A method for improving the quality of CGA device mold-free column connection

By forming a tin-containing coating on the surface of the soldering posts of CGA devices and performing low-temperature aging treatment, the heterogeneous interface is transformed into a homogeneous interface, which solves the problem of insufficient connection strength of mold-less posts in CGA devices and achieves higher connection quality and reliability. sex.

CN113921406BActive Publication Date: 2024-10-08SHANDONG KAINENG ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111182390.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-11
Publication Date
2024-10-08
Estimated Expiration
2041-10-11

AI Technical Summary

Technical Problem

The quality of mold-free post-mounted connection of CGA devices is limited by the grinding away of the scalloped intermetallic compounds at the interface, the thinness of the residual interface connection layer, the disparity in properties of dissimilar materials, and the insufficient connection strength caused by differences in thermophysical states.

Method used

A tin-containing coating is formed on the surface of the welding pillar and subjected to low-temperature aging treatment to form a continuous intermetallic compound layer, transforming the heterogeneous interface into a homogeneous interface, and achieving reliable connection through the rotation and pressing pillar planting technology.

Benefits of technology

Significantly improves the connection strength of CGA devices without mold pillars, solves the problems of weak interface connection layer, poor performance of dissimilar materials and vibration, and achieves higher connection quality and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113921406B_ABST
    Figure CN113921406B_ABST
Patent Text Reader

Abstract

A method for improving the connection quality of moldless column planting of CGA devices relates to the field of microelectronic packaging technology, and is intended to solve the problem of limited connection strength caused by continuous grinding of interface compounds during connection, and excessive thinness and discontinuity of the residual interface connection layer during moldless column planting of copper columns of CGA devices. The present invention manufactures a tin-containing coating on the surface of the solder column and then performs low-temperature aging to form a compound layer at the interface of the solder column / tin-containing coating; prints solder paste on the array-arranged pads, and heats to form an array of spherical crown solder balls; mounts the tin-coated solder column in the chuck of a high-precision drill press, rotates the solder column and slowly presses its end downward to drill into the spherical crown solder ball aligned with it to a predetermined depth, then stops feeding and rotating, opens and lifts the drill press chuck after cooling, and completes the column planting of a single tin-coated solder column; and implements the column planting of the tin-coated solder column on the array-arranged pads one by one with the same parameters, and ensures that the exposed ends are coplanar. The present invention is used for column planting of CGA devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microelectronic packaging, and in particular to a method for improving the quality of mold-free column connection of a CGA device. Background Art

[0002] Column Grid Array (CGA) packaging is a preferred packaging technology for high-frequency, high-power, high-I / O, and large-chip devices. Since its introduction, it has been widely used in aerospace, communications, military, automotive electronics, and other fields because its higher solder pillars can effectively improve the heat dissipation capacity of the device during thermal cycles and effectively alleviate the stress caused by the difference in thermal expansion coefficients between the chip carrier substrate and the printed circuit board. However, it is extremely difficult to arrange and connect the solder pillars with large aspect ratios and poor stability. The traditional method of using molds to position copper pillars and reflow soldering connections has problems such as high precision mold costs, poor mold versatility, easy scratches on solder pillars when removing molds after welding, and the presence of molds during welding affecting the effective transfer of heat from the heat source and the emission of flux gas in the solder paste, high porosity, and poor wettability.

[0003] In 2017, a pillar planting method for CuCGA devices was proposed. This method uses a micro-precision drilling machine to clamp the copper pillar and align it with the solder ball on the substrate array pad, so that the copper pillar rotates at a specific speed and presses down to drill into the solder ball to a predetermined depth. The friction heat-force between the copper pillar and the solder ball is used to achieve the positioning and connection of the copper pillar, so as to achieve the purpose of mold-free pillar planting. This mold-free pillar planting method does not require a set of high-precision molds to be customized for each array specification device, which greatly reduces the cost and is suitable for the production of CGA devices of various specifications; the process temperature of this method is much lower than reflow soldering and is easy to automate; this method does not require the setting of positioning molds between the array copper pillars, so there is no problem of pores and poor solder joint wetting caused by the existence of the mold affecting the effective transfer of heat from the heat source and the emission of flux gas in the solder paste during the welding process; there is also no problem of scratching and bending of the solder pillars due to the removal of the mold after welding, which damages the coplanarity of the copper pillars. However, with the deepening of research, it was found that this method has the following problems:

[0004] (1) During the connection process, the scalloped interface connection layer formed by the atomic interdiffusion at the interface of the copper pillar / solder ball is continuously polished away. The residual interface connection layer after welding is too thin and discontinuous, which limits the further improvement of the connection strength.

[0005] (2) The connection between the copper pillar and the solder ball is a dissimilar material connection. The thermal physical and mechanical properties of copper and solder are quite different, resulting in a large difference in the thermal physical state between the two during the pillar planting. The plastically deformed solder has weak adhesion to the copper pillar, and further improvement of the connection strength is limited by this.

[0006] (3) The connection between the copper pillar and the solder ball is a dissimilar material connection. The thermal physical and mechanical properties of copper and solder are quite different. The copper pillar is prone to vibration during pillar planting, the solder near the interface of the solder ball is easy to soften, and the elastic clamping force between the copper pillar / solder ball is low. Further improvement of the connection strength is limited by this. Summary of the invention

[0007] The present invention aims to solve the problem that the connection quality of the existing CGA device array copper pillar without mold-assisted pillar planting is limited by the scallop-shaped intermetallic compounds on the interface being continuously polished away during the connection, the residual interface connection layer being too thin and discontinuous, and the problem that the connection strength is limited by the great difference in performance between the copper pillar and the solder ball, the great difference in the thermal physical state during the connection, and the weak adhesion and holding force.

