Pigskin-like moisture-absorbing microfiber leather and preparation method thereof

By using a specific ratio of slurry and a multi-step process, the moisture absorption, breathability, color fastness, and abrasion resistance of microfiber leather have been improved, resulting in the production of imitation pigskin moisture-absorbing microfiber leather. This addresses the shortcomings of existing technologies and meets the application needs of the high-end market.

CN113954487BActive Publication Date: 2024-11-22SHANDONG TONGDA ISLAND NEW MATERIALS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111352892.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-16
Publication Date
2024-11-22
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

Existing moisture-wicking microfiber leathers are inadequate in terms of moisture absorption and breathability, surface texture, color fastness, and abrasion resistance, making it difficult to meet the demands of the high-end market.

Method used

The microfiber leather base fabric is surface-treated using a specific ratio of dry dyeing resin and N,N-dimethylformamide slurry. After the first surface slurry treatment, dyeing, coating and embossing, and the second surface slurry treatment, the genuine leather texture is formed and the surface smoothness and wear resistance are improved. Finally, the fabric is air-rubbed to correct the product color and feel.

Benefits of technology

The prepared imitation pigskin moisture-absorbing microfiber leather has a natural and full texture, good moisture absorption and breathability, color fastness and wear resistance, and a realistic leather feel, which is close to the appearance and touch of genuine leather.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113954487B_ABST
    Figure CN113954487B_ABST
Patent Text Reader

Abstract

The present invention provides a kind of imitation pigskin hygroscopic microfiber leather and its preparation method, and relates to the field of leather technology. The preparation method of the microfiber leather provided by the present invention adopts a slurry including a dry dyeing resin and N,N-dimethylformamide in a specific ratio to perform surface treatment on the microfiber leather base cloth to improve the surface flatness of the microfiber leather base cloth, which is conducive to improving the uniformity of the later coating; then dyeing and coating embossing are performed, so that the product forms a leather texture while a smooth film is formed on the surface layer, which increases the surface flatness and greatly improves the wear resistance; then a second surface slurry treatment is performed to correct the product color, light haze and feel, so that the product is closer to the leather in appearance and touch. The imitation pigskin hygroscopic microfiber leather prepared by the preparation method provided by the present invention has natural and full texture, has a moisture absorption and breathable effect, good color fastness and wear resistance, and a more realistic leather feel on the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather, in particular to a pigskin-like moisture-absorbing ultrafine fiber leather and a preparation method thereof. Background Art

[0002] Due to the limitation and restriction of natural conditions, the quantity of genuine leather is limited, so it is difficult to meet the wide demand and make it into various colors and styles and realize mechanized mass production. In view of the limited natural leather resources, the development of simulated synthetic leather with excellent performance is what people pursue.

[0003] At present, genuine leather occupies the high-end market with its high wearing comfort, while synthetic leather products are mainly distributed in the middle and low-end markets and used as matching leather. The good wearing comfort of genuine leather comes from its good hygienic properties, which are specifically reflected in the moisture absorption and breathability of leather.

[0004] In recent years, superfine fiber synthetic leather with superior properties and use value has developed rapidly. Superfine fiber synthetic leather is a cross-industry product, a new type of high-grade artificial leather made of extremely fine fibers, with the characteristics of genuine leather and superior indicators than genuine leather, and can be used for lining leather, luggage leather, casual shoes, etc. Its research and development and application technology involve many fields such as textiles, plastics, and chemicals.

[0005] However, the hygroscopic microfiber leather prepared by the existing hygroscopic processing method has deficiencies in terms of hygroscopic air permeability, surface texture, color fastness and wear resistance, which need to be improved.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a method for preparing a pigskin-like moisture-absorbing microfiber leather, which is simple and convenient.

[0008] The second purpose of the present invention is to provide a pigskin-like hygroscopic microfiber leather, which is prepared by the above method. The pigskin-like hygroscopic microfiber leather has natural and full texture, moisture absorption and breathability, good color fastness and wear resistance, and a more realistic leather surface.

