Composite particles and method for producing the same, personal care products, particles for personal care and method for producing the same, personal care products, and personal care compositions
By dissolving fibers in the solvent to form a dispersion of cellulose and chitin nanofibers, and covering the surface with droplets to form composite particles with porous structures, the problem of poor dispersion stability of porous particles in the prior art is solved, and oil absorption is achieved Improved sexual and moisturizing properties and reduced environmental load.
Patent Information
- Application Number
- CN202080041771.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-06
- Filing Date
- 2020-06-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-06-03
AI Technical Summary
The prior art is difficult to prepare porous particles with good dispersion stability, oil absorption and moisturizing properties, and it is difficult to take into account both oil absorption and moisturizing properties. The low concentration of solid components of the fine fibers leads to high transportation costs and poor processing properties.
Cellulose nanofibers and chitin nanofibers are used as microfibers to form a dispersion liquid by dissolving fibers in solvents, and the surface of the droplets is covered with microfibers. Then solidified to form core particles, and finally removed into pore agents to form pore structures. composite particles.
The dispersion stability and skin affinity of composite particles are achieved, and the oil absorption and moisturizing properties are significantly improved. By loading functional materials on microfibers, the dispersion stability of functional materials is maintained and the load on the environment is reduced. .
Smart Images

Figure CN114007572B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to composite particles, a method for producing the composite particles, and a personal care product containing the composite particles, as well as personal care particles, a method for producing the personal care particles, and a personal care product and a personal care composition. Background Art
[0002] Various functional materials are added to personal care products for the purpose of skin care or makeup, hair care, oral care, nail care, etc. For example, cosmetics such as foundation contain: oily raw materials headed by oils / waxes; functional materials such as ultraviolet absorbers or colorants, fungicides, antioxidants, preservatives, moisturizers, vitamins, amino acids, hormones, natural extracts; and microparticles for improving skin affinity. In addition, in skin care products, functional materials are added to a dispersion solvent composed of water, alcohol or oil in any proportion. These personal care products are used to meet the following various required characteristics: moisturizing, color development, ultraviolet protection, antibacterial, smoothness when applied to the skin, etc., and good skin affinity.
[0003] As personal care products that have been put into practical use, there are products composed of various microparticles or microcapsules. Generally, microparticles are micron-sized particles formed by various polymers such as polyethylene and polypropylene, and are widely used in the following personal care applications: in foundation to improve the feel and give soft focus; or as an exfoliant in facial cleansers.
[0004] For the fine particles used in foundation, in order to improve the feeling of foundation, impart oil absorption, impregnate active ingredients, and exhibit high soft-focus properties, studies have been conducted on making the fine particles porous or hollow.
[0005] In addition, attempts have been made to impart and express more functionality by forming a microcapsule structure with microparticles as the core material and a wall membrane covering the surface of the particles. Specifically, functional materials such as drugs, fragrances, enzymes, pigments, dyes, etc. are incorporated into the core material for microencapsulation, thereby enabling protection of the functional materials, control of release behavior, etc. The functional materials can also be further imparted to the wall membrane itself covering the core material.
[0006] However, micron-sized particles are generally prone to aggregation due to their large specific surface area, and thus dispersion stability becomes a problem.
[0007] Therefore, there is a strong demand for new microparticles that have good dispersion stability, exert various functions such as moisturizing, pore correction, and softening, have good skin affinity, and are suitable for personal care products.
[0008] On the other hand, in recent years, attempts have been actively made to miniaturize cellulose fibers in wood and chitin and / or chitosan constituting the shells of crustaceans such as crabs so that at least one side of the structure reaches nanometer order and use them as new materials.
[0009] For example, Patent Document 1 discloses that micronized cellulose, namely cellulose nanofibers (hereinafter also referred to as CNF), is obtained by repeatedly mechanically treating wood cellulose with a stirrer or a grinder. It is reported that the CNF obtained by this method has a short axis diameter of 10 to 50 nm and a long axis diameter of 1 μm to 10 mm. This CNF weighs 1 / 5 of steel, but has a strength of more than 5 times that of steel and has a diameter of 250 m. 2 Due to its huge specific surface area of more than 100 / g, it is expected to be used as a filler or adsorbent for resin reinforcement.
[0010] In addition, attempts have been actively made to produce CNF by chemically treating cellulose fibers in wood in advance to promote micronization, and then micronizing them by low-energy mechanical treatment similar to a household mixer. The chemical treatment method is not particularly limited, but a method in which anionic functional groups are introduced into cellulose fibers to promote micronization is preferred. By introducing anionic functional groups into cellulose fibers, the solvent can easily penetrate into the cellulose microfibril structure due to the osmotic pressure effect, and the energy required for micronization of the cellulose raw material can be greatly reduced.
[0011] The method for introducing the anionic functional group is not particularly limited, and for example, Non-Patent Document 1 discloses a method of selectively subjecting the surface of fine cellulose fibers to a phosphate esterification treatment using a phosphate esterification treatment.
[0012] Patent Document 2 discloses a method for carboxymethylation by reacting cellulose with monochloroacetic acid or sodium monochloroacetate in a high-concentration alkaline aqueous solution. Alternatively, carboxyl groups may be introduced by directly reacting carboxylic anhydride compounds such as maleic acid or phthalic acid vaporized in an autoclave with cellulose.
[0013] A method for selectively oxidizing the surface of cellulose microfibers by using a relatively stable N-oxyl compound, 2,2,6,6-tetramethylpiperidinyl-1-oxyl radical (TEMPO), as a catalyst has also been reported (for example, see Patent Document 3). The oxidation reaction using TEMPO as a catalyst (TEMPO oxidation reaction) can be environmentally friendly chemically modified in an aqueous system, at room temperature and pressure. When it is applied to cellulose in wood, no reaction occurs inside the crystal, so that only the primary carbon of the cellulose molecular chain on the surface of the crystal can be selectively converted into a carboxyl group.
[0014] Due to the osmotic pressure effect associated with the ionization of carboxyl groups selectively introduced into the crystal surface by TEMPO oxidation, cellulose single nanofibers (hereinafter also referred to as CSNF, TEMPO-oxidized cellulose nanofibers, TEMPO-oxidized CNF) dispersed in a solvent as cellulose microfibril units one by one can be obtained. CSNF exhibits high dispersion stability derived from the carboxyl groups on the surface. It has been reported that the wood-derived CSNF obtained from wood by TEMPO oxidation reaction is a structure with a high aspect ratio, in which the short axis diameter reaches about 3 nm and the long axis diameter reaches tens of nm to several μm, and its aqueous dispersion and molded body have high transparency. In addition, Patent Document 4 reports that a laminated film obtained by coating a CSNF dispersion and drying has gas barrier properties.
[0015] Further, research is being conducted to give more functions to CNF or CSNF. For example, more functions can be given by utilizing the carboxyl group on the CSNF surface. Patent documentation 5 discloses a composite (metal nanoparticle loaded CSNF) formed by metal reduction precipitation under the state of metal ion adsorption on the carboxyl group on the CSNF surface, thereby loading metal nanoparticles on the CSNF. The example of using metal nanoparticle loaded CSNF as a catalyst is disclosed in this patent documentation 5, and it is reported that metal nanoparticles can be stably dispersed under the state of high specific surface area, thereby improving catalytic activity.
