin film and a metal layer provided on one surface of the dielectric resin film, wherein the glass transition temperature of the dielectric resin film is 160° C. or higher and the density at 25° C. is 1.22 g / cm 3 Above 1.26g / cm 3 the following.
[0013] The film for a film capacitor of the present invention has a glass transition temperature of 160° C. or higher and a density of 1.22 g / cm at 25° C. 3 Above 1.26g / cm 3 the following.
[0014] Effects of the Invention
[0015] According to the present invention, it is possible to provide a film capacitor including a dielectric resin film having sufficient dielectric breakdown strength in a high temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 FIG. 1 is a cross-sectional view schematically showing an example of a thin film capacitor of the present invention. DETAILED DESCRIPTION
[0017] Hereinafter, the film capacitor and the film for the film capacitor of the present invention will be described.
[0018] However, the present invention is not limited to the following configurations, and can be applied with appropriate changes within the scope of the present invention.
[0019] A combination of two or more of the preferred structures of the present invention described below also constitutes the present invention.
[0020] [Film capacitors]
[0021] A film capacitor of the present invention includes a dielectric resin film and a metal layer provided on one surface of the dielectric resin film.
[0022] Hereinafter, as an embodiment of the film capacitor of the present invention, a winding type film capacitor is described as an example, in which a first dielectric resin film having a first metal layer and a second dielectric resin film having a second metal layer are wound in a stacked state.
[0023] Furthermore, the film capacitor of the present invention may be a laminated film capacitor or the like in which a first dielectric resin film provided with a first metal layer and a second dielectric resin film provided with a second metal layer are laminated.
[0024] Figure 1 FIG. 1 is a cross-sectional view schematically showing an example of a thin film capacitor of the present invention.
[0025] Figure 1 The film capacitor 1 shown is a wound film capacitor, comprising a first dielectric resin film 11 and a second dielectric resin film 12 in a wound state, and a first metal layer (first opposing electrode) 21 and a second metal layer (second opposing electrode) 22 that are opposite to each other with the first dielectric resin film 11 or the second dielectric resin film 12 interposed therebetween, and comprising a first external terminal electrode 31 electrically connected to the first metal layer 21 and a second external terminal electrode 32 electrically connected to the second metal layer 22.
[0026] The first metal layer 21 is formed on the first dielectric resin film 11, and the second metal layer 22 is formed on the second dielectric resin film 12. The first dielectric resin film 11 on which the first metal layer 21 is formed and the second dielectric resin film 12 on which the second metal layer 22 is formed are wound in a stacked state, thereby forming the film capacitor 1. The second dielectric resin film 12 may have a different structure from that of the first dielectric resin film 11, but preferably has the same structure as that of the first dielectric resin film 11.
[0027] The first metal layer 21 is formed on one surface of the first dielectric resin film 11 so as to reach one side edge but not the other side edge. On the other hand, the second metal layer 22 is formed on one surface of the second dielectric resin film 12 so as to reach the other side edge but not the one side edge. The first metal layer 21 and the second metal layer 22 are composed of, for example, aluminum layers or the like.
[0028] like Figure 1As shown, the first dielectric resin film 11 and the second dielectric resin film 12 are stacked with the film offset in the width direction so that the end of the first metal layer 21 on the side reaching the side edge of the first dielectric resin film 11 and the end of the second metal layer 22 on the side reaching the side edge of the second dielectric resin film 12 are exposed from the stacked films. The first dielectric resin film 11 and the second dielectric resin film 12 are wound in a stacked state, thereby setting the stacked state in which the first metal layer 21 and the second metal layer 22 are kept exposed at the end.
[0029] exist Figure 1 In the film capacitor 1 shown, the second dielectric resin film 12 is wound outside the first dielectric resin film 11, and the first metal layer 21 and the second metal layer 22 of each of the first dielectric resin film 11 and the second dielectric resin film 12 are oriented inward.
[0030] The first external terminal electrode 31 and the second external terminal electrode 32 are formed by spraying, for example, zinc, on each end surface of the capacitor body obtained as described above. The first external terminal electrode 31 is in contact with the exposed end portion of the first metal layer 21, thereby being electrically connected to the first metal layer 21. On the other hand, the second external terminal electrode 32 is in contact with the exposed end portion of the second metal layer 22, thereby being electrically connected to the second metal layer 22.