[0009] In a first aspect, the present invention provides a method for preparing a pigskin-like moisture-absorbing microfiber leather, comprising the following steps:

[0010] The dyeable microfiber leather base fabric is subjected to a first surface slurry treatment, dyeing, lamination and embossing and a second surface slurry treatment in sequence to prepare a pigskin-like hygroscopic microfiber leather;

[0011] Calculated by weight, the slurry for the first surface slurry treatment includes 32 to 48 parts of dry dyeing resin and 80 to 120 parts of N,N-dimethylformamide.

[0012] As a further technical solution, the slurry for the first surface slurry treatment includes 36 to 44 parts of dry dyeing resin and 90 to 110 parts of N,N-dimethylformamide, calculated by weight;

[0013] Preferably, the slurry for the first surface slurry treatment comprises 40 parts of dry dyeing resin and 100 parts of N,N-dimethylformamide, calculated by weight.

[0014] As a further technical solution, the dry dyeing resin includes dry dyeing resin XCS-5230DY and / or dry dyeing resin XCS-5260DY.

[0015] As a further technical solution, a printing press is used for the first surface slurry treatment;

[0016] The sizing amount of the first surface sizing treatment is 14-21 g / m 2 .

[0017] As a further technical solution, the dyeing includes dyeing with a neutral dye;

[0018] Preferably, the dyeing temperature is 95-105°C, and the dyeing time is 30-60 minutes;

[0019] Preferably, a drying step is further included after the dyeing is completed and before the lamination and embossing begins.

[0020] As a further technical solution, the lamination embossing includes covering the TPU hot melt transfer film during the embossing process;

[0021] Preferably, the roller surface temperature during the embossing process is 110-120°C and the pressure is 0.5-0.6 MPa;

[0022] Preferably, the TPU hot melt transfer film has a gram weight of 15-20 g / m 2 .

[0023] As a further technical solution, the second surface slurry treatment material includes 45-55 parts of Permutex WF-48-800, 2.5-3.5 parts of feel agent ROSILK2229, 1-3 parts of Permutex EVO HM-54-002 and 45-55 parts of water, calculated by weight.

[0024] Preferably, the material for the second surface slurry treatment includes, by weight, 50 parts of Permutex WF-48-800, 3 parts of feel agent ROSILK 2229, 2 parts of Permutex EVO HM-54-002 and 50 parts of water.

[0025] As a further technical solution, the second surface slurry treatment method includes spraying;

[0026] Preferably, the spraying amount is 57-71 g / m 2 .

[0027] As a further technical solution, the second surface slurry treatment also includes air kneading treatment.

[0028] In a second aspect, the present invention provides a pigskin-like moisture-absorbing microfiber leather prepared by the above-mentioned preparation method.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The preparation method of the imitation pigskin hygroscopic microfiber leather provided by the present invention comprises the following steps: surface treating a microfiber leather base cloth by using a slurry comprising a dry dyeing resin and N,N-dimethylformamide in a specific ratio, so as to improve the surface flatness of the microfiber leather base cloth, which is beneficial to improving the uniformity of the subsequent coating; then dyeing and coating embossing are performed, so that the product forms leather textures and a smooth film is formed on the surface, the surface flatness is increased, and the wear resistance effect is greatly improved; then a second surface slurry treatment is performed to correct the product color, light haze and feel, so that the product is closer to leather in appearance and touch.

[0031] The imitation pigskin moisture-absorbing superfine fiber leather prepared by the preparation method provided by the invention has natural and full texture, moisture-absorbing and breathable effect, good color fastness and wear resistance, and more realistic leather surface feel. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 The microfiber leather provided by Example 1 and Comparative Example 1 of the present invention;

[0034] Figure 2 The microfiber leather provided by Example 2 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0035] The embodiments of the present invention will be described in detail below in conjunction with the embodiments and examples, but it will be appreciated by those skilled in the art that the following embodiments and examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified, proceed according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] In a first aspect, the present invention provides a method for preparing a pigskin-like moisture-absorbing microfiber leather, comprising the following steps:

[0037] The dyeable microfiber leather base fabric is subjected to a first surface slurry treatment, dyeing, lamination and embossing and a second surface slurry treatment in sequence to prepare a pigskin-like hygroscopic microfiber leather;

[0038] In terms of weight percentage, the slurry for the first surface slurry treatment includes 32-48 parts of dry dyeing resin and 80-120 parts of N,N-dimethylformamide. The dry dyeing resin has the property of being dyeable after drying, and its weight percentage can be, for example, but not limited to 32 parts, 36 parts, 40 parts, 44 parts or 48 parts; the weight percentage of N,N-dimethylformamide (DMF) can be, for example, but not limited to 8 parts, 90 parts, 100 parts, 110 parts or 120 parts.

[0039] The preparation method of the microfiber leather provided by the present invention comprises the following steps: surface treating the microfiber leather base cloth with a slurry comprising a dry dyeing resin and N,N-dimethylformamide (the dry dyeable resin can ensure the dyeability of the treated base cloth without the occurrence of a mottled phenomenon; the main function of DMF is dilution, which reduces the viscosity of the working liquid and is beneficial to the operability of the surface slurry) in a specific ratio, so as to improve the surface flatness of the microfiber leather base cloth, which is beneficial to improving the uniformity of the subsequent coating; then dyeing and coating embossing are performed, so that the product forms a leather texture and a smooth film is formed on the surface, the continuity of the surface film formation is increased, and the wear resistance effect is greatly improved; then a second surface slurry treatment is performed to correct the product color, light haze and feel, so that the product is closer to leather in appearance and touch.

[0040] In some preferred embodiments, the slurry for the first surface slurry treatment includes 36 to 44 parts of dry dyeing resin and 90 to 110 parts of N,N-dimethylformamide, by weight;

[0041] Preferably, the slurry for the first surface slurry treatment comprises 40 parts of dry dyeing resin and 100 parts of N,N-dimethylformamide, calculated by weight.

[0042] By further optimizing and adjusting the ratio of dry dyeing resin and N,N-dimethylformamide in the slurry, the product will not have fuzzing during the dyeing process and the surface will be smoother after dyeing.

[0043] In some preferred embodiments, the dry dyeing resin includes but is not limited to dry dyeing resin XCS-5230DY and / or dry dyeing resin XCS-5260DY, or other dry dyeing resins known to those skilled in the art.

[0044] In some preferred embodiments, a printing press is used for the first surface slurry treatment. The present invention does not specifically limit the type of printing press, for example, a four-plate printing press can be used for the surface treatment.

[0045] The sizing amount of the first surface sizing treatment may be, for example, but not limited to, 14 g / m 2 , 16g / m 2 , 18g / m 2 , 20g / m 2 or 22g / m 2 .

[0046] By further optimizing and adjusting the sizing amount, the surface treatment of the fiber leather base fabric can be better achieved.

[0047] For a microfiber leather base cloth with a certain thickness, after the first surface slurry treatment, the leather base cloth can be split from the middle of its upper and lower surfaces to obtain an upper and lower layer of leather base cloth, the surface treated with the first surface slurry is used as the front side of the leather, and the split surface is used as the back side of the leather. The split surface is raised and can be sanded before subsequent processing.

[0048] In some preferred embodiments, the dyeing is preferably performed using neutral dyes to achieve dyeing of the leather base fabric.

[0049] Preferably, the dyeing temperature may be, for example, but not limited to, 95° C., 97° C., 99° C., 101° C., 103° C. or 105° C., and the dyeing time may be, for example, but not limited to, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min;

[0050] Preferably, a drying step is further included after the dyeing is completed and before the lamination and embossing begins. The drying allows the dye to be fixed on the leather base fabric to achieve the purpose of color fixation.