[0008] A method for improving the quality of mold-free column connection of CGA devices comprises the following steps:

[0009] Step 1: Preparation of tin-containing coating on the surface of solder column:

[0010] A tin-containing coating is formed on the surface of a standard-sized solder column by hot-dip tinning or electroplating, followed by a necessary cleaning process to prevent residual substances on the surface of the tin-containing coating that may affect subsequent connections.

[0011] Step 2: performing low-temperature aging treatment on the solder column containing the tin coating so as to form a continuous intermetallic compound layer having a suitable thickness and morphology at the interface of the solder column / tin coating;

[0012] Step 3: Print an appropriate amount of solder paste on the pads arranged in the array;

[0013] Step 4, heating the solder paste to wet the pads arranged in the array, forming an array of spherical crown-shaped solder balls with consistent height;

[0014] Step 5: Planting of a single tin-coated solder column:

[0015] The tin-containing coating solder column is clamped in the chuck of the micro-precision drilling machine, and the movement of the substrate where the column pad to be planted is located is controlled by the program so that the tin-containing coating solder column is located above the column pad to be planted and is aligned with the center of the pad. The chuck of the micro-precision drilling machine is used to drive the tin-containing coating solder column to rotate, and the end of the tin-containing coating solder column is slowly pressed down at a uniform speed to drill into the spherical crown-shaped solder ball to a predetermined depth S, and then the feeding movement and rotation of the tin-containing coating solder column are stopped, and then the tin-containing coating solder column remains stationary until the spherical crown-shaped solder ball cools to room temperature; the chuck of the drilling machine is opened and lifted, so that the tin-containing coating solder column remains in the spherical crown-shaped solder ball on the pad, and the column planting connection of a single tin-containing coating solder column is completed;

[0016] Step 6: Planting of tin-coated solder columns of the array:

[0017] Repeat the process of step 5 above with the same size parameters and process parameters to implement the process of implanting the tin-coated solder pillars on each array-arranged pad one by one, and ensure that the exposed ends of the array tin-coated solder pillars are coplanar after implantation.

[0018] Preferably, the solder column described in step 1 is any one of a copper column, a brass column, an iron-nickel alloy column, and an iron-nickel-cobalt alloy column of uniform specifications and sizes prepared according to standards. Preferably, the aspect ratio of the solder column is in the range of 6 to 20, and the diameter d of the solder column is not less than 1 / 5 of the pad diameter D and not more than 1 / 3 of the pad diameter D.

[0019] Preferably, the tin-containing coating described in step 1 can be any one of a pure tin coating, a SnCu-based solder coating, a SnAg-based solder coating, a SnAgCu-based solder coating, a SnSb-based solder coating, a SnBi-based solder coating, and a SnPb-based solder coating.

[0020] Preferably, the thickness of the tin-containing coating formed on the surface of the solder column in step 1 is 5 to 25 microns.

[0021] Preferably, the low-temperature aging temperature range of the tin-containing coating solder column in step 2 is 50° C. to 120° C.

[0022] Preferably, the thickness of the intermetallic compound layer formed at the solder column / tin-containing coating interface during the low-temperature aging of the tin-containing coating solder column in step 2 is 0.5 to 2.5 microns.

[0023] Preferably, the array-arranged pads described in step 3 are array-arranged pads on a chip carrier substrate or array-arranged pads on a printed circuit board; the method for improving the quality of moldless column planting connection of CGA devices is applicable to the column planting on the pads arranged in an array on a chip carrier substrate in the first-level packaging; it is also applicable to the column planting on the pads arranged in an array on a chip carrier substrate or array-arranged pads on a printed circuit board in the second-level packaging.

[0024] Preferably, the solder type in the solder paste described in step 3 is any one of SnCu series, SnAg series, SnAgCu series, and SnSb series soft solder.

[0025] Preferably, the height h of the array spherical crown solder balls described in step 4 is greater than or equal to 4 / 5 of the diameter D of the pad.

[0026] Preferably, the solder paste heating temperature in step 4 is 20° C. to 55° C. higher than the melting point of the solder in the solder paste.

[0027] Preferably, the tin-coated solder column described in step 5 is clamped in the chuck of the micro-precision drill instead of the drill bit, and the length of the tin-coated solder column exposed from the clamping chuck ranges from 1.2 to 2.0 times the height h of the solder ball, and this parameter remains consistent during the stud implantation process of each array of tin-coated solder columns to ensure that the tin-coated solder column has sufficient stiffness and is not bent.

[0028] Preferably, the rotational speed range of the tin-coated solder column driven by the chuck of the micro-precision drill described in step 5 is 2500 revolutions per minute to 8000 revolutions per minute.

[0029] Preferably, the end of the tin-coated solder column described in step 5 is pressed down and drilled into the spherical cap-shaped solder ball to a predetermined depth S, where 1 / 2h < S < h - 0.1 mm, and h is the height of the array of spherical cap-shaped solder balls.

[0030] Preferably, the process of the end of the tin-coated solder column drilling into the spherical cap-shaped solder ball includes processes such as frictional heat generation at the tin-coated / spherical cap-shaped solder ball interface, plastic deformation and generation of dislocations in the solder and tin coating near the interface, and dynamic recrystallization of the solder and tin coating in the large strain zone near the interface, which causes the original interface and defects to disappear and finally forms a reliable connection.