[0031] In the film capacitor of the present invention, the wound body of the dielectric resin film is preferably pressed into a flat shape such as an ellipse or an oblong shape, and is set to a shape that is more compact than when the cross-sectional shape is a perfect circle. In addition, the film capacitor of the present invention may also have a cylindrical winding shaft. The winding shaft is arranged on the central axis of the dielectric resin film in the wound state, and becomes the winding shaft when the dielectric resin film is wound.
[0032] In the thin film capacitor of the present invention, examples of the metal contained in the metal layer include aluminum (Al), titanium (Ti), zinc (Zn), magnesium (Mg), tin (Sn), and nickel (Ni).
[0033] In the thin film capacitor of the present invention, the thickness of the metal layer is not particularly limited, and is, for example, 5 nm to 40 nm.
[0034] The thickness of the metal layer can be determined by observing a cross section of a dielectric resin film provided with the metal layer cut in the thickness direction using an electron microscope such as a field emission scanning electron microscope (FE-SEM).
[0035] In the film capacitor of the present invention, the film for a film capacitor of the present invention is used as the dielectric resin film.
[0036] [Film for film capacitors]
[0037] The film for a film capacitor of the present invention is characterized in that the glass transition temperature is 160° C. or higher and the density at 25° C. is 1.22 g / cm 3 Above 1.26g / cm 3 the following.
[0038] The glass transition temperature of the film is set to 160°C or higher and the density of the film at 25°C is set to 1.22 g / cm 3 Above 1.26g / cm 3 If the dielectric breakdown strength of the film is increased to less than 125° C., the film can be provided with excellent voltage resistance in a high temperature environment.
[0039] It can be considered that the dielectric breakdown of film occurs easily at the hollow in the film. It can be considered that by improving the density of the film, the film densification, the hollow in the film decreases, so the dielectric breakdown strength increases, and the withstand voltage improves. It can be considered that when the density of the film is low, the distance between the molecules of the composition increases, so the cross-linking density after the thermal curing does not improve, and the withstand voltage decreases. On the other hand, if the density of the film becomes too high, the film formation is unstable, so the dielectric breakdown strength decreases instead, and the withstand voltage decreases. In addition, it can be considered that the higher the density of the film, the lower the toughness of the film, and this also has an impact on the decline of the withstand voltage.
[0040] The density of a film can be found by dividing the weight of the film by its volume. The volume of the film is calculated based on the area and average thickness of the film.
[0041] Alternatively, the storage modulus can be measured using a dynamic viscoelasticity measuring device (DMA), and the glass transition temperature of the film can be determined from the temperature at which the storage modulus begins to drop significantly.
[0042] In the film for a film capacitor of the present invention, the upper limit of the glass transition temperature is not particularly limited, and the glass transition temperature is, for example, 250° C. or lower.
[0043] The film for a film capacitor of the present invention preferably contains a curable resin as a main component. The curable resin may be a thermosetting resin or a photocurable resin.
[0044] In this specification, the so-called "main component" means the component with the largest weight percentage, preferably, the component with a weight percentage exceeding 50% by weight. Therefore, the film for film capacitors of the present invention may also contain additives such as silicone resin, uncured parts of starting materials such as the first organic material and the second organic material described later as components other than the main component.
[0045] In this specification, the so-called thermosetting resin means a resin that can be cured by heat, and the curing method is not limited. Therefore, as long as it is a resin that can be cured by heat, a resin that has been cured by a method other than heat (for example, light, electron beam, etc.) is also included in the thermosetting resin. In addition, depending on the material, there is a situation where the reaction starts by the reactivity of the material itself, and a curable resin that does not necessarily need to be cured by heat or light from the outside is also considered a thermosetting resin. The same is true for light-curing resins, and the curing method is not limited.
[0046] The curable resin may have at least one of a urethane bond and a urea bond, or may not have a urethane bond and a urea bond.
[0047] In addition, the presence of the urethane bond and / or the urea bond can be confirmed using a Fourier transform infrared spectrophotometer (FT-IR).
[0048] The thin film capacitor film of the present invention preferably includes a cured product of the first organic material and the second organic material, for example, a cured product obtained by reaction of a hydroxyl group (OH group) of the first organic material and an isocyanate group (NCO group) of the second organic material.