[0051] In some preferred embodiments, the lamination embossing includes covering the TPU hot melt transfer film during the embossing process. The purpose of this process is to form a thin coating with good continuity on the product surface, cover the fibers of the base fabric itself, and make the product surface closer to the appearance of the first layer of pigskin. The effect is better than other processes. For example, the film formed by the veneer process is thicker and cannot achieve the moisture absorption effect; adding fillers can achieve the moisture absorption effect, the scratch resistance is poor, and the physical properties are low; the roller coating process cannot form a continuous film, the base fabric fibers leak out, the simulation is poor, and the scratch resistance is slightly poor.

[0052] Preferably, the roller surface temperature in the embossing process may be, for example, but not limited to, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, and the pressure may be, for example, but not limited to, 0.5 MPa, 0.54 MPa, 0.58 MPa or 0.6 MPa.

[0053] Preferably, the gram weight of the TPU hot melt transfer film may be, for example, but not limited to, 15 g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 or 20g / m 2 .

[0054] By using the TPU hot melt transfer film of the above-mentioned weight, the surface wear resistance and scratch resistance can be improved after transfer, and the moisture absorption effect of the base fabric is less affected.

[0055] In some preferred embodiments, the second surface slurry treatment material includes, by weight, 45 to 55 parts of Permutex WF-48-800, 2.5 to 3.5 parts of feel agent ROSILK 2229, 1 to 3 parts of Permutex EVO HM-54-002 and 45 to 55 parts of water.

[0056] Permutex WF-48-800 is a matte top-coating water-based polymer, which can improve the scratch resistance and low noise effect of the product surface. In the slurry provided by the present invention, the mass fraction of Permutex WF-48-800 can be, for example, but not limited to 45 parts, 47 parts, 49 parts, 51 parts, 53 parts or 55 parts; the feel agent ROSILK2229 is an organic silicone feel agent with a smooth feel and an effect of improving the skin feel of the coating. In the slurry provided by the present invention, the mass fraction of the feel agent ROSILK2229 can be, for example, but not limited to 2.5 parts, 3 parts or 3.5 parts; Permutex EVO HM-54-002 is a water-based feel agent and wear-resistant additive, which can improve the scratch resistance of the coating. In the slurry provided by the present invention, Permutex EVO The mass fraction of HM-54-002 may be, for example, but not limited to 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts; in the slurry provided by the present invention, the mass fraction of water may be, for example, but not limited to 45 parts, 47 parts, 49 parts, 51 parts, 53 parts or 55 parts.

[0057] The slurry of the present invention is used to perform surface treatment on a product, so that the surface of the product is coated with water-based resin, the color, light haze and hand feel of the product are corrected, and the wear resistance of the product is improved.

[0058] Preferably, the material for the second surface slurry treatment includes, by weight, 50 parts of Permutex WF-48-800, 3 parts of feel agent ROSILK2229, 2 parts of PermutexEVO HM-54-002 and 50 parts of water.

[0059] By further optimizing and adjusting the slurry components, the appearance and feel of the product are closer to real leather.

[0060] In some preferred embodiments, the second surface slurry treatment is preferably performed by spraying;

[0061] Preferably, the spraying amount of the spraying can be, for example, but not limited to, 57 g / m 2 , 62g / m 2 , 66g / m 2 or 71g / m 2 .

[0062] By further optimizing and adjusting the spraying amount, the product surface can be treated while saving slurry usage.

[0063] In some preferred embodiments, the second surface slurry treatment further includes an air kneading treatment.

[0064] Through the air kneading process, the product is fully kneaded to make the texture natural and enhance the fullness.

[0065] In a second aspect, the present invention provides a pigskin-like moisture-absorbing microfiber leather prepared by the above-mentioned preparation method.

[0066] The imitation pigskin hygroscopic microfiber leather prepared by the preparation method provided by the present invention has natural and full texture, hygroscopic and breathable effect, good color fastness and wear resistance, and more realistic surface leather feel. Compared with genuine leather, it has higher physical properties, color fastness, and wear resistance; compared with veneer hygroscopic microfiber leather, the scratch resistance effect is significantly improved, and the texture is more natural and full; compared with roller-coated hygroscopic microfiber leather, the roller-coated hygroscopic inner lining has obvious microfiber characteristics (surface fibers, pinholes, etc.), and the texture of this product is more natural and full, with good wear resistance and more realistic surface leather feel.