[0031] The present invention has the following beneficial effects:

[0032] First, the tin coating on the surface of the solder column of the present invention and the low-temperature aging treatment form an intermetallic compound layer with continuous and appropriate thickness in the heterogeneous material transition zone between the solder column and the spherical cap-shaped solder ball. And during the subsequent stud implantation process, due to the existence of the peripheral tin coating, the intermetallic compound layer will not be polished off. Therefore, there is no problem of "the scallop-shaped intermetallic compound formed by atomic interdiffusion at the copper column / solder ball interface of the existing CGA device array is continuously polished off, the remaining interface connection layer after welding is too thin and discontinuous, and the connection strength is limited, thus affecting the stud implantation quality" in the copper column implantation connection without die assistance.

[0033] Second, there is a certain thickness of tin coating on the surface of the solder column of the present invention. The stud implantation connection interface changes from a heterogeneous interface of the solder column / spherical cap-shaped solder ball to a homogeneous interface between the tin coating / spherical cap-shaped solder ball. During the stud implantation process, there is mutual contact, frictional heat adhesion, atomic interdiffusion and dynamic recrystallization between the tin coating and the tin-based solder, and a reliable connection is formed. The present invention changes the connection of heterogeneous interfaces with greatly different material properties to the connection of homogeneous interfaces with similar or identical material properties, and the connectivity of the heterogeneous interface structure of the solder column / spherical cap-shaped solder ball is significantly improved.

[0034] Third, there is a tin-containing coating of a certain thickness on the surface of the solder column of the present invention, and the interface connection layer of the column is transformed into recrystallized grains of solder and the tin-containing coating. There is no problem of the existing CGA device array copper column without mold-assisted column connection that "the interface connection layer is an intermetallic compound layer, and the interface connection layer remaining after welding is too thin and discontinuous, and the connection strength is limited, which affects the quality of the column."

[0035] Fourth, there is a tin-containing coating of a certain thickness on the surface of the solder column of the present invention, and the column connection interface is transformed from a heterogeneous interface of the solder column / spherical crown solder ball to a homogeneous interface between the tin-containing coating / spherical crown solder ball. The differences in thermal physical and mechanical properties between the tin-containing coating and the tin-based solder are extremely small. The difference in thermal physical states between the tin coating and the tin-based solder during the connection process is extremely small, and the friction adhesion between the two is extremely good. The existing CGA device array copper column connection without mold-assisted column planting does not have the problems of "the disparity in performance between the solder column and the spherical crown solder ball, the disparity in thermal physical states during column planting, and weak adhesion leading to limited connection strength, which in turn affects the quality of column planting".

[0036] Fifth, there is a tin-containing coating of a certain thickness on the surface of the solder column of the present invention. During the column planting, the soft tin-containing coating acts as a stress buffer layer to a certain extent, and the vibration degree of the solder column is significantly reduced, thereby reducing the problems of the existing CGA device array copper column without mold-assisted column planting connection: "the copper column is prone to vibration during column planting, the near-interface solder of the solder ball is easy to soften, and the elastic clamping force between the copper column / solder solder ball is low, resulting in limited connection strength, which in turn affects the column planting quality."

[0037] Sixth, the method of improving the connection quality of mold-free pillar planting of CGA devices of the present invention can save the expensive precision mold manufacturing cost compared with the traditional method of mold positioning copper pillars and reflow soldering connection used in the field of microelectronic packaging technology; compared with the existing CGA device array copper pillar mold-free assisted pillar planting connection method, the pillar planting connection strength can be increased by 35%, and the connection quality is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of a single tin-containing coating solder pillar after implantation in the first specific implementation mode;

[0039] Figure 2 It is a schematic diagram of a single tin-containing coating solder column after implantation in the second specific implementation mode;

[0040] Figure 3 It is a schematic longitudinal section of a single interconnect structure formed after the tin-coated copper column is implanted and the other end of the tin-coated copper column is subsequently reflowed at low temperature in Example 1;

[0041] Figure 4It is a schematic longitudinal section of a single interconnect structure formed after the tin-coated iron-nickel alloy column is implanted and the other end of the tin-coated iron-nickel alloy column is subsequently reflowed at low temperature in Example 2. DETAILED DESCRIPTION Specific implementation method one:

[0043] A method for improving the quality of mold-free column connection of CGA devices comprises the following steps:

[0044] Step 1: Preparation of tin-containing coating on the surface of solder column:

[0045] Use hot-dip tinning or electroplating to form a tin-containing coating on the surface of a standard-sized solder column, followed by necessary cleaning processes to prevent residual substances on the surface of the tin-containing coating that affect subsequent connections; the thickness of the tin-containing coating must be no less than 5 microns and no more than 25 microns; the tin-containing coating must be uniform in thickness, have a bright surface, and be free of balling or non-wetting;

[0046] Step 2: performing low-temperature aging treatment on the solder column containing the tin coating, controlling the aging temperature and aging time, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the solder column / tin-containing coating;

[0047] Step 3, printing an appropriate amount of solder paste on the pads arranged in the printed circuit board array;

[0048] Similar to the traditional BGA ball placement process, a proper amount of solder paste is printed on the pads arranged in array on the printed circuit board with the help of a mature template printing process, and the amount of solder paste printed on the pads arranged in array is required to be consistent;

[0049] Step 4: Heat the solder paste to form an array of spherical crown-shaped solder balls with consistent height:

[0050] The solder paste is heated to activate the flux therein and remove the oxide film, so that the solder therein is melted and wets the array-arranged pads, thereby forming array spherical crown-shaped solder balls with consistent height on the array-arranged pads of the printed circuit board;