[0049] In the case of obtaining a cured product through the above-mentioned reaction, an uncured portion of the starting material may remain in the film. For example, the film for a film capacitor of the present invention may also contain at least one of a hydroxyl group and an isocyanate group. In this case, the film for a film capacitor of the present invention may contain either a hydroxyl group or an isocyanate group, or may contain both a hydroxyl group and an isocyanate group.
[0050] In addition, the presence of the isocyanate group and / or the hydroxyl group can be confirmed using a Fourier transform infrared spectrophotometer (FT-IR).
[0051] The first organic material is preferably a polyol having a plurality of hydroxyl groups in the molecule. Examples of the polyol include polyether polyol, polyester polyol, and polyvinyl alcohol acetal. As the first organic material, two or more organic materials may be used in combination.
[0052] The first organic material preferably has an epoxy group. In particular, the first organic material is preferably a phenoxy resin, and more preferably a high molecular weight bisphenol A type epoxy resin having an epoxy group at the end.
[0053] The second organic material is preferably a polyisocyanate having a plurality of isocyanate groups in the molecule. The second organic material reacts with the hydroxyl group of the first organic material to form a crosslinked structure, thereby functioning as a curing agent for curing the thin film.
[0054] As polyisocyanates, for example, aromatic polyisocyanates such as diphenylmethane diisocyanate (MDI) and toluene diisocyanate (TDI), aliphatic polyisocyanates such as hexamethylene diisocyanate (HDI), etc. can be cited. Modified bodies of these polyisocyanates can also be used, for example, modified bodies having carbodiimide or urethane can also be used. Among them, aromatic polyisocyanates are preferred, MDI or TDI is more preferred, and MDI is further preferred. As MDI, typical polymeric MDI or monomeric MDI can be used. In addition, MDI can also be a mixture type. As TDI, trimethylolpropane (TMP) adducts can be used. In addition, biuret modified bodies of TDI can also be used. As the second organic material, two or more organic materials can also be used in combination.
[0055] In the film capacitor film of the present invention, the weight ratio of the first organic material to the second organic material (first organic material / second organic material) is not particularly limited, but is preferably 10 / 90 or more, more preferably 20 / 80 or more, and further preferably 30 / 70 or more. In addition, it is preferably 90 / 10 or less, more preferably 80 / 20 or less, and further preferably 70 / 30 or less. In particular, it is preferred that the weight ratio of the first organic material to the second organic material (first organic material / second organic material) exceeds 50 / 50.
[0056] The film for film capacitors of the present invention may also contain additives for adding other functions. For example, smoothness can be imparted by adding a leveling agent. The additive is more preferably a material having a functional group that reacts with a hydroxyl group and / or an isocyanate group and forms a part of the cross-linked structure of the cured product. As such a material, for example, a resin having at least one functional group selected from the group consisting of a hydroxyl group, an epoxy group, a silanol group, and a carboxyl group can be cited.
[0057] The film for a film capacitor of the present invention is preferably obtained by molding a resin solution containing the first organic material and the second organic material into a film shape, and then performing a heat treatment to cure the film.
[0058] The resin solution is prepared, for example, by dissolving the first organic material and the second organic material in a solvent, mixing the mixture, and adding additives as needed. In addition, the solvent contained in the resin solution may remain as a residue in the film after curing.
[0059] The solvent contained in the resin solution becomes gas by heating such as heat treatment, and forms voids in the film. Therefore, if the amount of solvent in the resin solution is too much, a large amount of volatile gas is generated, thereby forming many voids, and there is a tendency for the density of the film to decrease. Therefore, when the ratio of the total weight of the first organic material and the second organic material in the resin solution is taken as the resin concentration, the resin concentration in the resin solution is preferably 5% by weight or more and 50% by weight or less.
[0060] As the solvent, a mixed solvent containing a first solvent selected from ketones and a second solvent selected from cyclic ether compounds is preferably used. Examples of ketones include methyl ethyl ketone and diethyl ketone. Examples of cyclic ether compounds include tetrahydrofuran and tetrahydropyran. The weight ratio of the first solvent to the second solvent (first solvent / second solvent) is preferably 15 / 85 or more and 85 / 15 or less.
[0061] The thickness of the film for the film capacitor of the present invention is not particularly limited, but if the film is too thin, it tends to become brittle, while if the film is too thick, defects such as cracks tend to occur during film formation. Therefore, the thickness of the film for the film capacitor of the present invention is preferably 1 μm or more and 10 μm or less.