[0067] The present invention is further described below by means of specific examples and comparative examples. However, it should be understood that these examples are only used for more detailed description and should not be construed as limiting the present invention in any form.

[0068] Example 1

[0069] A kind of pigskin-like moisture-absorbing microfiber leather, the preparation method is as follows:

[0070] Process: microfiber leather base cloth - first surface slurry treatment - peeling - sanding - dyeing - laminating and embossing - second surface slurry treatment - air kneading.

[0071] ① The first surface slurry treatment: Use a four-plate printing press to perform surface treatment on the front and back of the base fabric.

[0072] Slurry (mass ratio): XCS-5230DY:dmf=40:100.

[0073] (XCS-5230DY is a dry dyeing resin produced by Asahikawa Chemical), the sizing amount is controlled at 14-21g / m 2 .

[0074] ②Leather peeling-sanding-dyeing-drying

[0075] The leather base fabric that has undergone the first surface treatment is split (the leather base fabric is cut in the middle of the upper and lower surfaces to obtain two thinner leather base fabrics), and then the cut portion is sanded, and then dyed with neutral dyes produced by Taifeng, the dyeing temperature is controlled at 95-105°C, the dyeing time is 30-60 minutes, and then dried after dyeing.

[0076] ③Embossed: Use process ① with the surface as the front side for embossing.

[0077] During the embossing process, a thin TPU hot-melt transfer film (Nantong Hehe Plastic New Materials Co., Ltd.) is covered to form a smooth film on the surface while the product has texture.

[0078] Production conditions:

[0079] During the production process, the roller surface temperature is controlled at 110-120℃ and the pressure is 0.5-0.6mpa.

[0080] TPU hot melt transfer film requirements:

[0081] Choose a film weight of 15-20g / m 2 Range of TPU hot melt transfer films.

[0082] ④Spraying: The product surface is coated with water-based resin to correct the color, light haze and feel.

[0083] Slurry ratio:

[0084] Slurry name Proportion Permutex WF-48-800 50 water 50 ROSILK 2229 3 Permutex EVO HM-54-002 2

[0085] Spraying amount is controlled at: 57-71g / m 2 .

[0086] ⑤ Air kneading: fully knead the skin to make the texture natural and enhance the fullness.

[0087] Example 2

[0088] A pigskin-like hygroscopic microfiber leather, the preparation method of which is different from that of Example 1 in that the dry-dyed resin used in the first slurry treatment is the dry-dyed resin XCS-5260DY produced by Asahikawa Chemical.

[0089] Comparative Example 1

[0090] A veneered moisture-absorbing microfiber leather.

[0091] Process flow: base fabric dyeing - veneer - leather kneading.

[0092] 1. dyeing process is with embodiment 1.

[0093] ② Veneer: Select the texture according to your needs.

[0094] Veneer slurry:

[0095] Surface resin:

[0096] Resin: matting powder: calcium carbonate: DMF: moisture absorbing agent = 100:1:5:90:5 (mass ratio);

[0097] Base resin:

[0098] Resin: matting powder: calcium carbonate: DMF: hygroscopic agent = 100:1:8:70:5 (mass ratio);

[0099] The slurry gap is 0.15mm for the surface layer and 0.15mm for the bottom layer; the slurry gap refers to the resin thickness of the surface layer and the bottom layer in the undried state.

[0100] ③ Kneading the leather: Roller kneading the leather helps to increase looseness and improve the overall moisture absorption effect.

[0101] Problem: Poor scratch resistance (such as Figure 1 As shown, Figure 1 The left side is the product of Example 1, and the right side is the product of Comparative Example 1. After cutting the middle position of the two products, it can be seen that the scratch on the right product is more obvious than that on the left product). The coating amount has a greater effect on moisture absorption, and the moisture absorption stability is slightly poor.

[0102] Comparative Example 2

[0103] The utility model relates to a roller-coated moisture-absorbing microfiber leather.

