Graft copolymers and their preparation methods

By adjusting the water content percentage in the extruder, graft copolymer pellets with high volume density are formed, which solves the problem of easy aggregation in the dry powder form and achieves good storage properties and maintenance of physical properties of the graft copolymer.

CN113939549BActive Publication Date: 2024-10-01LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080042549.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-25
Filing Date
2020-11-23
Publication Date
2024-10-01
Estimated Expiration
2040-11-23

AI Technical Summary

Technical Problem

Graft copolymers in dry powder form are prone to particle aggregation and agglomeration during storage, resulting in quality changes and difficulty in use.

Method used

The graft copolymer is prepared by emulsion polymerization, and the water content percentage is adjusted in the extruder to form a pellet form with a volume density of 450kg/m3 to 700kg/m3 to avoid particle aggregation and agglomeration.

Benefits of technology

It achieves good storage and quality stability of the graft copolymer, reduces the aggregation phenomenon between particles, maintains the physical properties and whiteness index, and is suitable for thermoplastic resin compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113939549B_ABST
    Figure CN113939549B_ABST
Patent Text Reader

Abstract

The invention relates to a graft copolymer and a preparation method thereof, wherein the graft copolymer has the advantages of superior storage convenience and high whiteness index compared with existing dry powders, and can therefore be widely used in various fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2019-0152004 filed in the Korean Intellectual Property Office on November 25, 2019, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0004] The present invention relates to a graft copolymer having smaller inter-particle aggregation than a dry powder type graft copolymer and thus having the advantages of being easy to transport and having less temporal variation in product quality during long-term storage. Background Art

[0005] Graft copolymers, for example, ABS-based copolymers such as acrylonitrile-butadiene-styrene, or ASA-based copolymers such as acrylate-styrene-acrylonitrile, have relatively satisfactory physical properties such as moldability and glossiness as well as stiffness, chemical resistance and shock resistance, and are therefore widely used as housings or interior / exterior materials for various products such as electrical parts, electronic parts, office equipment, or automotive parts.

[0006] Generally, in order to improve shock resistance, styrene and acrylonitrile are graft copolymerized onto a rubber latex such as polybutadiene or poly(butyl acrylate) by an emulsion polymerization method, and then the product is kneaded with a SAN-based resin such as a styrene-acrylonitrile copolymer or a thermoplastic resin such as polystyrene or polymethyl methacrylate to prepare the graft copolymer as a resin composition. In this preparation process, the graft copolymer is usually prepared in the form of a dry powder (DP) before kneading with the thermoplastic resin, and the graft copolymer in the form of a dry powder can be kneaded with the thermoplastic resin immediately after preparation, but can also be kneaded with the thermoplastic resin by a separate kneading process after a predetermined time has passed from the time of preparation. Therefore, the easy storage of the graft copolymer itself and the time change characteristics of the quality of the graft copolymer stored for a long time are the main factors that should be considered when preparing the graft copolymer.

[0007] Meanwhile, the graft copolymer in the form of dry powder has the advantage of easy preparation process, but when not kneaded immediately with the thermoplastic resin, the graft copolymer in the form of dry powder may cause agglomeration phenomenon in which powder particles aggregate with each other during long-term storage and are not easily separated from each other. Therefore, for the prepared graft copolymer, it is necessary to study how to improve easy storage and minimize time variation of quality.

[0008] [Prior art documents]

[0009] [Patent document]

[0010] (Patent Document 1) KR 10-2019-0059037A Summary of the invention

[0011] Technical issues

[0012] One aspect of the present invention provides a graft copolymer whose temporal quality change is minimized even in long-term storage and whose inter-particle aggregation is small during storage.

[0013] Technical Solution

[0014] According to one aspect of the present invention, a graft copolymer is provided, which comprises: one or more units from conjugated diene monomers and units from acrylate monomers; and one or more units from vinyl cyanide monomers and units from aromatic vinyl monomers, and the volume density of the graft copolymer is 450 kg / m 3 Up to 700kg / m 3 .

[0015] According to another aspect of the present invention, a pellet formed from a graft copolymer is provided.

[0016] According to another aspect of the present invention, a method for preparing a copolymer is provided, the method comprising: (S1) polymerizing a conjugated diene polymer or an acrylate polymer with one or more of a vinyl cyan monomer and an aromatic vinyl monomer to obtain a reaction product comprising a graft copolymer; and (S2) forming the reaction product in pellet form by an extruder.

[0017] Beneficial Effects

[0018] The graft copolymer provided by the present invention has excellent easy storage, small inter-particle aggregation even in long-term storage, minimized quality time change, and low amount of residual monomers, so the graft copolymer can be later applied to thermoplastic resin compositions, etc., and the physical properties of the product can be excellently maintained. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 An extruder equipped with a venting component that can be used in preparing the graft copolymer of the present invention is shown;

[0020] Figure 2 An extruder equipped with side slots which can be used in preparing the graft copolymer of the present invention is shown;

[0021] Figure 3 The results of the caking occurrence test of the pellets prepared in the examples of the present invention and the dry powders prepared in the comparative examples are arranged and shown. DETAILED DESCRIPTION

[0022] Hereinafter, the present invention will be described in more detail.