[0016] Patent document 6 discloses that chitosan and / or chitosan extracted from crab shells, etc., are crushed into ultrafine fibers to obtain chitosan nanofibers (chitosan nanofibers). Chitosan nanofibers are a recycling resource, have antibacterial properties and biodegradability, and can be expected to be used for food and cosmetics addition, film reinforcement fibers, etc., agricultural resource utilization, medical use, etc.
[0017] Since chitin and / or chitosan are tightly bound to each other by strong hydrogen bonds, it is not easy to prepare completely individual nanofibers from chitin and / or chitosan. According to the chitosan nanofibers and the method for producing the same described in Patent Document 6, a dispersion containing chitosan nanofibers separated into individual fibers can be obtained by a simple process.
[0018] As described above, various studies have been conducted on the development of highly functional components by imparting new functions to fine fibers derived from natural materials such as cellulose nanofibers and chitin nanofibers.
[0019] Here, for the practical application of these fine fibers, the problem is that the solid content concentration of the obtained fine fiber dispersion may be as low as about 0.1 to 5%. For example, when it is desired to transport the fine fiber dispersion, there is a problem that the transportation cost is high because it is equivalent to transporting a large amount of solvent and the processability is significantly impaired.
[0020] However, if the solvent of the dispersion of fine fibers is simply removed by heating and drying, the fine fibers will aggregate / keratinize or form a film, making it difficult to effectively utilize the large specific surface area of the fine fibers and thus difficult to exhibit stable functions. In addition, since the solid content concentration of the fine fibers is low, the process of removing the solvent by drying itself consumes a lot of energy, which is also a reason why processability is impaired.
[0021] As such, the operation of treating fine fibers such as cellulose nanofibers and chitin nanofibers in a dispersion state itself causes the processability to be impaired. Therefore, as composite particles having fine fibers bonded to the surface, it is strongly desired that they have a new treatment mode that can effectively utilize the large specific surface area of the fine fibers and can be easily washed and separated from the solvent.
[0022] Prior art literature
[0023] Patent Literature
[0024] Patent Document 1: Japanese Patent Application Publication No. 2010-216021
[0025] Patent Document 2: International Publication No. 2014 / 088072
[0026] Patent Document 3: Japanese Patent Application Publication No. 2008-001728
[0027] Patent Document 4: International Publication No. 2013 / 042654
[0028] Patent Document 5: International Publication No. 2010 / 095574
[0029] Patent Document 6: Japanese Patent Application Publication No. 2010-180309
[0030] Non-patent literature
[0031] Non-patent document 1: Noguchi Y, Homma I, Matsubara Y. Complete nanofibrillation of cellulose prepared by phosphorylation. Cellulose. 2017; 24: 1295.10.1007 / s10570-017-1191-3 Summary of the invention
[0032] Problems to be Solved by the Invention
[0033] As described above, a novel particle having good skin affinity and applicable to personal care products is strongly desired, but when porous particles are prepared by conventional methods, the particle shape cannot be maintained and the feel of use is poor. In addition, in conventional methods, it is difficult to achieve both oil absorption and moisture retention in porous particles.
[0034] The first object of the present invention is to provide composite particles having fine fibers bonded to the surface, which can maintain a spherical shape even if they are porous particles or hollow particles with high porosity, and have excellent dispersion stability, good skin affinity, and can exhibit excellent oil absorption and moisturizing properties.
[0035] A second object of the present invention is to provide personal care particles that have good dispersion stability, exhibit various functions such as moisture retention and color development, and have good skin affinity.
[0036] Solutions to Solve Problems
[0037] In order to solve the above-mentioned first problem, the present invention provides the following first aspect, second aspect, and third aspect.
[0038] [First method]
[0039] A composite particle comprises: a core particle having pores; and fine fibers composed of at least one of cellulose nanofibers and chitin nanofibers which are inseparable and bonded to the surface of the core particle.
[0040] [Second Method]
[0041] A method for producing composite particles, comprising: (1) defibration of either or both of a cellulose raw material and a chitin / chitosan raw material in a solvent to obtain a dispersion in which fine fibers, at least one of cellulose nanofibers and chitin nanofibers, are dispersed; (2) droplets containing a pore-forming agent that generates pores by removal and a core material that becomes a core particle by solidification are dispersed in the dispersion so that the surfaces of the droplets are covered with the fine fibers; (3) the core material inside the droplets is solidified to obtain a dispersion of core particles containing a pore-forming agent inside and covered with fine fibers on the surface; and (4) recovering the core particles from the obtained dispersion of the core particles and removing the pore-forming agent from the inside of the recovered core particles to generate pores inside the core particles.
[0042] [Third Method]
[0043] A method for producing composite particles, comprising: (11) defibration of either or both of a cellulose raw material and a chitin / chitosan raw material in a solvent to obtain a dispersion in which fine fibers of at least one of cellulose nanofibers and chitin nanofibers are dispersed; (12) dispersing droplets containing a pore-forming agent that generates pores by removal in a core material that becomes a core particle by solidification to prepare a W / O type emulsion, dispersing droplets containing the W / O type emulsion in the fine fibers of the core material; (13) a process for solidifying the core material inside the droplets of the W / O / W emulsion to obtain a dispersion of core particles containing droplets composed of a pore-forming agent and having their surfaces covered with fine fibers; and (14) a process for recovering the core particles from the obtained dispersion of the core particles and removing the pore-forming agent from the inside of the recovered core particles to generate pores inside the core particles.
[0044] The composite particles of the first aspect may be included in a personal care product.
[0045] In order to solve the above-mentioned second problem, the present invention provides the following fourth aspect, fifth aspect, and sixth aspect.
[0046] [Fourth Method]
[0047] A particle for personal care comprises: a core particle formed of a material containing a polymer; fine fibers composed of at least one of cellulose nanofibers and chitin nanofibers which are inseparable and bonded to the surface of the core particle; and a functional material which performs a personal care function and is carried on the fine fibers.
[0048] [Fifth Method]
[0049] A method for producing particles for personal care, comprising: (21) defibration of either or both of a cellulose raw material and a chitin / chitosan raw material in a solvent to obtain a dispersion of microfibers that are at least one of cellulose nanofibers and chitin nanofibers; (22) loading a functional material that exerts a personal care function on the microfibers in the dispersion of the microfibers to obtain a dispersion of microfibers loaded with the functional material; (23) dispersing droplets containing a core material in the dispersion of microfibers loaded with the functional material so that the surface of the droplets is coated with the microfibers loaded with the functional material; and (24) solidifying the core material inside the droplets coated with the microfibers loaded with the functional material.
[0050] [Sixth Method]
[0051] A method for producing particles for personal care, comprising: (31) defibration of either or both of a cellulose raw material and a chitin / chitosan raw material in a solvent to obtain a dispersion of fine fibers that are at least one of cellulose nanofibers and chitin nanofibers; (32) dispersing droplets containing a core material in the dispersion of fine fibers so that the surfaces of the droplets are covered with the fine fibers; (33) solidifying the core material inside the droplets to obtain a dispersion of particles in which the surfaces of the core particles are covered with fine fibers; and (34) in the dispersion of the particles, loading a functional material that exerts a personal care function on the fine fibers on the surfaces of the particles covered with the fine fibers.
[0052] The personal care particles of the fourth embodiment can be contained in personal care products and personal care compositions.
[0053] Effects of the Invention
[0054] According to the first embodiment of the composite particles of the present invention, it can be expected that a composite particle having fine fibers bonded to the surface can maintain a spherical shape even if it is a porous particle or a hollow particle with a high porosity, and has excellent dispersion stability, good skin affinity, and can exhibit excellent oil absorption and moisturizing properties.