[0051] Step 5: Planting of a single tin-coated solder column:

[0052] The tin-coated solder column is clamped in the chuck of a micro-precision drilling machine. The printed circuit board where the pad of the column to be planted is located is controlled by a program to move so that the tin-coated solder column is located above the pad of the column to be planted and aligned with the center of the pad. The chuck of the micro-precision drilling machine is used to drive the tin-coated solder column to rotate, and the end of the tin-coated solder column is slowly pressed down at a uniform speed to drill into the spherical crown solder ball to a predetermined depth S. After that, the feeding movement and rotation of the tin-containing coating solder column are stopped, and then the tin-containing coating solder column remains stationary until the spherical crown solder ball cools to room temperature; the drill press chuck is opened and lifted, so that the tin-containing coating solder column remains in the spherical crown solder ball on the pad, and the column planting connection of a single tin-containing coating solder column on the printed circuit board pad is completed; due to the process of the tin-containing coating solder column rotating, pressing down and drilling into the spherical crown solder ball to a predetermined depth and the subsequent cooling to room temperature, the homogeneous interface temperature between the tin-containing coating / spherical crown solder ball increases, and the tin-containing coating and the tin-based solder are mutually contacted, plastically deformed, heat-generated adhesion by friction, atomic mutual diffusion, dynamic recrystallization, and the spherical crown solder ball expands due to temperature increase and contracts due to temperature decrease to hold the tin-containing coating solder column, and finally a reliable connection is formed; the column planting connection of the tin-containing coating solder column is the result of the combined action of the plastic deformation connection mechanism, the diffusion connection mechanism, the recrystallization connection mechanism and the mechanical expansion connection mechanism;

[0053] The schematic diagram of a single tin-coated solder column after implantation is as follows Figure 1 As shown, A is a cylindrical solder column; B is the tin-containing coating on the periphery of the cylindrical solder column; C is the intermetallic compound layer generated between the solder column and the tin-containing coating; D is a spherical crown solder ball formed after solder paste reflow; E is a printed circuit board; F is a metal film pad on the printed circuit board; and G is a solder mask.

[0054] Step 6: Planting of tin-coated solder columns of the array:

[0055] Repeat the process of step 5 above with the same size parameters and process parameters to implement the process of implanting the tin-coated solder columns on each pad arranged in an array on the printed circuit board one by one, and ensure that the exposed ends of the tin-coated solder columns in the array are coplanar after implantation.

[0056] The present invention can be used to achieve high-quality column planting of array solder columns of high-frequency, high-power, high-I / O, large-chip CGA devices with high reliability requirements in the fields of aerospace, communications, military industry, automotive electronics, etc. Specific implementation method 2:

[0058] A method for improving the quality of mold-free column connection of CGA devices comprises the following steps:

[0059] Step 1: Preparation of tin-containing coating on the surface of solder column:

[0060] Use hot-dip tinning or electroplating to form a tin-containing coating on the surface of a standard-sized solder column, followed by necessary cleaning processes to prevent residual substances on the surface of the tin-containing coating that may affect subsequent connections; the thickness of the tin-containing coating must be no less than 5 microns and no more than 25 microns; the tin-containing coating must be uniform in thickness, have a bright surface, and be free of balling or non-wetting;

[0061] Step 2: performing low-temperature aging treatment on the solder column containing the tin coating, controlling the aging temperature and aging time, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the solder column / tin-containing coating;

[0062] Step 3, printing an appropriate amount of solder paste on the pads arranged in the chip carrier substrate array;

[0063] Similar to the traditional solder bumping process, a proper amount of solder paste is printed on the pads arranged in array on the chip carrier substrate using a mature template printing process, and the amount of solder paste printed on the pads arranged in array is required to be consistent;

[0064] Step 4: Heat the solder paste to form an array of spherical crown solder balls with consistent height:

[0065] The solder paste is heated to activate the flux therein and remove the oxide film, so that the solder therein is melted and wets the pads arranged in an array, and an array of spherical crown-shaped solder balls having a consistent height are formed on the pads arranged in an array on the chip carrier substrate;

[0066] Step 5: Planting of a single tin-coated solder column:

[0067] The tin-containing coating solder column is clamped in the chuck of a micro-precision drilling machine, and the movement of the chip carrier substrate where the column pad to be planted is located is controlled by a program so that the tin-containing coating solder column is located above the column pad to be planted and aligned with the center of the pad. The chuck of the micro-precision drilling machine is used to drive the tin-containing coating solder column to rotate, and the end of the tin-containing coating solder column is slowly pressed down at a uniform speed to drill into the spherical crown-shaped solder ball to a predetermined depth S, and then the feeding movement and rotation of the tin-containing coating solder column are stopped, and then the tin-containing coating solder column remains stationary until the spherical crown-shaped solder ball cools to room temperature; the chuck of the drilling machine is opened and lifted, so that the tin-containing coating solder column remains in the spherical crown-shaped solder ball on the pad, and the column connection of a single tin-containing coating solder column on the chip carrier substrate is completed; Due to the process of the tin-containing coating solder column rotating, pressing down and drilling into the spherical crown solder ball to a predetermined depth and the subsequent cooling to room temperature, the homogeneous interface temperature between the tin-containing coating and the spherical crown solder ball increases, and the tin-containing coating and the tin-based solder are in contact with each other, plastic deformation, friction heat adhesion, atomic mutual diffusion, dynamic recrystallization, and the spherical crown solder ball expands due to temperature increase and contracts due to temperature decrease, which causes the tin-containing coating solder column to hold tightly, and finally a reliable connection is formed; the tin-containing coating solder column is connected by the combined action of the plastic deformation connection mechanism, the diffusion connection mechanism, the recrystallization connection mechanism and the mechanical expansion connection mechanism.