[0023] It should be understood that the words or terms used in this specification and claims should not be interpreted as the meanings defined in commonly used dictionaries. It should also be understood that the words or terms are interpreted as having the same meanings as they are in the relevant technical background and the technical concept of the present invention, based on the inventors' ability to appropriately define the meanings of the words or terms in order to best illustrate the principles of the present invention.

[0024] Graft copolymer

[0025] Acrylonitrile-butadiene-styrene copolymers or graft copolymers such as acrylate-styrene-acrylonitrile, which are widely used in various industrial fields, are prepared by mixing vinyl cyanide monomers and aromatic vinyl monomers constituting the shell with a rubber polymer as the core of the particle, and then performing graft polymerization.

[0026] Although the polymerization reaction in this preparation process can be performed by various methods such as emulsion polymerization, solution polymerization or bulk polymerization, emulsion polymerization is preferred in terms of achieving uniform reaction, easy adjustment of molecular weight and high polymerization speed.

[0027] Meanwhile, when the graft copolymer is prepared by the emulsion polymerization method, the reaction product obtained by completing the reaction contains, in addition to the graft copolymer finally polymerized, a dispersion medium such as water, an emulsifier, a surfactant, etc. which should be added for the emulsion polymerization, and the graft copolymer exists in the form of being dispersed in the reaction product. Therefore, in order to use the completely polymerized graft copolymer as a product later, it is necessary to remove the dispersion medium and impurities and agglomerate the dispersed graft copolymer, and therefore, after polymerization, agglomeration, dispersion medium removal (dehydration) and drying processes are performed in the graft copolymer preparation process.

[0028] When this process of aggregation, dispersion medium removal and drying is performed, most of the dispersion medium is removed and the graft copolymer is dried in an aggregated state, thereby preparing the final product in the form of a dry powder. The graft copolymer in the form of a dry powder can be directly made into a product later as needed, or mixed with another thermoplastic resin and used as a thermoplastic resin composition.

[0029] However, when the graft copolymer has the form of the above-mentioned dry powder, the phenomenon of aggregation between powder particles may occur during storage or transportation before later use. In particular, when a large amount of dry powder is stored or transported, the powder located at the lower part may form a cake-like mass due to the pressure of the powder located at the upper part, and this agglomeration phenomenon not only causes difficulty in using the dry powder later, but also reduces the quality of the dry powder particles.

[0030] In order to solve these problems, the inventors of the present invention did not completely dehydrate the reaction product prepared by the existing emulsion polymerization method, but adjusted the percentage of water content within a specific range, and then prepared the reaction product in the form of pellets by an extruder, thereby inventing a graft copolymer that can solve the conventional problems caused by the form of dry powder.

[0031] Specifically, the present invention provides a bulk density of 450 kg / m 3 Up to 700kg / m 3 For example, the volume density of the graft copolymer provided by the present invention is not less than 450 kg / m 3 , 500kg / m 3 、530kg / m 3 or 550kg / m 3 And not more than 700kg / m 3 、650kg / m 3 、600kg / m 3 or 570kg / m 3 , while the bulk density of conventional graft copolymers prepared in dry powder form is less than 450 kg / m 3 Or less than 400kg / m 3 The graft copolymer of the present invention is characterized in that, since a large number of graft copolymers are physically combined with each other, the graft copolymer of the present invention exhibits a larger bulk density than the graft copolymer in the form of dry powder.

[0032] In the present invention, the graft copolymer specifically includes one or more of a unit derived from a conjugated diene-based monomer and a unit derived from an acrylate-based monomer, and one or more of a unit derived from a vinyl cyan-based monomer and a unit derived from an aromatic vinyl-based monomer.

[0033] More specifically, the graft copolymer may include units derived from conjugated diene monomers, units derived from vinyl cyan monomers, and units derived from aromatic vinyl monomers, or may include units derived from acrylate monomers, units derived from vinyl cyan monomers, and units derived from aromatic vinyl monomers.

[0034] In particular, when the graft copolymer specifically contains units derived from conjugated diene monomers, units derived from vinyl cyan monomers, or units derived from aromatic vinyl monomers, the graft copolymer can be obtained by graft-polymerizing vinyl cyan monomers and aromatic vinyl monomers onto conjugated diene monomers. In addition, when the graft copolymer contains units derived from acrylate monomers, units derived from vinyl cyan monomers, or units derived from aromatic vinyl monomers, the graft copolymer can be obtained by graft-polymerizing vinyl cyan monomers and aromatic vinyl monomers onto acrylate monomers.