[0055] According to the production methods of the second and third aspects of the present invention, the composite particles of the first aspect of the present invention can be produced.
[0056] The personal care particles according to the fourth aspect of the present invention are expected to have good smoothness and skin affinity and excellent moisturizing properties by coating the core particles with fine fibers having high safety, high hydrophilicity and a large specific surface area.
[0057] In addition, since the functional material is loaded on fine fibers with a large specific surface area, the dispersion stability of the functional material can be maintained, thereby providing personal care particles that can effectively exert the functions of functional materials such as UV protection (absorption and / or scattering), color development, and antibacterial.
[0058] Furthermore, since cellulose nanofibers and chitin nanofibers are composed of cellulose and chitin / chitosan, which are biodegradable polymers, personal care particles with reduced environmental load can be provided by using a biodegradable polymer as a polymer contained in the core particle.
[0059] According to the production methods of the fifth and sixth aspects of the present invention, the personal care particles of the fourth aspect of the present invention can be produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] [ Figure 1A ] is a schematic diagram showing composite particles according to the first embodiment (an embodiment of the first mode) of the present invention.
[0061] [ Figure 1B ] is a schematic diagram showing composite particles according to the first embodiment (an embodiment of the first mode) of the present invention.
[0062] [ Figure 1C ] is a schematic diagram showing composite particles according to the first embodiment (an embodiment of the first mode) of the present invention.
[0063] [ Figure 2 ] is a diagram for illustrating the method for producing composite particles according to the first embodiment (production method I).
[0064] [ Figure 3 ] is a diagram for illustrating the method for producing composite particles according to the first embodiment (production method II).
[0065] [ Figure 4 ] is a schematic diagram showing the personal care particles according to the second embodiment (an embodiment of the fourth embodiment) of the present invention.
[0066] [ Figure 5 ] is a diagram for illustrating the method for producing personal care particles according to the second embodiment (production method III).
[0067] [ Figure 6 ] is a diagram for illustrating the method for producing personal care particles according to the second embodiment (production method IV).
[0068] [ Figure 7 ] is a graph showing the results of spectral transmission spectrum measurement of the aqueous dispersion of cellulose nanofibers obtained in Example 1.
[0069] [ Figure 8 ] is a graph showing the results of steady-state viscoelasticity measurement of the aqueous dispersion of cellulose nanofibers obtained in Example 1 using a rheometer.
[0070] [ Fig. 9 ] is a microscope photograph (SEM image) of the personal care particles loaded with silver particles obtained in Example 21.
[0071] [ Fig.10 ] is a microscope photograph (SEM image) of the personal care particles loaded with flat silver particles obtained in Example 22.
[0072] [ Fig.11 ] is a microscope photograph (SEM image) of the personal care particles loaded with gold particles obtained in Example 29. DETAILED DESCRIPTION
[0073] Hereinafter, the embodiments of the present invention will be described using the accompanying drawings. In addition, in each of the drawings described below, the corresponding parts are marked with the same symbols, and the repeated parts will be appropriately omitted in the following description. In addition, this embodiment illustrates the structure for concretizing the technical idea of the present invention, and the material, shape, structure, configuration and size of each part are not limited to the following description. The technical idea of the present invention can be variously changed within the technical scope defined by the claims recorded in the claims.
[0074] [First embodiment]
[0075] like Figure 1A , Figure 1B , Figure 1C As shown, the composite particle 1 of this embodiment has: a core particle 2 having pores (pores: pores) 4; and fine fibers 3 which are at least one of cellulose nanofibers and chitin nanofibers and are inseparable from the surface of the core particle 2. That is, the fine fibers 3 may be only one of the cellulose nanofibers and the chitin nanofibers, or may contain both.
[0076] exist Figure 1A In the composite particle 1 shown, the core particle 2 has a large number of small pores 4. That is, Figure 1A The composite particle 1 is shown in which the core particle 2 is a porous particle. In the core particle 2, there are parts where the pores 4 exist independently, and there are also parts where a plurality of pores 4 are connected together. Some of the pores 4 existing in the periphery of the core particle 2 are open on the surface of the core particle 2, and some are not open.
[0077] exist Figure 1BIn the composite particle 1 shown, the core particle 2 has a plurality of relatively large pores 4. That is, Figure 1B The composite particle 1 in which the core particle 2 is a multi-hollow particle is shown.
[0078] exist Figure 1C In the composite particle 1 shown, the core particle 2 has a large pore 4. That is, Figure 1C A composite particle 1 in which the core particle 2 is a single hollow particle is shown.
[0079] Thus, the size, shape, and number of the pores 4 of the core particle 2 are not particularly limited, and the number of the pores 4 may be one or more. In addition, the pores 4 may exist independently, or multiple pores 4 may be connected together, and the pores 4 may be open on the surface of the core particle 2 or closed.
[0080] In the present embodiment, the fine fibers 3 are formed as a coating layer covering the surface of the core particle 2. That is, in the composite particles of the first embodiment, the fine fibers are preferably formed as a coating layer covering the surface of the core particle.
[0081] The method for producing the composite particles 1 is not particularly limited, and a known method can be used, such as a chemical production method or a physicochemical production method.
[0082] Examples of the chemical preparation method include polymerization granulation methods (emulsion polymerization method, suspension polymerization method, seed polymerization method, radiation polymerization method, etc.) in which particles are formed from polymerizable monomers during polymerization.
[0083] Examples of the physicochemical preparation method include a dispersion granulation method (spray drying method, liquid solidification method, solvent evaporation method, phase separation method, solvent dispersion cooling method, etc.) in which particles are formed from a polymer solution in the form of microdroplets.
[0084] For example, first, droplets containing a pore former (a material that generates pores by removal in a later step) and a core material (core particle precursor, core precursor) that forms core particles by solidification are dispersed in a dispersion of fine fibers to form an O / W type Pickering emulsion.
[0085] Next, the core material inside the droplet is solidified. Thus, the core particle containing the pore-forming agent inside and covered with fine fibers on the surface can be combined with the fine fibers and in an inseparable state. Next, during or after the core material is solidified, the pore-forming agent is removed. As a result, a composite particle 1 can be obtained in which the fine fibers 3 are inseparably combined with the surface of the core particle 2 having pores 4.
[0086] According to this method, by using fine fibers, stable droplets can be formed without using additives such as surfactants, and a true spherical shape can be maintained even with a high porosity, and composite particles with high dispersibility, good smoothness, and good skin affinity can be obtained.
[0087] Here, the O / W emulsion is also referred to as an oil-in-water emulsion, that is, water is used as a continuous phase, and oil is dispersed in the form of oil droplets (oil particles).
[0088] The core material is not particularly limited, as long as it is a material that can form core particles by solidification. As the core material, for example, a polymerizable monomer, a molten polymer, or a soluble polymer can be used. The solidification method of the core material is not particularly limited, and the core material can be solidified by polymerizing the polymerizable monomer, solidifying the molten polymer, and removing the solvent from the soluble polymer.
[0089] As pore-forming agents, non-polymerizable solvents, linear polymers, solid particles, etc. can be used. Examples of non-polymerizable solvents include hydrophobic solvents such as n-hexane, n-heptane, n-dodecane, and toluene; hydrophilic solvents such as ethanol and methanol; and water. Examples of linear polymers include polymethyl methacrylate, polyethylene oxide, polypropylene oxide, and polymethylsiloxane. Examples of solid particles include calcium carbonate, etc.