[0068] The schematic diagram of a single tin-coated solder column after implantation is as follows Figure 2 As shown, A is a cylindrical solder column; B is a tin-containing coating on the periphery of the cylindrical solder column; C is an intermetallic compound layer generated between the solder column and the tin-containing coating; D is a spherical crown solder ball formed after solder paste reflow; E1 is a chip carrier substrate; F is a metal film pad on the chip carrier substrate; and G is a solder resist film.

[0069] Step 6: Planting of tin-coated solder columns of the array:

[0070] Repeat the process of step 5 above with the same size parameters and process parameters, and implement the process of implanting the tin-coated solder pillars on each pad arranged in an array on the chip carrier substrate one by one, and ensure that the exposed ends of the tin-coated solder pillars in the array are coplanar after implantation.

[0071] The present invention can be used to achieve high-quality column planting of array solder columns of high-frequency, high-power, high-I / O, large-chip CGA devices with high reliability requirements in the fields of aerospace, communications, military industry, automotive electronics, etc. Specific implementation method three:

[0073] The solder column described in step 1 of this embodiment is any one of a copper column, a brass column, an iron-nickel alloy column, and an iron-nickel-cobalt alloy column of uniform specifications and sizes prepared according to standards; the aspect ratio of the solder column described in step 1 of this embodiment is in the range of 6 to 20, and the diameter d of the solder column is not less than 1 / 5 of the pad diameter D and not more than 1 / 3 of the pad diameter D.

[0074] The other steps and parameters are the same as those in the first or second embodiment. Specific implementation method four:

[0076] The tin-containing coating described in step 1 of this embodiment is any one of a pure tin coating, a SnCu-based solder coating, a SnAg-based solder coating, a SnAgCu-based solder coating, a SnSb-based solder coating, a SnBi-based solder coating, and a SnPb-based solder coating.

[0077] The other steps and parameters are the same as those in the first to third embodiments. Specific implementation method five:

[0079] The thickness of the tin-containing coating formed on the surface of the solder column in step 1 of this embodiment is 5 to 25 microns.

[0080] The other steps and parameters are the same as those in Specific Embodiments 1 to 4. Specific implementation method six:

[0082] The low-temperature aging temperature range of the tin-containing coated solder column described in step 2 of this embodiment is 50°C to 120°C; the thickness of the intermetallic compound layer formed at the solder column / tin-containing coating interface during the low-temperature aging of the tin-containing coated solder column described in step 2 of this embodiment is 0.5 to 2.5 microns.

[0083] The other steps and parameters are the same as those in the first to fifth embodiments. Specific implementation method seven:

[0085] The type of solder in the solder paste described in step 3 of this embodiment is any one of SnCu-based, SnAg-based, SnAgCu-based, and SnSb-based soft solders.

[0086] The other steps and parameters are the same as those in the first to sixth embodiments. Specific implementation eight:

[0088] The solder paste heating temperature described in step 4 of this embodiment mode is 20°C to 55°C higher than the melting point of the solder in the solder paste; the height h of the array spherical crown solder balls described in step 4 of this embodiment mode is greater than or equal to 4 / 5 of the pad diameter D.

[0089] The other steps and parameters are the same as those in the first to seventh embodiments. Specific implementation method nine:

[0091] In step 5 of this embodiment, the tin-coated solder column is used to replace the drill bit and is clamped in the chuck of the micro-precision drill. The length of the tin-coated solder column exposed from the clamping chuck ranges from 1.2 to 2.0 times the height h of the solder ball, and this parameter remains consistent during the stud implantation process of each array of tin-coated solder columns to ensure that the tin-coated solder column has sufficient stiffness and is not bent. In step 5 of this embodiment, the end of the tin-coated solder column is pressed down and drilled into the spherical cap-shaped solder ball to a predetermined depth S, where 1 / 2h < S < h - 0.1 mm, and h is the height of the array of spherical cap-shaped solder balls.

[0092] Other steps and parameters are the same as those in any one of the first to eighth specific embodiments. Specific embodiment ten:

[0094] In step 5 of this embodiment, the rotational speed range of the tin-coated solder column driven by the chuck of the micro-precision drill is 2500 revolutions per minute to 8000 revolutions per minute.

[0095] Other steps and parameters are the same as those in any one of the first to ninth specific embodiments.

[0096] Example

[0097] Example 1:

[0098] The single tin-coated solder column interconnection structure in the CGA device array solder column interconnection structure can be referred to Figure 3 . Among them, 1 is a cylindrical copper column; 2 is the tin coating around the copper column; 3 is the intermetallic compound layer formed between the copper column and the tin coating; 4 is the spherical cap-shaped solder ball at the stud implantation end; 5 is the solder fillet formed after low-temperature reflow soldering at the other end of the tin-coated copper column after stud implantation; for the stud implantation situation of the array solder columns in the second-level packaging, 6 is the chip carrier substrate, 7 is the printed circuit board, 8 is the metal film solder pad on the chip carrier substrate / printed circuit board, and 9 is the solder mask on the chip carrier substrate / printed circuit board.