[0062] The thickness of the thin film refers to the thickness of the thin film alone excluding the thickness of the metal layer. The thickness of the thin film can be measured using an optical interference film thickness meter.
[0063] In the film for a film capacitor of the present invention, a metal layer may be provided on one surface. In this case, it is preferred that a metal layer having a fuse portion is provided on one surface.
[0064] The so-called fuse portion means a portion where the electrode portion and the electrode portion are connected to each other by dividing the metal layer that will become the opposing electrode into a plurality of electrodes. The pattern of the metal layer having the fuse portion is not particularly limited, and for example, the electrode patterns disclosed in Japanese Patent Publication No. 2004-363431, Japanese Patent Publication No. 5-251266, etc. can be used.
[0065] Example
[0066] Hereinafter, examples are shown which more specifically disclose the thin film for a thin film capacitor of the present invention. However, the present invention is not limited to these examples.
[0067] [Thin film production]
[0068] (Film 1 ~ Film 5)
[0069] A phenoxy resin was prepared as the first organic material, and MDI (4,4'-diphenylmethane diisocyanate) was prepared as the second organic material.
[0070] As the phenoxy resin, a phenoxy resin which is a high molecular weight bisphenol A type epoxy resin having an epoxy group at the terminal is used.
[0071] As the MDI, Millionate MTL (manufactured by Tosoh Corporation) was used.
[0072] The first organic material and the second organic material dissolved in methyl ethyl ketone (MEK) were mixed, and then diluted with a mixed solvent containing MEK and tetrahydrofuran (THF). The weight ratio of the first organic material and the second organic material in the obtained resin solution was first organic material / second organic material=66.5 / 33.5. In addition, the weight ratio of MEK and THF was MEK / THF=50 / 50.
[0073] In the present example, as shown in Table 1, the total weight of the phenoxy resin and MDI in the resin solution (resin concentration) was adjusted to 5 wt %, 10 wt %, 15 wt %, 25 wt % or 50 wt %.
[0074] The obtained resin solution was molded on a PET film by a knife coater, and the solvent was dried to obtain an uncured film with a thickness of 3 μm. The film was then treated in a hot air oven set at 150° C. for 4 hours to be thermally cured, and then peeled from the PET film to obtain a film.
[0075] (Film 6 ~ Film 10)
[0076] A phenoxy resin was prepared as the first organic material, and a modified TDI (toluene diisocyanate) was prepared as the second organic material.
[0077] As the phenoxy resin, a phenoxy resin which is a high molecular weight bisphenol A type epoxy resin having an epoxy group at the terminal is used.
[0078] As the TDI, Coronate L (manufactured by Tosoh Corporation) was used.
[0079] The first organic material and the second organic material dissolved in MEK were mixed, and then diluted with a mixed solvent containing MEK and THF. The weight ratio of the first organic material and the second organic material in the obtained resin solution was first organic material / second organic material=66.5 / 33.5. In addition, the weight ratio of MEK and THF was MEK / THF=50 / 50.
[0080] In the present example, as shown in Table 2, the resin solution was prepared so that the total weight of the phenoxy resin and TDI (resin concentration) was 5 wt %, 10 wt %, 15 wt %, 25 wt % or 50 wt %.
[0081] The obtained resin solution was molded on a PET film by a knife coater, and the solvent was dried to obtain an uncured film with a thickness of 3 μm. The film was then treated in a hot air oven set at 150° C. for 4 hours to be thermally cured, and then peeled from the PET film to obtain a film.
[0082] (Film 11)
[0083] A polypropylene (PP) film having a thickness of 2.8 μm was prepared.
[0084] [Evaluation of film]
[0085] The following properties were evaluated for the films 1 to 11 .
[0086] (Determination of dielectric breakdown strength)
[0087] Aluminum vapor-deposited electrodes (the electrode area of the overlapping portion was 30 cm) were formed on both sides of each film. 2 ) was prepared as an evaluation sample. A voltage of 100 V / μm was applied to the prepared sample for 10 minutes, and then the voltage was increased at intervals of 25 V / μm. Each voltage was maintained for 10 minutes, and the electric field strength when a breakdown mark was produced in the film was recorded. The measurement was continued at a total of 16 locations until a breakdown was observed. Based on the recorded results, a Weibull plot was made, and the value at which the failure rate reached 50% was taken as the insulation breakdown strength. The peripheral temperature of the film during the measurement was set to 125°C.