[0090] The method for removing the porogen is not particularly limited, and examples thereof include a method of drying under normal pressure or reduced pressure, at normal temperature or under heating, or dissolving the porogen using a good solvent such as toluene, depending on the porogen used.
[0091] For example, when a non-polymerizable solvent is used as a pore-forming agent, the core material is mixed and dissolved in the non-polymerizable solvent to obtain a solution, and droplets containing the solution (core material and non-polymerizable solvent) are dispersed in a dispersion of fine fibers so that the surface of the droplets is covered with fine fibers. Next, the core material inside the droplets is solidified. Here, the non-polymerizable solvent dissolved in the core material comes out of the droplets and enters the dispersion during the solidification of the core material, thereby being removed. As a result, composite particles in which the portion where the non-polymerizable solvent once existed becomes pores can be obtained.
[0092] In addition, composite particles having pores can also be obtained by mixing an excess of an oil-soluble surfactant into the core material. When an excess of an oil-soluble surfactant is contained above the critical micelle concentration, micelles are formed. When micelles are contained in the droplets, the hydrophilic solvent of the continuous phase is absorbed into the droplets, thereby playing a role as a pore-forming agent.
[0093] In addition, a hydrophilic solvent (pore former) such as water is dispersed in a core material using an oil-soluble surfactant or a stabilizer such as fine fibers in advance to prepare a W / O type emulsion, and the resulting W / O type emulsion is dispersed in a dispersion of fine fibers to prepare a W / O / W type emulsion, and then the core material is solidified and the hydrophilic solvent such as water is removed, thereby obtaining porous or hollow composite particles.
[0094] Here, W / O type emulsion is also called water-in-oil type, that is, oil is used as the continuous phase, and water is dispersed in the form of water droplets (water particles). W / O / W type emulsion is also called water-in-oil-in-water type emulsion, which is a double emulsion in which oil droplets (oil particles) with water droplets (water particles) dispersed inside are dispersed in water.
[0095] Furthermore, by including a linear polymer in the core material, the linear polymer can be dissolved using a good solvent such as toluene after preparing particles covered with fine fibers.
[0096] Personal care products refer to cosmetics, toiletries, and other products that keep human skin clean, modify or beautify the appearance. They are hair care, oral care, odor care, nail care, body care, skin care, cosmetics related products, etc. For example: toothpaste, perfume, nail polish, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair spray, hair spray, shampoo, conditioner, hair toner, body lotion, face cream, and soap, etc.
[0097] The composite particles 1 of this embodiment can be Figure 2 and Figure 3 The manufacturing method shown is used to manufacture.
[0098] Figure 2 The manufacturing method shown is equivalent to the manufacturing method of the second mode described above (manufacturing method I), and includes a first step, a second-i step, a third-i step, and a fourth step.
[0099] like Figure 2 As shown in (a), the first step is to defibrate a cellulose raw material or a chitin / chitosan raw material in a hydrophilic solvent 7 to obtain a dispersion liquid 11A of fine fibers 3 that are either cellulose nanofibers or chitin nanofibers (a dispersion liquid obtained by dispersing the fine fibers 3 in a hydrophilic solvent 7).
[0100] Step 2-i is a step of dispersing droplets 6 containing a pore-forming agent and a core material in a dispersion 11A of fine fibers 3 so that the surface of the droplets 6 is covered with the fine fibers 3. Figure 2 As shown in (b), through this step, an O / W type Pickering emulsion is obtained, in which the dispersion 11A of fine fibers 3 is used as a continuous phase and the droplets 6 containing the pore-forming agent and the core material are used as a dispersed phase.
[0101] like Figure 2 As shown in (c), step 3-i is a step of solidifying the core material inside the droplet 6 to obtain a dispersion 12 of particles 10 having a core particle 2 containing a pore former (for example, the droplet 9) inside and the surface of which is covered with fine fibers 3.
[0102] The fourth step is to Figure 2 (c) A step of recovering particles 10 from the dispersion 12 in the state shown in FIG. 1 and then removing the pore former (e.g., droplets 9) contained in the solidified core particle 2. This step can obtain composite particles (particles having fine fibers 3 coated on the surface of the core particle 2 having pores 4) 1.
[0103] That is, in the manufacturing method I, the O / W type Pickering emulsion is stabilized by adsorbing the fine fibers 3 on the interface of the droplets 6 dispersed in the hydrophilic solvent 7 and containing the pore former and the core material. Then, while maintaining the stabilized state, the core material inside the droplets 6 of the emulsion is solidified to form core particles, and the pore former (the non-polymerizable solvent contained in the droplets 6, or the hydrophilic solvent 7 absorbed by the droplets 6 under the action of the excess oil-soluble surfactant contained in the droplets 6, etc.) is removed from the core particles, thereby obtaining the composite particles 1.
[0104] When a hydrophobic non-polymerizable solvent is contained in the liquid droplets 6 , the non-polymerizable solvent precipitates as oil droplets inside the core particle 2 when the core material is solidified. Therefore, the core particle 2 having pores 4 can be obtained by removing the oil droplets.
[0105] When a large amount of oil-soluble surfactant is contained in the droplet 6 at a concentration higher than the critical micelle concentration, the hydrophilic solvent 7 is absorbed into the droplet 6, thereby playing a role as a pore former. When the core material is solidified, a core particle 2 containing the hydrophilic solvent 7 can be obtained, and by removing the hydrophilic solvent 7, a core particle 2 having pores 4 can be obtained.
[0106] Figure 3 The manufacturing method shown is equivalent to the manufacturing method of the third embodiment (manufacturing method II) described above, and includes a first step, a second-ii step, a third-i step, and a fourth step.
[0107] like Figure 3 As shown in (a), the first step is a step of defibrillating a cellulose raw material or a chitin / chitosan raw material in a hydrophilic solvent 7 to obtain a dispersion 11A of fine fibers 3 that are either cellulose nanofibers or chitin nanofibers.
[0108] Step 2-ii is a step of preparing a W / O type emulsion of hydrophilic droplets by dispersing a pore-forming agent such as a hydrophilic solvent in a core material using a stabilizer in advance, and dispersing the emulsion as hydrophobic droplets in the dispersion 11A of the fine fibers 3 so that the surface of the hydrophobic droplets is covered with the fine fibers 3. That is, in step 2-ii, a W / O / W type emulsion is obtained in which droplets composed of the W / O type emulsion are a dispersed phase and the hydrophilic solvent 7 is a continuous phase.
[0109] In step 2-ii, first, Figure 3 As shown in (b), a pore former such as a hydrophilic solvent is dispersed in a core material (any of a polymerizable monomer, a soluble polymer, and a molten polymer) 41 using a stabilizer 8, thereby preparing a W / O type emulsion 13 of droplets 9 composed of a hydrophilic pore former.
[0110] Next, if Figure 3 As shown in (c), by adding the W / O type emulsion 13 to the dispersion liquid 11A of the fine fibers 3, the droplets 6 containing the W / O type emulsion are dispersed in the W / O type emulsion 13, so that the surfaces of the droplets 6 containing the W / O type emulsion are covered with the fine fibers 3, thereby preparing the W / O / W type emulsion 14. Figure 3 (d) is an enlarged view of droplet 6.