[0035] The conjugated diene monomers can be prepared and used by directly emulsifying and polymerizing the conjugated diene monomers, or by purchasing commercially available conjugated diene polymer products, and various forms such as latex, powder, etc. can be used as the conjugated diene polymer. Specific types of conjugated diene monomers include 1,3-butadiene, isoprene, chloroprene, piperylene, etc., among which 1,3-butadiene is more commonly used.

[0036] The acrylic acid ester monomer may be prepared and used by directly emulsifying and polymerizing the acrylic acid ester monomer, or may be used by purchasing a commercially available acrylic acid ester polymer, and various forms such as latex, powder, etc. may be used as the acrylic acid ester polymer.

[0037] Specific types of acrylate monomers include acrylate, methyl acrylate, ethyl acrylate, butyl acrylate, etc., among which butyl acrylate is more commonly used.

[0038] Specific types of aromatic vinyl monomers include styrene, α-methylstyrene, α-ethylstyrene, p-methylstyrene, etc., among which styrene is more commonly used. Specific types of vinyl cyan monomers include acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, α-chloroacrylonitrile, etc., among which acrylonitrile is more commonly used.

[0039] Meanwhile, the "unit derived from" in the present invention may refer to a repeating unit derived from a compound participating in a polymerization reaction as a monomer in a polymer or a copolymer and contained in the polymer or the copolymer.

[0040] The whiteness index (WI) of the graft copolymer according to the present invention may be 15 or more, and more preferably 20 or more. When the graft copolymer is prepared by the method for preparing the graft copolymer of the present invention to be described, the graft copolymer is immediately granulated in the state of the reaction product, and a graft copolymer having an excellent whiteness index can be prepared. On the contrary, in order to improve the poor easy storage of the existing dry powder, it can be considered to re-granulate the dry powder by an extruder and store the product, but when the dry powder that has been prepared is re-granulated, smoke is generated on the surface of the dry powder due to the heat and pressure applied during the granulation process, and therefore, the final whiteness index will be lower than the whiteness index of the graft copolymer of the present invention. When the copolymer exhibits a high whiteness index, the copolymer has the advantage of being easily applied to fields requiring various colors in the future.

[0041] The present invention provides a pellet formed by the above-mentioned graft copolymer. The pellet of the present invention can have a shape such as a sphere, a cylinder or a polygonal cylinder, and can also have an irregular shape that is difficult to specify as a specific shape. Those skilled in the art can appropriately adjust and use the shape of the pellet according to the established goals.

[0042] In the pellets of the present invention, the long diameter of the pellets may be 1 mm to 5 mm, preferably 2 mm to 4 mm, and the short diameter may be 1 mm to 5 mm, preferably 2 mm to 4 mm. The long diameter and the short diameter are defined as the lengths of the longest axis and the shortest axis passing through the center of the pellets, respectively. When the long diameter and the short diameter of the pellets meet the above ranges, the pellets have an appropriate size, are easy to prepare and store, minimize problems occurring in existing dry powders, and are appropriately used later according to the conditions required in various industrial fields.

[0043] Preparation method of graft copolymer

[0044] The present invention also provides a method for preparing the above-mentioned graft copolymer. Specifically, the preparation method may include: (S1) grafting one or more of vinyl cyanide monomers and aromatic vinyl monomers onto a conjugated diene polymer or an acrylate polymer to obtain a reaction product containing the graft copolymer; and (S2) forming the reaction product in the form of pellets through an extruder.

[0045] Step S1 is a step of preparing the graft copolymer by emulsion polymerization as described above. As is well known in the art, the emulsion polymerization in this step can be carried out in the presence of an emulsifier, a polymerization initiator, an activator, a molecular weight regulator, and the like.

[0046] For example, the emulsifier may be one or more selected from the following: sodium dicyclohexyl sulfosuccinate, sodium dihexyl sulfosuccinate, sodium di-2-ethylhexyl sulfosuccinate, potassium di-2-ethylhexyl sulfosuccinate, sodium dioctyl sulfosuccinate, sodium dodecyl sulfate, sodium dodecylbenzene sulfate, sodium octadecyl sulfate, sodium oleyl sulfate, sodium dodecyl sulfate, potassium octadecyl sulfate, potassium rosinate and sodium rosinate, among which sodium dodecylbenzene sulfate is suitable.

[0047] Based on 100 parts by weight of the monomer and polymer as the polymerization target, the emulsifier can be added in an amount of 0.1 to 2 parts by weight or 0.3 to 0.7 parts by weight, wherein it is desirable to add an emulsifier in an amount of 0.3 to 0.7 parts by weight. When the above range is met, the polymerization reaction can be stably carried out, thereby suppressing the formation of a cured product.

