The invention relates to a manufacturing method of annealing-free cold-drawing medium-carbon high-
sulfur steel which is round steel, takes Fe as a basic element and comprises the following chemical components: 0.40 to 0.50 percent of C, 0.15 to 0.35 percent of Si, 1.35 to 1.65 percent of Mn, less than or equal to 0.040 percent of P, 0.24 to 0.33 percent of S, less than or equal to 0.30 percent of Cr, less than or equal to 0.30 percent of Ni, less than or equal to 0.30 percent of Cu, less than or equal to 0.20 percent of Mo, less than or equal to 0.010 percent of Al and
impurity elements. The production method comprises the steps of converter
smelting, LF refining,
continuous casting of billets, heating and cogging of the
continuous casting billets, finishing of intermediate billets, high-speed
wire rod rolling, acid
pickling and
film coating and combined drawing. Ferroaluminum and
ferrous sulfide are added during converter tapping, the stability of [S] is improved, fine and dispersed aluminum
oxide provides
nucleation conditions for
sulfide inclusions, aluminum deoxidation is not used in the refining process, the
oxygen content in steel is increased, the
oxygen content in
molten steel is controlled to be 0.0020-0.0040%, the form of the
sulfide inclusions in a
casting blank is improved, and through bloom cogging and intermediate blank rolling, the content of the sulfide inclusions in the
casting blank is increased.
Sulfide inclusions which are small in size, uniform in distribution and low in length-
width ratio are obtained through two times of high-temperature rolling, the appropriate drawing
area reduction rate and the appropriate drawing speed are controlled, and the medium
carbon steel cold drawing
cracking phenomenon is restrained.