[0099] Taking the stud implantation situation of the array solder columns in the second-level packaging as an example, the process of the CGA device array solder column interconnection structure mainly includes the stud implantation process of the array solder columns on the array-arranged solder pads of the printed circuit board in the early stage and the reflow soldering process of the other ends of the implanted array solder columns with the array-arranged solder pads and the solder paste on the chip carrier substrate in the later stage.

[0100] For the early stud implantation process, the method for improving the quality of die-less stud implantation connection of CGA devices according to the present invention includes the following steps:

[0101] Step 1. Fabrication of the tin coating on the surface of the solder column:

[0102] According to the design standard, a cylindrical copper column of uniform specifications and sizes matching the diameter D of the pad of the printed circuit board is prepared, the diameter of the copper column is d (D / 5≤d≤D / 3), the height of the copper column is l, and the aspect ratio is 9; after ultrasonic cleaning in an alcohol solution, a tin-containing coating is formed on the surface of the copper column of standard size by hot-dip tinning or electroplating, and then ultrasonic cleaning is performed to avoid residual substances on the surface of the tin-containing coating that affect subsequent connections; the thickness of the prepared tin-containing coating is not less than 5 microns and not more than 25 microns, and the tin-containing coating is required to be uniform in thickness, bright on the surface, and free of balling or non-wetting;

[0103] Step 2: performing low-temperature aging treatment on the tin-containing coating copper column, controlling the aging temperature and aging time, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the solder column / tin-containing coating;

[0104] Step 3: Print an appropriate amount of solder paste on the pads arranged in array on the printed circuit board; Same as the traditional BGA ball planting process, use a mature template printing process to print an equal and sufficient amount of Sn3.0Ag0.5Cu lead-free solder paste on the pads arranged in array on the printed circuit board, and the amount of solder paste printed should make the height h of the solder ball after reflow soldering not less than 4 / 5 times the pad diameter D;

[0105] Step 4: Heat the solder paste to form an array of spherical crown-shaped solder balls with consistent height:

[0106] The solder paste is heated according to the reflow heating curve of the Sn3.0Ag0.5Cu lead-free solder paste, wherein the reflow peak temperature is controlled within the range of 35°C±5°C above the melting point of the solder, firstly the solder therein is activated and the oxide film is removed, and then the solder therein is melted and wetted the array-arranged pads, so as to form array spherical crown-shaped solder balls with a consistent height on the array-arranged pads of the printed circuit board;

[0107] Step 5: Planting of a single tin-coated solder column:

[0108] The tin-coated copper column is clamped in the chuck of the micro-precision drilling machine. The length of the tin-coated copper column exposed from the clamping head is 1.5 times the height h of the solder ball, and this parameter is kept consistent for each tin-coated copper column during the column planting process. The program controls the movement of the printed circuit board where the column pad to be planted is located, so that the tin-coated copper column is located above the column pad to be planted and aligned with the center of the pad. The micro-precision drilling machine chuck drives the tin-coated copper column to rotate at a speed of 5000 rpm, while the end of the tin-coated copper column is slowly pressed down at a uniform speed to drill into the spherical crown solder ball to a predetermined depth. After that, the feeding movement and rotation of the tin-coated copper column are stopped, and then the tin-coated copper column remains stationary until the spherical crown solder ball cools to room temperature; the drill press chuck is opened and lifted, so that the tin-coated copper column remains in the spherical crown solder ball on the pad, and the column planting connection of a single tin-coated copper column on a single pad of the printed circuit board is completed; due to the process of the tin-coated copper column rotating, pressing down and drilling into the spherical crown solder ball to a predetermined depth and the subsequent cooling to room temperature, the homogeneous interface temperature between the tin-coated coating / spherical crown solder ball increases, and the tin-coated coating and the tin-based solder are mutually contacted, plastically deformed, frictionally heat-generated adhesion, atomic mutual diffusion, dynamic recrystallization, and the spherical crown solder ball expands due to temperature increase and contracts due to temperature decrease to hold the tin-coated copper column, and finally a reliable connection is formed; the column planting connection of the tin-coated copper column is the result of the combined action of the plastic deformation connection mechanism, the diffusion connection mechanism, the recrystallization connection mechanism and the mechanical expansion connection mechanism;

[0109] Step 6: Planting of tin-coated solder columns of the array:

[0110] Repeat the process of step five with the same size parameters and process parameters to implement the process of implanting the tin-coated copper pillars on each pad arranged in an array on the printed circuit board one by one, and ensure that the exposed ends of the tin-coated copper pillars in the array are coplanar after implantation.

[0111] First of all, the column is planted on the printed circuit board, and then the low-temperature reflow soldering process is completed between the other end of the planted array tin-coated copper column and the array arrangement pad on the chip carrier substrate (the melting point of the solder paste used should be at least 40°C lower than the melting point of the spherical crown solder ball at the planting column end, and the peak temperature is controlled within the range of 25°C±5°C above the melting point of the low-melting solder paste). During this period, the aforementioned column planting part is also in the same low-temperature reflow soldering heating environment, and the mutual diffusion of atoms at the interface of the tin-coated copper column / spherical crown solder ball in the high-temperature solid phase state can further promote the strength of the column connection, thereby realizing the interconnection of the two ends of the array tin-coated copper column, which has no mechanical impact on the chip and the chip carrier substrate, and has a protective effect on the chip. It is also possible to first plant the column on the chip carrier substrate using the steps described in this embodiment, and then complete the low-temperature reflow soldering process between the other end of the planted array tin-coated copper column and the array arrangement pad on the printed circuit board.