[0048] The type of polymerization initiator can be one or more selected from the following: sodium persulfate, potassium persulfate, ammonium persulfate, potassium perphosphate, hydrogen peroxide, tert-butyl peroxide, cumene hydroperoxide, p-menthane hydroperoxide, di-tert-butyl peroxide, tert-butyl isopropyl peroxide, acetyl peroxide, isobutyl peroxide, octanoyl peroxide, dibenzoyl peroxide, peroxide 3,5,5-trimethylhexanol, tert-butyl peroxyisobutyrate, azobisisobutyronitrile, azobis-2,4-dimethylvaleronitrile, azobiscyclohexanecarbonitrile and azobisisobutyric acid (butyric acid) methyl ester, wherein tert-butyl peroxide is desirable. Based on 100 parts by weight of the monomer and polymer used as the polymerization target, the initiator can be added in an amount of 0.01 to 1 parts by weight or 0.05 to 0.5 parts by weight, wherein it is desirable to add an initiator in an amount of 0.05 to 0.5 parts by weight. When the above range is satisfied, the polymerization reaction proceeds uniformly, and the shock resistance of the polymer can be more excellent.

[0049] The activator is selected from one or more of the following: sodium formaldehyde sulfoxylate, disodium edetate, ferrous sulfate, glucose, sodium pyrophosphate, anhydrous sodium pyrophosphate and sodium sulfate, wherein it is desirable to be selected from one or more of glucose, ferrous sulfate and sodium pyrophosphate. Based on 100 parts by weight of the monomer and polymer used as the polymerization target, the activator can be added in an amount of 0.01 to 1 part by weight or 0.1 to 0.5 parts by weight, wherein it is desirable to add the activator in an amount of 0.1 to 0.5 parts by weight. When the above range is met, the flow index, shock resistance and color characteristics of the prepared polymer can be excellent.

[0050] The molecular weight regulator may be one or more selected from the following: α-methylstyrene dimer, tert-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, carbon tetrachloride, methylene chloride, methylene bromide, tetraethylthiuram disulfide, dipentamethylenethiuram disulfide and diisopropyl xanthate disulfide, wherein tert-dodecyl mercaptan is desirable. The molecular weight regulator may be added in an amount of 0.01 to 1.5 parts by weight or 0.1 to 1 parts by weight based on 100 parts by weight of the monomer and polymer as the polymerization target, wherein 0.1 to 1 parts by weight of the molecular weight regulator is desirable. When the above range is met, the balance between the flow index, shock resistance and color characteristics of the prepared polymer may be excellent.

[0051] Furthermore, in this step, water may be used as a dispersion medium.

[0052] The reaction product containing the graft copolymer prepared by the above step S1 has the form of an emulsion in which the graft polymer is dispersed in water. Therefore, in order to selectively make only the graft copolymer in the emulsion into a product, it is necessary to remove the dispersion medium in the reaction product. The reaction product obtained by step S1 of the present invention is then added to an extruder through step S2 and the dispersion medium inside the reaction product is removed, and the reaction product is formed into a pellet form. As described above, the bulk density of the pellet can be 450kg / m 3 Up to 700kg / m 3 .

[0053] Therefore, the extruder used in the present invention should be able to maximize the removal of the residual dispersion medium in the reaction product, while suppressing the backflow of the dispersion medium removed during the extrusion process, and can form, for example, a sealing area to prevent the backflow of the dispersion medium inside the extruder. The sealing area refers to the area in which the reaction product does not move substantially and completely fills the inside of the extruder, because the amount of the reaction product added in the sealing area is the same as the amount of the reaction product going out from the sealing area, therefore, the movement of gas or liquid before and after the area can be prevented, specifically, the sealing area can be formed by various internal configurations of the extruder, for example, it can be formed by a combination of an annular structure inside the extruder, a reverse screw and a neutral screw, etc. Due to such a sealing area, the backflow of the dispersion medium removed from the reaction product during the extrusion process can be suppressed.

[0054] At the same time, since the reaction product prepared by step S1 contains a large amount of dispersion medium, when the reaction product is added to the extruder after removing a portion of the dispersion medium, the subsequent granulation can be easier. Therefore, the preparation method of the graft copolymer according to the present invention is characterized in that it also includes: before the above-mentioned step S2, (S-1) the percentage of water content in the reaction product is adjusted to less than 30%, wherein the extruder is provided with one or more ventilation components, or further includes: before the above-mentioned step S2, (S1-2) the percentage of water content is adjusted to 30% to 60%, wherein the extruder is provided with two or more side grooves.

[0055] When including adjusting the percentage of water content to less than 30% (S1-1), since the amount of the remaining dispersion medium in the reaction product added to the extruder is small, most of the dispersion medium is evaporated by the heat applied during the extrusion process and is therefore removed in a gaseous state. Therefore, in this case, the extruder is expected to have one or more ventilation components to smoothly remove a large amount of gas. For the ventilation component, a configuration used as a channel can be applied, through which the evaporated material can pass in a conventional extruder, such as a side ventilation stuffer, a side feeder or an open barrel.

[0056] More specifically, the extruder provided with the ventilation component may have Figure 1 The extruder is characterized in that it includes a barrel 10, a screw 30 installed inside the barrel 10, a ventilation component 40 for discharging steam inside the barrel 10 to the outside, and a heater component 60 for heating the barrel 10. In addition, a sealing area is formed by the molten raw material (reaction product) inside the barrel 10.