[0111] like Figure 3 As shown in (e), step 3-i is a step of solidifying the core material inside the droplet 6 to obtain a dispersion 12 of particles 10 in which the surface of the core particle 2 is covered with fine fibers 3. The core particle 2 contains droplets 9 composed of a pore-forming agent.
[0112] The fourth step is as follows: Figure 3 (e) The particles 10 are recovered from the dispersion 12 in the state shown, and the pore-forming agent (hydrophilic solvent dispersed in the form of droplets 9 in the droplets 6) contained in the core particle 2 is removed to generate pores 4 in the core particle 2. Through this process, composite particles (particles in which the surface of the core particle 2 having pores 4 is covered with fine fibers 3) 1 can be obtained.
[0113] That is, in manufacturing method II, the W / O / W type Pickering emulsion is stabilized by adsorbing the fine fibers 3 on the interface of "droplets 6 composed of liquid formed by dispersing droplets (droplets of hydrophilic pore former) 9 in the core material 41" dispersed in the hydrophilic solvent 7. Then, while maintaining this stabilized state, the core material 41 contained in the droplets 6 in the emulsion is solidified. Next, by filtering or the like, the free fine fibers 3 and the continuous phase of the hydrophilic solvent 7 are separated from the dispersion 12 of the particles 10 in which the surface of the core particle 2 is coated with the fine fibers 3, and then the hydrophilic solvent (pore former) dispersed in the form of droplets 9 inside the core particle 2 is removed, thereby obtaining a composite particle 1.
[0114] The term "inseparable" as used herein means that the core particles and the fine fibers are not separated and the core particles are kept covered with the fine fibers even after repeated operations such as centrifuging a dispersion containing particles or composite particles covered with fine fibers and removing the supernatant, further adding a solvent for redispersion, thereby recovering and washing the particles or composite particles covered with fine fibers, or washing with a solvent by filtering and washing using a membrane filter. The coating state can be confirmed by observing the surface of the composite particles using a scanning electron microscope.
[0115] In the above-mentioned manufacturing method, when obtaining particles or composite particles coated with microfibers, the bonding mechanism of the microfibers and the core particles is still uncertain, but it can be inferred as follows. First, the particles or composite particles coated with microfibers are made using an O / W type emulsion that is stabilized by the microfibers as a template. Then, when the microfibers are in contact with the core material inside the droplets of the emulsion, the core material is solidified to become a core particle. Therefore, it can be inferred that the microfibers are physically fixed on the surface of the core particles, and finally the core particles and the microfibers reach an inseparable state.
[0116] Although not particularly limited, when the particles or composite particles coated with fine fibers are prepared using the O / W type emulsion stabilized by the fine fibers as a template, since the O / W type emulsion becomes stable, true spherical particles or composite particles coated with fine fibers derived from the O / W type emulsion can be obtained. Specifically, it is preferred that a coating layer composed of fine fibers is formed on the surface of the true spherical core particle with a relatively uniform thickness.
[0117] In the composite particles of this embodiment, since the surface of the core particle is covered with high-strength fine fibers, the spherical shape can be maintained even if the porosity (pore ratio or hollow ratio) is high, thereby achieving high light diffusion, smooth feel, excellent moisturizing properties and dispersibility.
[0118] The particle size of the composite particles can be confirmed by optical microscopic observation. For example, the average particle size can be calculated by measuring the diameters of 100 randomly selected composite particles and averaging the particle diameters. The average particle size is not particularly limited, but is preferably 0.1 μm to 1000 μm.
[0119] From the viewpoint of dispersion stability, the fine fibers are preferably formed on the surface of the core particle in the form of a coating layer. The coating layer preferably covers the entire surface of the core particle, but does not necessarily have to cover the entire surface.
[0120] The thickness of the coating layer composed of fine fibers is not particularly limited, but is preferably 3 nm to 1000 nm.
[0121] The average thickness of the coating layer can be calculated by the following method: the material obtained by fixing the composite particles by embedding resin is cut using a microtome, and then observed under a scanning electron microscope. The thickness of the coating layer in the cross-sectional image of the composite particles in the image is measured at 100 random points on the image, and the average value is taken.
[0122] In addition, it is preferred that the composite particles are uniformly coated with a coating layer having a relatively uniform thickness. When the coating layer has a uniform thickness, dispersion stability is high. Specifically, the coefficient of variation of the value of the thickness of the coating layer is preferably 0.5 or less, more preferably 0.4 or less.
[0123] The fine fibers constituting the composite particles of the present embodiment are cellulose nanofibers and / or chitin nanofibers.
[0124] Cellulose nanofibers are fibers composed of cellulose or cellulose derivatives, with a number average minor axis diameter of 1 nm to 1000 nm. Chitin nanofibers are fibers composed of chitin and / or chitosan, or chitosan and / or chitosan derivatives, with a number average minor axis diameter of 1 nm to 1000 nm.
[0125] Cellulose nanofibers (CNF) are microfibers that are obtained by crushing cellulose raw materials obtained from wood and the like into extremely fine fibers. They are safe and biodegradable.
[0126] Chitosan nanofibers (chitosan NF) are microfibers obtained by crushing chitosan and / or chitosan (hereinafter referred to as chitosan / chitosan) raw materials extracted from crab shells, etc. into ultrafine fibers. They are safe, biodegradable, and antibacterial. In particular, chitosan nanofibers produced by the method of patent document 6 are composed of chitosan and / or chitosan that have not been chemically modified, and do not need to confirm safety, so they are more easily applied in (especially) food, medical treatment, medicine, personal care, etc., which are used by ingestion into the body.
[0127] It should be noted that the crystal surface of the microfiber preferably has an ionic functional group. By having an ionic functional group, the aggregation of the composite particles can be suppressed, thereby obtaining a personal care product with good skin affinity. In addition, the functional material can be loaded on the surface of the composite particles by utilizing the ionic functional group. For example, if it is a microfiber with an anionic functional group, a cationic functional material can be loaded, and if it is a microfiber with a cationic functional group, an anionic functional material can be easily loaded.
[0128] The type of ionic functional group is not particularly limited, but anionic functional groups are preferred. By having anionic functional groups, for example, in the case of loading metal particles, metal ions coordinate with anionic functional groups of fine fibers and are reduced and precipitated, thereby effectively loading metal particles. In addition, the fine fibers have the function of a dispersion stabilizer, so that the shape and particle size of the generated metal particles can be controlled. In addition, the metal particles can be prevented from detaching from the fine fibers in the composite particles.
[0129] In addition, usually, when metal particles are dried, they aggregate and thus cannot exhibit the optical properties generated by the localized surface plasmon resonance (LSPR) described later, but when the composite particles are made into a dry powder, the metal particles do not aggregate and thus can exhibit optical properties even in a dry powder. If the metal particles are silver particles, antibacterial properties can be imparted.
[0130] The anionic functional group is not particularly limited, and examples thereof include a carboxyl group, a phosphoric acid group, and a sulfonic acid group. Among them, a carboxyl group and a phosphoric acid group are preferred, and a carboxyl group is preferred because it can be selectively introduced easily onto the surface of cellulose crystals.
[0131] The content of the ionic functional group is preferably 0.1 mmol to 5.0 mmol per 1 g of the fine fiber raw material and / or fine fibers. If it is less than 0.1 mmol, the dispersion stability of the composite particles 1 may be deteriorated, while if it exceeds 5.0 mmol, it may be difficult to stably produce the composite particles 1.