[0112] Embodiment 2:

[0113] In addition to being used for connecting the secondary package chip carrier substrate and the printed circuit board, the CGA device array solder column interconnection structure can also be used for connecting the primary package chip and the chip carrier substrate. Figure 4, wherein 1 is a cylindrical iron-nickel alloy column; 2 is a tin-containing coating on the periphery of the iron-nickel alloy column; 3 is an intermetallic compound layer formed between the iron-nickel alloy column and the tin-containing coating; 41 is a spherical crown solder ball at the end of the column; 51 is a solder fillet formed after low-temperature reflow soldering at the other end of the tin-containing coated iron-nickel alloy column after the column is planted; 61 is a chip; 71 is a chip carrier substrate, 81 is a metal film pad on the chip / chip carrier substrate, and 91 is a solder resist film on the chip / chip carrier substrate.

[0114] Taking the implantation of the array solder pillars in the first-level package as an example, the process of the CGA device array solder pillar interconnection structure mainly includes the early implantation process of the solder pillars on the chip carrier substrate array arrangement pads and the later reflow soldering process between the other end of the implanted array solder pillars and the chip front array arrangement pads and the solder paste thereon.

[0115] In view of the early pillar planting process, the present invention provides a method for improving the quality of mold-free pillar planting connection of CGA devices, comprising the following steps:

[0116] Step 1: Preparation of tin coating on the surface of solder column:

[0117] According to the design standard, a cylindrical iron-nickel alloy column of uniform specifications and sizes matching the diameter D1 of the chip carrier substrate pad is prepared, the diameter of the iron-nickel alloy column is d1 (D1 / 5≤d1≤D1 / 3), the height of the iron-nickel alloy column is l1, and the aspect ratio is 16; after ultrasonic cleaning in an alcohol solution, a tin-containing coating is formed on the surface of the standard-sized iron-nickel alloy column by hot-dip tinning or electroplating, and then ultrasonic cleaning is performed to avoid residual substances on the surface of the tin-containing coating that affect subsequent connections; the thickness of the prepared tin-containing coating is not less than 5 microns and not more than 25 microns, and the tin-containing coating is required to be uniform in thickness, bright on the surface, and free of balling or non-wetting;

[0118] Step 2: performing low-temperature aging treatment on the tin-containing coating iron-nickel alloy column, controlling the aging temperature and aging time, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the solder column / tin-containing coating;

[0119] Step 3: Print an appropriate amount of solder paste on the pads arranged in array on the chip carrier substrate; Same as the conventional solder bumping process, print an equal and sufficient amount of Sn5.0Sb lead-free solder paste on the pads arranged in array on the chip carrier substrate with the help of a mature template printing process, and the amount of solder paste printed should make the solder ball height h after reflow soldering not less than 4 / 5 times the pad diameter D1;

[0120] Step 4: Heat the solder paste to form an array of spherical crown-shaped solder balls with consistent height:

[0121] The solder paste is heated according to the reflow heating curve of the Sn5.0Sb lead-free solder paste, wherein the reflow peak temperature is controlled within the range of 30°C±5°C above the melting point of the solder, firstly the solder therein is activated and the oxide film is removed, then the solder therein is melted and wets the pads arranged in an array, and an array of spherical crown-shaped solder balls with a consistent height are formed on the pads arranged in an array on the chip carrier substrate;

[0122] Step 5: Planting of a single tin-coated solder column:

[0123] The tin-coated iron-nickel alloy column is clamped in the chuck of the micro-precision drilling machine. The length of the tin-coated iron-nickel alloy column exposed from the clamping head is 1.8 times the height h of the solder ball, and this parameter is kept consistent for each tin-coated iron-nickel alloy column during the column planting process. The movement of the chip carrier substrate where the column pad to be planted is located is controlled by a program, so that the tin-coated iron-nickel alloy column is located above the column pad to be planted and aligned with the center of the pad. The tin-coated iron-nickel alloy column is driven by the chuck of the micro-precision drilling machine to rotate at a speed of 6500 rpm, while the end of the column is slowly pressed down at a uniform speed to drill into the spherical crown solder ball to a predetermined depth. After that, the feeding movement and rotation of the tin-coated iron-nickel alloy column are stopped, and then the tin-coated iron-nickel alloy column remains stationary until the spherical crown-shaped solder solder ball cools to room temperature; the drill press chuck is opened and lifted, so that the tin-coated iron-nickel alloy column remains in the spherical crown-shaped solder solder ball on the pad, and the column planting connection of a single tin-coated iron-nickel alloy column on a single pad of the chip carrier substrate is completed; due to the process of the tin-coated iron-nickel alloy column rotating, pressing down and drilling into the spherical crown-shaped solder solder ball to a predetermined depth and the subsequent cooling to room temperature, the tin-coated iron-nickel alloy column is The temperature of the homogeneous interface between the spherical crown solder balls increases, and during the column planting process, the tin-containing coating and the tin-based solder are in contact with each other, plastic deformation, friction heat adhesion, atomic mutual diffusion, dynamic recrystallization, and the spherical crown solder balls expand when the temperature increases and contract when the temperature decreases, which causes a clamping effect on the tin-containing coating iron-nickel alloy column and finally forms a reliable connection; the column planting connection of the tin-containing coating iron-nickel alloy column is the result of the combined action of the plastic deformation connection mechanism, the diffusion connection mechanism, the recrystallization connection mechanism and the mechanical expansion connection mechanism;

[0124] Step 6: Planting of tin-coated solder columns of the array:

[0125] Repeat the above step five process with the same size parameters and process parameters to implement the pillar planting process of the tin-coated iron-nickel alloy pillars on each pad arranged in an array on the chip carrier substrate one by one, and ensure that the exposed ends of the tin-coated iron-nickel alloy pillars in the array are coplanar after pillar planting.