[0057] The cylinder 10 has a hollow tube shape in its longitudinal direction, a hopper 20 for adding raw materials is coupled to one side of the cylinder, and a discharge port 11 for discharging the dehydrated raw materials, ie, the graft copolymer of the present invention, is formed at the other side of the cylinder.

[0058] The cylinder 10 is desirably manufactured by using a metal having excellent chemical resistance to prevent corrosion due to volatile substances and steam exhausted from the raw materials, or by coating the inner surface of the cylinder with a protective material or the like, and is manufactured to have sufficient rigidity to withstand the heat and pressure generated inside the cylinder.

[0059] The screw 30 has a rod shape and a structure in which threads (M) 31 are formed on an outer peripheral surface thereof. In addition, the screw is connected to the inside of the barrel 10 and moves the raw material added from the hopper 20 while rotating around an axis in one direction.

[0060] At this time, in the screw 30, the thread (M) forms a streamline shape along the longitudinal direction on the outer circumferential surface of the screw, wherein the portion of the thread M formed along the direction in which the raw material moves toward the addition port is divided into a forward zone (F1, F2 and F3 segments), and the portion in which the thread is formed so that the raw material stops moving and only rotates, or moves in the opposite direction (i.e., from the discharge port of the barrel to the feeding hopper) is defined as a kneading zone 30A.

[0061] Meanwhile, in the present invention, the screw 30 may have segments ( F1 , F2 , and F3 ) forming a plurality of advancing zones and segments ( K1 and K2 ) forming a plurality of kneading zones.

[0062] In the first forward zone, a forward-direction screw thread 31 is formed so that the raw material added from the hopper 20 moves toward the discharge port 11 during the shaft rotation, and in the kneading zone 30A, a neutral-type screw thread 32 or a reverse-direction screw thread 33 is formed so that the moving raw material is compressed in the first forward zone during the shaft rotation of the screw 30. In addition, also in the sub-kneading zone 30B, in the same manner as in the kneading zone 30A, a neutral screw thread 32 or a reverse-direction screw thread 33 is formed, and in the second and third forward zones, forward-direction screw threads are formed as in the first forward zone.

[0063] In addition, a ventilation member 40 is mounted on the cylinder 10 to discharge steam (and separated gas, etc.) after the raw material passes through the kneading zone 30A from the hopper 20. The ventilation member 40 may be formed in the shape of a simple pipe opening toward the upper side of the cylinder 10, but may also be configured such that an openable / closable valve, a discharge device for forcibly discharging steam, and a safety valve that opens only at a predetermined pressure or higher are combined with the ventilation member.

[0064] In addition, a heater member 60 for generating heat is coupled to the outer surface (or the inside) of the barrel 10. The heater member 60 may be a device that converts electrical energy into thermal energy, or may be a device that receives a heat source from the outside and heats the barrel.

[0065] A plurality of heater blocks 60 are connected to the entire cylinder, and the heater blocks 60 are respectively configured so that their temperatures can be adjusted individually. Thus, the cylinder 10 is applied so that each section (advancing zone and kneading zone) can be adjusted individually.

[0066] In the extruder of the present invention having the above configuration, when the raw material stored in the hopper 20 is supplied to the barrel 10 , the raw material is fed into the barrel 10 through the screw 30 and heated (or cooled) to a target temperature by the heater part 60 .

[0067] At this time, when the raw material passes through the first advancing zone and reaches the kneading zone 30A, the raw material is subjected to pressure due to the drag of the raw material continuously supplied in a heated state and the rotational force of the screw 30 .

[0068] Therefore, the heated and pressurized raw material is melted in the kneading zone 30A (or before reaching the kneading zone), and at least a part or most of the raw material undergoes a phase change to become a liquid state.

[0069] That is, when a phase change from a solid state to a high-viscosity liquid state is performed in the heated and pressurized raw material in the kneading zone 30A, a force acts to radially diffuse the raw material due to the centrifugal force generated in the kneading zone 30A.

[0070] Therefore, in the front side (close to the hopper side) of the kneading zone 30A, the solid raw material, the steam separated from the raw material, etc. are diffused in the space between the screw 30 and the barrel 10, and as the heat and pressure are continuously applied, most of the raw material in the solid state is melted into a liquid state at the rear side (close to the discharge port side) of the kneading zone 30A. At this time, the molten raw material forms a sealing area that shields the cross section of the barrel 10 by centrifugal force.

[0071] At this time, the thickness and position of the sealing area can be changed according to the rotation speed of the screw 30, the heating temperature of the heater part 60 and the structure of the thread formed inside the kneading zone 30A, but the sealing area is not formed in a fixed state but in a fluid state inside the barrel 10.

[0072] That is, the sealing area forms a liquid film, and when the raw materials are continuously supplied, the raw material that first forms the sealing area passes through the kneading area 30A and is discharged to the second forward area, and the raw material supplied subsequently turns into a liquid state and replenishes the raw material discharged first and maintains the sealing area.