[0132] In addition, the microfibers preferably have a fiber shape derived from a microfibril structure. Specifically, it is preferred that the microfibers are fibrous, the number average minor axis diameter is 1 nm or more and 1000 nm or less, the number average major axis diameter is 50 nm or more, and the number average major axis diameter is 5 times or more of the number average minor axis diameter. In addition, the crystallinity of the microfibers is preferably 50% or more. The crystal structure of the cellulose nanofibers is preferably cellulose type I. The crystal structure of the chitin nanofibers can be any one of α-chitin and β-chitin, preferably α-chitin.
[0133] like Figure 1A to Figure 1C As shown, the core particle 2 constituting the composite particle 1 of this embodiment has pores 4. The shape, size, and number of the pores 4 can be controlled by the type and amount of the pore-forming agent used. In addition, the core particle 2 of the composite particle 1 can be a porous particle or a hollow particle.
[0134] Here, porous particles refer to particles having a large number of pores. When the core particles constituting the composite particles are porous particles, the core particles have a large specific surface area, so when the composite particles are used as personal care products, they can absorb skin oil to give a refreshing touch.
[0135] When the core particle of the composite particle is a porous particle, the pore size (diameter of the pores) is not particularly limited, but is preferably 2 nm or more and 30 μm or less. In order to obtain a porous composite particle 1 having oil absorption, the pore size is preferably 2 nm or more and 50 nm or less. When the pore size is less than 2 nm, sufficient water absorption or oil absorption cannot be obtained. In addition, when the pore size exceeds 50 nm, it is difficult to retain functional components.
[0136] The specific surface area of the composite particles is preferably 2 m 2 / g above 1000m 2 / g or less, more preferably 3m 2 / g above 400m 2 / g or less, more preferably 5m 2 / g above 300m 2 / g or less. When the specific surface area is less than 2m 2 / g, it cannot fully exert its water and oil absorption; when it exceeds 1000m 2 / g, the spherical shape cannot be maintained, and a smooth feel cannot be obtained.
[0137] The pore size and specific surface area can be measured by a gas adsorption method. For example, it can be measured by the BET method (nitrogen adsorption method) of JIS Z 8830. The BET nitrogen adsorption isotherm of the dry powder of the composite particles 1 is measured using an automatic specific surface area / pore distribution measuring device, and the specific surface area is calculated using the BET multi-point method based on the nitrogen adsorption amount. The pore size (average pore size) and pore volume are calculated by the BJH method.
[0138] The composite particles of this embodiment preferably have an oil absorption of 30 ml / 100 g or more and 800 ml / 100 g or less, more preferably 50 ml / 100 g or more and 500 ml / 100 g or less, and further preferably 70 ml / 100 g or more and 300 ml / 100 g or less. When the oil absorption is less than 30 ml / 100 g, the lasting effect of the composite particles may be insufficient when used in powdery cosmetics such as powder foundation. On the other hand, when the oil absorption exceeds 800 ml / 100 g, other components may be absorbed.
[0139] The water absorption of the composite particles of this embodiment is preferably 30 ml / 100 g or more and 800 ml / 100 g or less, more preferably 50 ml / 100 g or more and 500 ml / 100 g or less, and further preferably 70 ml / 100 g or more and 300 ml / 100 g or less. When the water absorption is less than 30 ml / 100 g, it is difficult to absorb sweat when used for foundation, etc. When the water absorption exceeds 800 ml / 100 g, it absorbs surrounding moisture, and the moisturizing effect is reduced.
[0140] The oil absorption can be evaluated by the method of JIS K 5101-13-1. The powder of composite particles 1 is placed on a measuring plate, and refined linseed oil is gradually added by dropping 4 or 5 drops from a burette each time. The refined linseed oil is kneaded into the sample using a palette knife each time the addition is made. This operation is repeated, and the addition is continued until a mass of refined linseed oil and the sample can be formed. Afterwards, the operation is repeated by dropping drop by drop and kneading completely. The end point is the hardness of the slurry becoming smooth. In the above method, pure water can be used instead of linseed oil to evaluate the water absorption.
[0141] Hollow particles are particles with a closed cavity inside. When the core particles constituting the composite particles are hollow particles, high soft focus properties can be achieved regardless of the refractive index of the surrounding particles. Even if liquid foundation is dispersed in the oil phase, the oil component does not penetrate into the interior, thereby maintaining high soft focus properties.
[0142] The number of pores (voids) in the hollow particles is not particularly limited, and the particles may be single hollow particles with one pore or multiple hollow particles with a plurality of pores. The porosity of the composite particles as hollow particles is not particularly limited, but the porosity is preferably 10% to 90%, more preferably 20% to 80%, and further preferably 40% to 60%. When the porosity is less than 10%, it is difficult to achieve sufficient soft focus. On the other hand, when the porosity exceeds 90%, it is difficult to obtain spherical composite particles 1.
[0143] The porosity can be calculated by observing the composite particles using a transmission electron microscope. The dried powder of the composite particles 1 is observed using a transmission electron microscope, and the average particle size and average inner diameter of more than 100 particles are calculated. According to the formula "(average inner diameter) 3 / (average particle size) 3 ×100”, the average porosity can be calculated.
[0144] When a highly hydrophobic non-polymerizable solvent is used as a pore-forming agent, the non-polymerizable solvent gathers in the center during the solidification of the core material, so that hollow composite particles are easily obtained. On the other hand, when a highly hydrophilic non-polymerizable solvent is used as a pore-forming agent, porous composite particles are easily obtained.
[0145] The composite particles of this embodiment are preferably spherical, particularly preferably true spherical. When they are true spherical, a smooth feel can be obtained when used as cosmetics such as foundation. The index of true sphericity can be evaluated based on the circularity measured by an image analysis type particle size distribution meter. The circularity is preferably greater than 0.6, more preferably greater than 0.7, and further preferably greater than 0.9. When the circularity is less than 0.6, it is difficult to obtain a smooth feel. The average circularity can be calculated as the average value of the circularities of more than 1000 particles measured using an image analysis type particle size distribution meter. It should be noted that when the area of the composite particles on the image is set to S and the perimeter is set to L, the circularity can be expressed by the formula "circularity = 4πS / L 2 " to calculate.
[0146] The composite particles of the present embodiment have pores and therefore exhibit excellent light diffusibility. The light diffusibility can be evaluated by the light diffusion index measured by the following method.
[0147] The glass plate containing the dry powder was placed on a spectral variable angular difference meter GC5000 manufactured by Nippon Denshoku Industries, and the spectral reflectance R1 when receiving incident light at an angle of -45° at a 0° angle and the spectral reflectance R2 when receiving incident light at an angle of -45° at a 45° angle were measured at wavelengths of 400nm to 700nm. Based on the measurement results, the ratio of R1 to R2 at a wavelength of 600nm was calculated as the light diffusion index.
[0148] The light diffusion index of the composite particles is preferably 0.6 or more, more preferably 0.7 or more, and further preferably 0.9 or more. When the light diffusion index is less than 0.6, the pore correction effect and the soft focus effect when used for foundation etc. may be insufficient.
[0149] The core particles constituting the composite particles of the present embodiment preferably contain an organic compound that is solid at 25° C. For example, paraffin, polymers, oils and fats, and the like.
[0150] In addition, the core particles are preferably formed of a material containing one or more polymers. As the polymer, a known polymer may be used, or a polymer obtained by polymerizing a polymerizable monomer by a known method may be used.