[0126] First of all, the column is planted on the chip carrier substrate, and then the low-temperature reflow soldering process is completed between the other end of the planted array tin-coated iron-nickel alloy column and the chip front array arrangement pad (the melting point of the solder paste used should be at least 40°C lower than the melting point of the spherical crown solder ball at the column end, and the peak temperature is controlled within the range of 25°C±5°C above the melting point of the low-melting point solder paste). During this period, the aforementioned column planting position is also in the same low-temperature reflow soldering heating environment, and the mutual diffusion of atoms at the interface of the tin-coated iron-nickel alloy column / spherical crown solder ball in the high-temperature solid phase state can further promote the improvement of the column connection strength, thereby realizing the interconnection of the two ends of the array tin-coated iron-nickel alloy column, which has no mechanical impact on the chip and has a protective effect on the chip.

Claims

1. A method for improving the quality of mold-free column connection of CGA devices, characterized in that: The following steps are involved: Step 1: Preparation of tin-containing coating on the surface of solder column: Hot-dip tinning or electroplating is used to form a tin-containing coating on the surface of standard-sized solder pillars, followed by a cleaning process to prevent residual substances on the surface of the tin-containing coating that may affect subsequent connections; Step 2, performing low-temperature aging treatment on the tin-containing coating solder column, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the solder column / tin-containing coating, and the low-temperature aging temperature range of the tin-containing coating solder column is 50° C. to 120° C.; Step 3: Print an appropriate amount of solder paste on the pads arranged in the array; Step 4, heating the solder paste to wet the pads arranged in the array, forming an array of spherical crown-shaped solder balls with consistent height; Step 5: Planting of a single tin-coated solder column: The tin-containing coating solder column is clamped in the chuck of the micro-precision drilling machine, and the movement of the substrate where the column pad to be planted is located is controlled by a program so that the tin-containing coating solder column is located above the column pad to be planted and is aligned with the center of the pad. The chuck of the micro-precision drilling machine is used to drive the tin-containing coating solder column to rotate, and the end of the tin-containing coating solder column is slowly pressed down at a uniform speed to drill into the spherical crown-shaped solder ball to a predetermined depth S, and then the feeding movement and rotation of the tin-containing coating solder column are stopped, and then the tin-containing coating solder column remains stationary until the spherical crown-shaped solder ball cools to room temperature; Open and lift the drill press chuck, so that the tin-containing coating solder column remains in the spherical crown solder ball on the pad, completing the column planting connection of a single tin-containing coating solder column; during the column planting process, the tin-containing coating and the tin-based solder will contact each other, plastic deformation, friction heat adhesion, atomic mutual diffusion, dynamic recrystallization, and the spherical crown solder ball will expand due to temperature increase and contract due to temperature decrease, which will cause a tightening effect on the tin-containing coating solder column and finally form a reliable connection; Step 6: Planting of tin-coated solder columns of the array: Repeat the process of step 5 above with the same size parameters and process parameters to implement the process of implanting the tin-coated solder pillars on each array-arranged pad one by one, and ensure that the exposed ends of the array tin-coated solder pillars are coplanar after implantation.

2. A method for improving the quality of mold-free column connection of CGA devices according to claim 1, characterized in that: The solder column described in step 1 is any one of a copper column, a brass column, an iron-nickel alloy column, and an iron-nickel-cobalt alloy column of uniform specifications and sizes prepared according to standards, and the aspect ratio of the solder column is in the range of 6 to 20, and the diameter d of the solder column is not less than 1 / 5 of the pad diameter D and not more than 1 / 3 of the pad diameter D.

3. A method for improving the quality of mold-free column connection of CGA devices according to claim 2, characterized in that: The tin-containing coating described in step 1 is any one of a pure tin coating, a SnCu-based solder coating, a SnAg-based solder coating, a SnAgCu-based solder coating, a SnSb-based solder coating, a SnBi-based solder coating, and a SnPb-based solder coating.

4. A method for improving the quality of mold-free column connection of CGA devices according to claim 3, characterized in that: The thickness of the tin-containing coating formed on the surface of the solder column in step 1 is 5 to 25 microns.

5. A method for improving the quality of mold-free column connection of CGA devices according to claim 4, characterized in that: The thickness of the intermetallic compound layer formed at the solder column / tin-containing coating interface during the low-temperature aging of the tin-containing coating solder column in step 2 is 0.5 to 2.5 microns.

6. A method for improving the quality of mold-free column connection of CGA devices according to claim 5, characterized in that: The solder type in the solder paste described in step 3 is any one of SnCu series, SnAg series, SnAgCu series, and SnSb series soft solder.

7. A method for improving the quality of mold-free column connection of CGA devices according to claim 6, characterized in that: The rotation speed range of the tin-containing coating solder column driven by the micro-precision drilling machine chuck in step 5 is 2500 rpm to 8000 rpm.

8. A method for improving the quality of mold-free column connection of CGA devices according to claim 7, characterized in that: The tin-coated solder column described in step 5 is clamped in the chuck of the micro-precision drill instead of the drill bit. The length range of the tin-coated solder column exposed from the clamping chuck is 1.2 to 2.0 times the height h of the solder ball. And the predetermined depth S of pressing down and drilling into the solder ball described in step 5 satisfies 0.5h < S < h - 0.1 mm, where h is the height of the solder ball.