[0073] The heating temperature and the shaft rotation speed of the screw are controlled according to the state and amount of the raw material added in order to continuously maintain the sealing area.

[0074] The liquid raw material and gaseous steam passing through the kneading zone are fed to the area of ​​the second forward zone, at which time the liquid raw material is continuously fed along the screw 30, and the gaseous steam (and the gas generated during the phase change process, etc.) is discharged to the outside through the ventilation part 40. At this time, the steam is prevented from flowing back into the hopper 20 by the sealing area formed in the kneading zone 30A.

[0075] In addition, the raw material reaching the sub-kneading zone 30B forms a sealing zone again in the sub-kneading zone 30B, and is discharged to the discharge port 11 through the third forward zone. When the raw material is fed through the third forward zone, impurities (residual monomers, etc.), gas, residual steam generated during the phase change process, etc. contained in the raw material are discharged to the outside through the sub-ventilation part 50.

[0076] At this time, the raw material discharged to the discharge port 11 of the cylinder 10 is discharged in the form of solid blocks by separating steam, gas, etc. and cooling.

[0077] The raw material discharged in the form of solid blocks is cut into the form of pellets having a certain size by the pulverizing device 70 which pulverizes the dehydrated (dried) raw material.

[0078] Meanwhile, in the extruder of the present invention, it is desirable to limit the distance between the components to improve drying and dehydration performance. Relative to the diameter D of the barrel 10, the distance from the hopper 20 to the kneading zone 30A is ideally determined to be 5D to 10D, the distance between the kneading zone 30A and the ventilation component 40 is ideally determined to be more than 3D, and the distance between the sub-kneading zone 30B and the sub-ventilation component 50 is ideally determined to be less than 3D. However, these relative distances are not limited to the above ranges and can vary according to the length of the screw 30, the shaft rotation speed, the state of the raw material, the output of the heater component 60, etc.

[0079] In the extruder according to the present invention having the above-described configuration, when dehydration of the raw material is performed, a sealed area is formed in the kneading zone 30A, thus having an effect that backflow of steam into the hopper 20 can be prevented or minimized.

[0080] Since the kneading zone 30A may include a neutral zone or a reverse zone, or a combination thereof, the configuration of the kneading zone 30A may be selected according to the state and properties of the raw materials.

[0081] Furthermore, since the screw 30 may further include the sub-kneading zone 30B in the present invention, a sealing area may also be formed, and steam may be maximally discharged from the ventilation member 40 while more effectively preventing steam from flowing back.

[0082] Furthermore, in the extruder according to the present invention, since moisture contained in the raw material is discharged to the ventilation part 40 while being extruded, impurities (residual monomers, etc.) contained in the raw material can be maximally discharged from the sub-ventilation part 50 .

[0083] When including adjusting the percentage of water content in the reaction product to 30% to 60% (S1-2), the amount of dispersion medium remaining in the reaction product is relatively large, so the dispersion medium is not removed in a gaseous state but in a liquid state during extrusion, and therefore, the extruder is ideally provided with side grooves to smoothly remove the liquid dispersion medium. In addition, when the percentage of water content is high, the amount of dispersion medium is large, and therefore, it is ideal that the number of side grooves is two or more. At the same time, adjusting the percentage of water content to 30% to 60% (S1-2) can be a step of specifically adjusting the percentage of water content to 30% to 50%, more specifically 30% to 40%, and the number of side grooves can be 2 to 10, preferably 2 to 5.

[0084] At the same time, if Figure 2 As shown, a specific shape of the extruder including the side slots may include slot members 40A and 40B instead of the vent members in the configuration of the extruder including the vent members described above.

[0085] In the groove members 40A and 40B, a plurality of grooves are formed with gaps therebetween. The grooves are each formed in a long hole shape and are ideally arranged parallel to the longitudinal direction of the barrel 10.

[0086] At this time, the grooves may be formed along the periphery of the barrel 10 with a certain gap therebetween. That is, when the barrel 10 is a cylindrical tube type, the groove part 40A may be formed so that the grooves constitute a ring-shaped configuration along the entire periphery of the barrel 10. However, the grooves may be formed only in a specific portion of the barrel 10 so that the discharge direction of the steam can be controlled inside the barrel 10.

[0087] That is, when grooves are also formed at the lower part of the barrel 10, not only moisture but also a part of the raw material will be discharged, and therefore, grooves cannot be formed on the lower surface of the barrel 10. In addition, for these reasons, the grooves in a specific area may have a larger width or area than other grooves. For example, the grooves formed on the lower surface of the barrel 10 may be formed to be narrow and small in order to prevent the raw material from falling, and the grooves formed on the upper surface of the barrel may be formed to be wider and larger to facilitate the discharge of steam.