[0151] Examples of the polymer include acrylic polymers, epoxy polymers, polyester polymers, amino polymers, silicone polymers, fluorine polymers, and urethane-isocyanate polymers.
[0152] Although not particularly limited, the polymer is preferably a biodegradable polymer. Biodegradability refers to a polymer that can be degraded and disappear in the earth environment such as soil and seawater, or / and a polymer that can be degraded and disappear in a living body. Generally speaking, polymers are degraded in soil or seawater by enzymes possessed by microorganisms, while enzymes are not required in the body, but are degraded by physicochemical hydrolysis. Degradation of a polymer refers to the molecular weight of the polymer being reduced or becoming water-soluble so that the form disappears. Degradation of a polymer is not particularly limited, and occurs, for example, by hydrolysis of the main chain, side chain, crosslinking point, or oxidative degradation of the main chain.
[0153] Biodegradable polymers include natural polymers derived from nature or synthetic polymers.
[0154] Examples of natural polymers include polysaccharides produced by plants (cellulose, starch, alginic acid, etc.), polysaccharides produced by animals (chitin, chitosan, hyaluronic acid, etc.), proteins (collagen, gelatin, albumin, etc.), polyesters produced by microorganisms (poly (3-hydroxyalkanoate)), polysaccharides (hyaluronic acid, etc.), etc.
[0155] Examples of the synthetic polymer include aliphatic polyesters, polyols, and polycarbonates.
[0156] Examples of aliphatic polyesters include glycol / dicarboxylic acid polycondensation polyesters (polyethylene succinate, polybutylene succinate, etc.), polylactic acids (polyglycolic acid, polylactic acid, etc.), polylactones (β-caprolactone, ε-caprolactone, etc.), and others (polybutylene terephthalate, adipate, etc.).
[0157] Examples of the polyol include polyvinyl alcohol and the like.
[0158] Examples of the polycarbonate include polyester carbonate and the like.
[0159] In addition, polyanhydrides, polycyanoacrylates, polyorthoesters, polyphosphazenes, etc. are also biodegradable synthetic polymers.
[0160] The material forming the core particle may also contain other ingredients besides the polymer.
[0161] Examples of other ingredients include colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, deodorant ingredients, fragrances, flavors, anti-dandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials such as fats and waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), etc.
[0162] The other components may be in any form of solid, gas, or liquid. The content of the other components in the composite particles is not particularly limited, but is preferably within a range that allows the composite particles to stably maintain their form. The content of the other components is preferably 0.001 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the composite particles.
[0163] The composite particles of the present embodiment preferably contain functional components in the pores. By containing the functional components, their functions can be exerted. As methods for containing functional components, there can be listed: a method of impregnating the functional components in the composite particles, or a method of encapsulating the functional components during the production process of the composite particles.
[0164] Functional ingredients are substances that affect and exert functions on organisms such as animals, plants, and fungi. Although not particularly limited, examples thereof include: mildew inhibitors, fragrances, fertilizers (biofertilizers, chemical fertilizers, organic fertilizers, etc.), pH adjusters, pesticides (insecticides, fungicides, herbicides, etc.), plant activators, plant life extenders, repellents for pests and animals, soil penetrants, nutrients (minerals, etc.), plant hormones, inorganic particles (titanium oxide, silicon dioxide, clay, etc.), antibacterial ingredients, etc.
[0165] The composite particles 1 of this embodiment preferably contain functional ingredients that function as personal care products in the pores 4. Examples of the functional ingredients include: oily raw materials headed by oils and waxes, colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, exfoliants, sebum inhibitors, blood circulation promoting ingredients, whitening ingredients, anti-aging ingredients, anti-inflammatory ingredients, cooling ingredients, warming ingredients, deodorizing ingredients, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, aromatics, fragrances, anti-dandruff active substances, skin softeners, insect repellents, preservatives, vitamins, amino acids, hormones, natural extracts, etc. Among them, it is preferred to contain at least any one of ultraviolet absorbers, ultraviolet scatterers, fragrances, deodorizing ingredients, exfoliants, anti-aging ingredients, whitening ingredients, anti-inflammatory ingredients, and colorants.
[0166] Examples of the ultraviolet absorber include trimethylcyclohexyl salicylate, 2-ethylhexyl 2-cyano-3,3-diphenylprop-2-enoate, di-p-methoxycinnamate-mono-2-ethylhexanoin, p-aminobenzoic acid and its esters, and 4-tert-butyl-4′-methoxydibenzoylmethane.
[0167] Examples of the ultraviolet scattering agent include titanium oxide and zinc oxide.
[0168] As fragrances, there are natural fragrances extracted from animals and plants, synthetic fragrances synthesized by chemical synthesis, and mixed fragrances obtained by mixing multiple fragrances. Among them, as natural fragrances, for example, there can be listed: flowers such as jasmine, rose, carnation, clove, cyclamen, lily of the valley, violet, lavender, and olive; citrus such as orange, lemon, and lime; spices such as cinnamon and nutmeg; wood essential oils such as cypress essential oil, cypress essential oil, and cedar essential oil.
[0169] Examples of synthetic fragrances include hydrocarbons such as limonene, pinene, and camphene; alcohols such as linalool, geraniol, menthol, citronellol, and benzyl alcohol; aldehydes such as citral, citronellal, nonadienal, benzaldehyde, and cinnamaldehyde; ketones such as acetophenone, methylacetophenone, methylnonylketone, irone, and menthone; phenols such as methyl anisole and eugenol; lactones such as decalactone, nonalactone, and undecalactone; esters such as linalyl acetate, geranyl acetate, benzyl acetate, terpinyl acetate, citronellyl acetate, methyl benzoate, ethyl benzoate, isoamyl benzoate, benzyl benzoate, methyl cinnamate, and ethyl cinnamate; and the like.
[0170] Examples of deodorizing ingredients include diphenols such as catechol, 4-methylcatechol, 5-methylcatechol, resorcinol, 2-methylresorcinol, 5-methylresorcinol, and hydroquinone; biphenyldiols such as 4,4'-biphenyldiol and 3,4'-biphenyldiol; catechins such as catechin, epicatechin, epigallocatechin, and epicatechin gallate; polyphenols derived from plants such as catechol derivatives such as dopa, dopamine, chlorogenic acid, caffeic acid, p-coumaric acid, and tyrosine, or polyphenols extracted from plants; deodorizing ingredients derived from coffee, apples, grapes, tea (green tea, roasted tea, black tea, oolong tea, mate tea, etc.), persimmon, soybean, cocoa, rosemary, aloe, and the like.
[0171] Examples of the peeling agent include glycolic acid, salicylic acid, and lactic acid.
[0172] Examples of the anti-aging ingredients include retinyl palmitate, fullerene, acetyl hexapeptide-8, palmitoyl pentapeptide-4, ubiquinone, and platinum.
[0173] Examples of the whitening ingredient include magnesium ascorbyl phosphate, arbutin, placenta extract, and chamomile extract.
[0174] Examples of the anti-inflammatory ingredient include licorice root extract, dipotassium glycyrrhizinate, glycyrrhizic acid stearate, allantoin, and coix seed extract.
[0175] Examples of the colorant include organic synthetic pigments (dyes, lakes, organic pigments), natural pigments, inorganic pigments, metal fine particles, polymer powders, etc. Among them, organic synthetic pigments, natural pigments, inorganic pigments, and metal fine particles are preferred.