[0104] Process flow: base fabric surface treatment - dyeing - roller coating - air kneading;

[0105] Base fabric treatment: Surface treatment and dyeing are the same as in Example 1.

[0106] Roller coating: Apply the slurry in step ④ of Example 1 in the same coating amount;

[0107] Wind kneading: wind kneading machine kneading pattern.

[0108] Problem: Poor scratch resistance (such as Figure 2 As shown, Figure 2 The left side is the product of Example 2, and the right side is the product of Comparative Example 2. After cutting the middle position of the two products, it can be seen that the scratches on the right product are more obvious than those on the left product). The texture is the natural texture of the base fabric, the texture is single and has poor three-dimensional sense, poor surface film formation, and poor leather feel.

[0109] Test Example 1

[0110] The performance of the microfiber leather of Example 1-2 was tested, and the results were as follows:

[0111] After testing, the color fastness of the imitation pigskin moisture-absorbing microfiber leather of Example 1 and Example 2 is: dry rubbing color fastness ≥ level 4; wet rubbing color fastness ≥ level 3.5; Martindale test: dry friction 25600 turns ≥ level 4, water vapor permeability coefficient ≥ 70 mg / cm 2 .

[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a pigskin-like hygroscopic microfiber leather, characterized in that: The following steps are involved: The dyeable microfiber leather base fabric is subjected to a first surface slurry treatment, dyeing, lamination and embossing and a second surface slurry treatment in sequence to prepare a pigskin-like hygroscopic microfiber leather; The slurry for the first surface slurry treatment includes 32 to 48 parts of dry dyeing resin and 80 to 120 parts of N,N-dimethylformamide by weight; The lamination embossing is to cover the TPU hot melt transfer film during the embossing process; The roller surface temperature during the embossing process is 110-120°C and the pressure is 0.5-0.6 MPa; The weight of the TPU hot melt transfer film is 15-20g / m 2 ; The slurry for the second surface slurry treatment includes 45-55 parts of Permutex WF-48-800, 2.5-3.5 parts of the feel agent ROSILK 2229, 1-3 parts of Permutex EVO HM-54-002 and 45-55 parts of water in parts by weight; The first surface slurry treatment is performed using a printing press; the sizing amount of the first surface slurry treatment is 14-21 g / m 2 ; The dyeing process includes dyeing with a neutral dye; the dyeing temperature is 95-105° C., and the dyeing time is 30-60 minutes; and a drying step is also included after the dyeing process is completed and before the lamination and embossing process begins.

2. The preparation method according to claim 1, characterized in that: Calculated by weight, the slurry for the first surface slurry treatment includes 36-44 parts of dry dyeing resin and 90-110 parts of N,N-dimethylformamide.

3. The preparation method according to claim 2, characterized in that: The slurry for the first surface slurry treatment includes 40 parts of dry dyeing resin and 100 parts of N,N-dimethylformamide by mass.

4. The preparation method according to claim 1, characterized in that: The dry dyeing resin includes dry dyeing resin XCS-5230DY and / or dry dyeing resin XCS-5260DY.

5. The preparation method according to claim 1, characterized in that The slurry for the second surface slurry treatment includes, by weight, 50 parts of Permutex WF-48-800, 3 parts of the feel agent ROSILK 2229, 2 parts of Permutex EVO HM-54-002 and 50 parts of water.

6. The preparation method according to claim 1, characterized in that: The second surface slurry treatment method includes spraying; The spraying amount of the spraying is 57~71g / m 2 .

7. The preparation method according to claim 1, characterized in that: The second surface slurry treatment also includes air kneading treatment.

8. The pigskin-like hygroscopic microfiber leather prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Thin type micro villus polyurethane certificate leather and preparation method thereof

    CN103469608A

  • Preparation method of moisture-absorbing ventilating superfine fiber polyurethane synthetic leather

    CN104452326A

  • Manufacturing method for acylamino polyurethane suede artificial leather convenient for dyeing

    CN106758306A

  • Manufacturing method of microfiber top leather

    CN106948180A

  • Suede nap ultra-soft protein leather

    CN109098008A