[0088] In addition, the groove parts 40A and 40B can also be simply set to form a hole shape, but an openable / closable valve, a discharge device for forced discharge of steam, and a safety vent that opens only at a certain pressure or higher can also be combined thereon.

[0089] Furthermore, in the extruder including the groove member, the distance from the hopper 20 to the kneading zone 30A is ideally determined to be 5D to 10D with respect to the diameter D of the barrel 10. Furthermore, the distance between the kneading zone 30A and the groove member 40A is ideally determined to be 3D or less, the distance between the groove member 40A and the first sub-kneading zone 30B is ideally determined to be 3D or more, and the distance between the first sub-kneading zone 30B and the sub-groove member 40B and the distance between the sub-ventilation member 50 and the second sub-kneading zone 30C are ideally determined to be 3D or less.

[0090] However, such a relative distance is not limited to the above range and may vary according to the length of the screw 30 , the shaft rotation speed, the state of the raw material, the output of the heater part 60 , and the like.

[0091] exist Figure 2 In the extruder shown, the remaining configuration except the groove part can be Figure 1 The extruder shown is described in the same manner as described above.

[0092] The adjustment of the percentage of water content in step S1-1 and step S1-2 can be carried out by the same method as the conventional dehydration and drying process, and those skilled in the art can select and apply specific methods and devices for dehydration and drying according to the target range of the percentage of water content. In addition, the "percentage of water content" in the present invention is not limited to the case where the dispersion medium is water, and also in the case where a liquid other than water is used as a dispersion medium, the content of the dispersion medium remaining in the reaction product can be referred to as the "percentage of water content".

[0093] Thermoplastic resin composition

[0094] The present invention provides a thermoplastic resin composition comprising the graft copolymer and a thermoplastic resin.

[0095] The graft copolymer according to the present invention can be provided as a thermoplastic resin composition by mixing with various thermoplastic resins such as conventional copolymer dry powder.

[0096] Thermoplastic resins that may be mixed with the graft copolymer according to the present invention may include polystyrene resins such as styrene-acrylonitrile (SAN) resins, poly(meth)acrylate resins, polycarbonate resins, and the like.

[0097] The thermoplastic resin composition provided by the present invention exhibits an excellent whiteness index while exhibiting satisfactory physical properties, and thus can be widely used in fields requiring various colors.

[0098] Hereinafter, preferred examples are provided to help understand the present invention. However, the following examples merely illustrate the present invention and cannot be construed as limiting the scope of the present invention.

[0099] Example 1

[0100] The reaction product was prepared by adding 60 parts by weight of a polybutadiene polymer, 30 parts by weight of a styrene monomer and 10 parts by weight of an acrylonitrile monomer to ion exchange water as a dispersion medium and subjecting the mixture to an emulsion reaction. The reaction product was dehydrated and the percentage of water content was adjusted to 18%, and then the resulting product was fed to Figure 1 The reaction product was prepared into pellets in an extruder equipped with a ventilation component. The prepared pellets had a long diameter of 3 mm and a short diameter of 1.5 mm.

[0101] Example 2

[0102] The reaction product prepared in Example 1 was dehydrated to adjust the percentage of water content to 33%, and then fed to Figure 2The extruder was equipped with a groove part to prepare pellets. The long diameter of the prepared pellets was 3 mm and the short diameter was 1.5 mm.

[0103] Comparative Example 1

[0104] The reaction product prepared in the above Example 1 was prepared into a dry powder form through the processes of aggregation, washing, dehydration and drying.

[0105] Comparative Example 2

[0106] The reaction product was prepared by adding 50 parts by weight of polybutyl acrylate polymer, 40 parts by weight of styrene monomer and 10 parts by weight of acrylonitrile monomer to ion exchange water as a dispersion medium and subjecting the mixture to an emulsion reaction. The prepared reaction product was prepared into a dry powder form through a process of aggregation, washing, dehydration and drying.

[0107] Experimental Example 1. Confirmation of bulk density of prepared copolymer

[0108] The bulk density of the copolymers prepared in the above-mentioned embodiments and comparative examples was measured. Specifically, the prepared copolymers were completely filled in a container having a certain volume, and then their weights were measured, and the bulk density was measured by dividing the measured weight by the volume of each container. The measurement results are shown in Table 1 below.

[0109] [Table 1]

[0110]

[0111] From the results in the above table, it can be confirmed that the copolymer according to the present invention has a higher bulk density than the copolymer in the form of dry powder prepared by the existing method.

[0112] Experimental Example 2: Confirming whether agglomeration occurs

[0113] It was confirmed whether agglomeration occurred in the copolymers prepared in Example 2 and Comparative Example 1. Specifically, the prepared copolymers were respectively completely filled in a cylindrical mold (diameter 60 mm) to which lubricating oil was applied, and then particle aggregation was generated by increasing a load of a specific value and applying pressure, and then the mold was removed and the shape of the product was confirmed, thereby confirming how much particle aggregation occurred and the extent to which the aggregation phenomenon was not resolved even after a certain period of time. Figure 3 The applied load and the results according to the elapsed time are shown in FIG.