[0088] (Determination of density)
[0089] The weight of each film was determined, and the density of the film was determined by dividing the weight by the volume.
[0090] For each film, 80 samples cut into 100 mm × 50 mm were prepared and the weight of the samples was measured. Then, the thickness of the film was measured using an optical interference film thickness meter (manufactured by Filmetrics), and the volume of the film was calculated based on the obtained results and the area of the film. As the thickness of the film, the average thickness of a total of 400 points was used. Based on the results obtained by the above measurement, the density of the film was calculated. The measurement temperature was set to 25°C.
[0091] (Determination of glass transition temperature)
[0092] Each film was fixed to a width of 5 mm × a length of 6 mm, and the glass transition temperature of the film was measured using a dynamic viscoelasticity measuring device RSA3 (manufactured by TA Instruments Japan). The temperature was raised from 40°C to 230°C at a heating rate of 20°C / min, and the temperature at which the storage elastic modulus began to drop significantly was taken as the glass transition temperature.
[0093] Regarding Film 5 and Film 10, the crystallinity of the films was too high, so the toughness was extremely low, and the glass transition temperature could not be measured.
[0094] [Table 1]
[0095]
[0096] [Table 2]
[0097]
[0098] [Table 3]
[0099]
[0100] In Tables 1 to 3, films marked with * are comparative examples outside the scope of the present invention.
[0101] According to Table 1, in the film obtained by thermally curing the mixture of phenoxy resin and MDI, if the density of the film is 1.23 g / cm 3 Above 1.26g / cm 3 Below, the dielectric breakdown voltage of the film becomes 390V / μm or more. In particular, when the density of the film is 1.26g / cm 3 In the case of , the dielectric breakdown strength of the film is 430 V / μm, which is the highest.
[0102] On the other hand, the density of the film is 1.21 g / cm 3 or 1.37 g / cm 3 In the case of , the dielectric breakdown strength of the film is significantly reduced. It can be said that when the density of the film is too low or too high, sufficient dielectric breakdown strength cannot be maintained.
[0103] According to Table 2, in the film obtained by thermally curing the mixture of phenoxy resin and TDI, if the density of the film is 1.22 g / cm 3 Above 1.26g / cm 3 Below, the dielectric breakdown voltage of the film becomes 400V / μm or more. In particular, when the density of the film is 1.26g / cm 3 In the case of , the dielectric breakdown strength of the film is 440 V / μm, which is the highest.
[0104] On the other hand, when the density of the film is 1.20 g / cm 3 or 1.41 g / cm 3 In the case of , the dielectric breakdown strength of the film is significantly reduced. It can be said that when the density of the film is too low or too high, sufficient dielectric breakdown strength cannot be maintained.
[0105] According to Table 3, the density of the film is 0.86 g / cm 3 In the PP film, the insulation breakdown voltage of the film is as low as 270V / μm.
[0106] Furthermore, the glass transition temperatures of films 2 to 4 and films 7 to 8 are all 160° C. or higher, showing high heat resistance. From the above, it can be said that in order to show excellent dielectric breakdown strength at high temperatures, the film needs to have a high density and a high glass transition temperature.
[0107] Description of Reference Numerals
[0108] 1: Film capacitor;
[0109] 11: first dielectric resin film;
[0110] 12: second dielectric resin film;
[0111] 21: first counter electrode (first metal layer);
[0112] 22: second counter electrode (second metal layer);
[0113] 31: 1st external terminal electrode;
[0114] 32: Second external terminal electrode.
Claims
1. A film capacitor comprising: a dielectric resin film; and A metal layer is provided on one surface of the dielectric resin film, in, The glass transition temperature of the dielectric resin film is above 160° C., and the density at 25° C. is 1.22 g / cm 3 Above and 1.26g / cm 3 the following, The dielectric resin film includes a cured product of a first organic material and a second organic material. The first organic material is a phenoxy resin having a plurality of hydroxyl groups and epoxy groups in the molecule. The second organic material is a polyisocyanate having a plurality of isocyanate groups in a molecule.
2. A film for a film capacitor, wherein: The glass transition temperature is 160°C or higher, and the density at 25°C is 1.22 g / cm 3 Above and 1.26g / cm 3 the following, A cured product comprising a first organic material and a second organic material, The first organic material is a phenoxy resin having a plurality of hydroxyl groups and epoxy groups in the molecule. The second organic material is a polyisocyanate having a plurality of isocyanate groups in a molecule.