[0114] like Figure 3As shown, it can be confirmed that in the case of the copolymer prepared in the form of a dry powder, the aggregation phenomenon occurs directly after the load is applied, and a certain degree of aggregation phenomenon is not resolved even after a maximum of 15 days have passed, however, in the copolymer (DPE) prepared in the form of pellets in Example 2, the aggregation phenomenon does not occur at all, and even when a relatively high load is applied, the aggregation phenomenon is easily resolved compared to the dry powder.

[0115] Experimental Example 3. Measurement of yield strength

[0116] The graft copolymers prepared in Example 2, Comparative Example 1 and Comparative Example 2 were subjected to agglomeration in the same manner as in Example 2 above, and then the unconfined yield strength (UYS), which is the force when the formed filter cake shape is destroyed, was measured. The conditions for causing the agglomeration phenomenon were set to 80° C., a pressure of 4.5 kg (15.7 kPa), and a time of 8 days, and the measurement was repeated four times to confirm the reproducibility and obtain the average value. Zwick was used as an apparatus for measuring UYS. The measurement results are shown in Table 2 below.

[0117] [Table 2]

[0118] Example 2 Comparative Example 1 Comparative Example 2 UYS(kPa) Unable to measure 63.1 106.8

[0119] As can be confirmed from the above results, in Comparative Examples 1 and 2 having a dry powder form, a certain degree of force is required until the filter cake shape is destroyed, but in Example 2 having a granular form, since the self-agglomeration phenomenon is not easy to occur, the yield strength cannot be measured. That is, it can be confirmed that the agglomeration phenomenon hardly occurs in the graft copolymer according to the present invention, and the filter cake can be so easily destroyed that the yield strength cannot be measured even if the agglomeration phenomenon occurs, and therefore, the graft copolymer does not strongly aggregate during storage. In contrast, the existing dry powders strongly aggregate with each other when the agglomeration phenomenon occurs during storage, and are therefore not easily decomposed.

[0120] Experimental Example 4: Confirmation of whiteness index and yellowness index

[0121] The copolymer prepared in Comparative Example 1 was fed into the extruder again and prepared into a pellet shape, and the whiteness index (WI) and yellowness index (YI) of the copolymer prepared into a pellet shape in Example 2 and the copolymer prepared into a pellet shape in the comparative example were confirmed by a colorimeter. The results are shown in Table 3 below.

[0122] [Table 3]

[0123] L* a* b* WI YI Example 2 83.02 -2.17 7.20 32.34 12.00 Comparative Example 1 69.32 -1.39 25.67 -29.71 43.67

[0124] In the indexes of Table 3 above, a high whiteness index indicates that the color of the prepared graft copolymer is close to white, and a high yellowness index indicates that the color of the prepared copolymer is close to yellow. As can be confirmed from the results of Table 3, it can be confirmed that the copolymer directly prepared in the form of pellets in the examples of the present invention shows a higher whiteness index and a lower yellowness index than the copolymer prepared in the form of pellets from dry powder in the comparative examples, and even when used with various pigments, etc., the target color can be accurately achieved, and therefore, it can be widely used in industrial fields requiring various colors.

[0125] Description of Reference Numerals

[0126] 10: Cylinder

[0127] 11: Exhaust port

[0128] 20: Hopper

[0129] 30: Screw

[0130] 30A to 30C: Kneading zone

[0131] 31: Thread

[0132] 40: Ventilation components

[0133] 40A: Slot parts

[0134] 40B: Sub-slot component

[0135] 50: Sub-ventilation components

[0136] 60: Heater components

[0137] 70: Crushing device

Claims

1. A method for preparing graft copolymer pellets formed from graft copolymers, the preparation method include: S1 polymerizing a conjugated diene polymer or an acrylate polymer with one or more of a vinyl cyan monomer and an aromatic vinyl monomer to obtain a reaction product comprising a graft copolymer; as well as S2 forms the reaction product in the form of pellets through an extruder, Wherein, the extruder comprises: a barrel, a screw installed inside the barrel, a ventilation component for discharging steam inside the barrel to the outside, and a heater component for heating the barrel; A hopper is coupled to one side of the barrel, and a discharge port for discharging the reaction product is formed on the other side of the barrel; The screw has a segment forming a plurality of advancing zones and a segment forming a plurality of kneading zones; A forward-direction screw thread is formed in the forward zone, and a neutral-type screw thread or a reverse-direction screw thread is formed in the kneading zone.

2. The preparation method according to claim 1, in, The bulk density of the pellets is 450 kg / m 3 Up to 700kg / m 3 .

3. The preparation method according to claim 1, include: S-1 Before step S2, the percentage of water content is adjusted to be less than 30%, wherein the extruder includes a side ventilation component.

4. The preparation method according to claim 1, include: S1-2 Before step S2, the percentage of water content is adjusted to 30% to 60%, wherein the extruder includes two or more side slots.