[0176] In addition, in the composite particles 1 of the present embodiment, when the functional material is loaded on the fine fibers coated on the surface of the core particles, the dispersion stability of the functional material is improved, so that its function can be effectively exerted. The functional material is "loaded" on the fine fibers, which means that the functional material is physically or chemically, reversibly or irreversibly bound or adsorbed on the fine fibers. The functional material can be loaded by a known method.
[0177] It is preferred that the functional material and the fine fiber are in an "inseparable" state. The "inseparable" state between the fine fiber and the functional material means that the fine fiber and the functional material are not separated even after repeated operations of recovering / washing the composite particles by centrifuging the dispersion containing the composite particles and removing the supernatant, further adding a solvent for redispersion, or repeatedly washing with a solvent by filtration washing using a membrane filter.
[0178] Functional materials are materials that play their functions in personal care products, and known functional materials can be used. As functional materials, for example, oily raw materials headed by grease / wax, colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, exfoliants, sebum inhibitors, blood circulation promoting ingredients, whitening ingredients, anti-aging ingredients, anti-inflammatory ingredients, cold-sensing ingredients, warm-sensing ingredients, deodorizing ingredients, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, aromatics, fragrances, anti-dandruff active substances, skin softeners, insect repellents, preservatives, vitamins, amino acids, hormones, natural extracts, etc. Among them, it is preferred to contain at least any one of ultraviolet absorbers, ultraviolet scatterers, fragrances, deodorizing ingredients, and colorants.
[0179] The method of loading the functional material on the microfiber is not particularly limited, and for example, composite particles loaded with the functional material can be prepared by the following method. First, after loading the functional material on the microfiber, the obtained microfiber loaded with the functional material is used to prepare an O / W type Pickering emulsion having droplets containing a non-polymerizable solvent or surfactant and a core material. Next, the core material inside the droplets of the emulsion is solidified, filtered and washed, and the pore-forming agent is removed.
[0180] Alternatively, an O / W type Pickering emulsion having droplets containing a non-polymerizable solvent or surfactant and a core material is prepared using fine fibers, and the core material inside the droplets of the emulsion is solidified, filtered and washed to remove the pore-forming agent, thereby preparing composite particles. Subsequently, composite particles loaded with functional materials can be prepared by loading functional materials on the fine fibers on the surface of the composite particles.
[0181] The method of supporting the functional material on the fine fibers is not particularly limited. For example, a commercially available or pre-made functional material may be added and mixed into a dispersion of the fine fibers or composite particles to allow the functional material to adhere.
[0182] A method of preparing the functional material in a dispersion of fine fibers or composite particles is preferred. By preparing the functional material in a dispersion of fine fibers or composite particles, the functional material can be stably supported on the fine fibers and aggregation of the functional material can be suppressed.
[0183] <About the method for producing composite particles>
[0184] As described above, the composite particles 1 of the embodiment can be Figure 2 and Figure 3 The manufacturing method is as shown in FIG. 1 (manufacturing method I and manufacturing method II).
[0185] The composite particles 1 obtained by the manufacturing method I and the manufacturing method II are obtained in the form of dry solid matter, and can be made into a dispersion by redispersion. The particles 10 or composite particles 1 coated with fine fibers can be recovered by filtration or centrifugal separation, etc., and further heat-dried or vacuum-dried in an oven, etc., to obtain a dry solid matter. At this time, the dry solid matter of the composite particles 1 obtained is not in the form of a film or an aggregate, but is obtained in the form of a fine and smooth powder.
[0186] The reason for this is not yet clear, but it is known that, generally, when the solvent is removed from the dispersion of the fine fibers 3, the fine fibers 3 are strongly aggregated and form a film. On the other hand, in the case of a dispersion containing particles 10 or composite particles 1 coated with fine fibers, since spherical particles 10 or composite particles 1 having the fine fibers 3 fixed on the surface are obtained, it is believed that even if the hydrophilic solvent 7 is removed, the fine fibers 3 are not aggregated, and the particles 10 or composite particles 1 coated with fine fibers are in contact with each other only in a point-to-point manner, so that the dry solid material is obtained in the form of a fine powder.
[0187] The particles 10 or composite particles 1 coated with fine fibers do not aggregate with each other, so in powdered cosmetics such as foundation, smooth and skin-friendly cosmetics can be obtained. In addition, porous or hollow particles can obtain a lighter texture than solid particles, and have high light diffusivity, so they are excellent in soft focus. In addition, functional ingredients can be contained in the porous or hollow particles, and by loading the functional materials on the fine fibers 3, the aggregation of the functional materials can be suppressed, so that uniform powdered cosmetics can be obtained.
[0188] It should be noted that the dry powder of the composite particles 1 is a dry solid substance that contains almost no solvent such as the hydrophilic solvent 7 and is further redispersible in the solvent. Specifically, the solid content can be set to 80% or more, further to 90% or more, and further to 95% or more. Since the solvent can be almost removed, a preferred effect can be obtained from the viewpoints of reducing transportation costs, preventing decay, increasing the addition rate, and improving the kneading efficiency with the resin.
[0189] Since the fine fibers 3 on the surface of the composite particles 1 have high hydrophilicity, the dry powder of the composite particles 1 has the characteristic of absorbing moisture such as sweat or exhibiting high moisture retention.
[0190] Furthermore, the composite particles 1 obtained in the form of dry powder can be easily redispersed in a solvent, and even after redispersion, dispersion stability derived from the fine fibers 3 bonded to the surface of the composite particles 1 is exhibited. Therefore, the composite particles 1 can be included in beauty serums, emulsions, creams, and the like.
[0191] Hereinafter, each step will be described in detail.
[0192] As described above, the manufacturing method I includes the first step, the second-i step, the third-i step, and the fourth step, and the manufacturing method II includes the first step, the second-ii step, the third-i step, and the fourth step.
[0193] (1st step)
[0194] The first step is a step of defibrillating a fine fiber raw material in a solvent to obtain a fine fiber dispersion. The fine fiber raw material refers to a raw material of cellulose nanofibers and / or chitin nanofibers, that is, a cellulose raw material and a chitin / chitosan raw material.
[0195] First, various fine fiber raw materials are dispersed in a solvent to form a suspension. The concentration of the fine fiber raw material in the suspension is preferably 0.1% or more and less than 10%. When it is less than 0.1%, productivity is impaired due to excessive solvent, which is not preferred. When it is set to 10% or more, the viscosity of the suspension increases rapidly as the fine fiber raw material is defibrated, making it difficult to perform uniform defibration treatment, which is not preferred.
[0196] As a solvent for preparing the suspension, a hydrophilic solvent is preferably used. The hydrophilic solvent is not particularly limited, but is preferably water; alcohols such as methanol, ethanol, isopropanol; cyclic ethers such as tetrahydrofuran; or a mixture thereof. Preferably, it contains 50% or more of water. When the proportion of water in the suspension is less than 50%, the dispersion of the fine fibers is hindered in the step of defibrillating the fine fiber raw material in the solvent to obtain a fine fiber dispersion liquid described later. In addition, as a solvent contained other than water, the above-mentioned hydrophilic solvent is preferred.
[0197] If necessary, the pH of the suspension may be adjusted to improve the dispersibility of the fine fiber raw material and the generated fine fibers. Examples of the alkaline aqueous solution used for pH adjustment include organic bases such as sodium hydroxide aqueous solution, lithium hydroxide aqueous solution, potassium hydroxide aqueous solution, ammonia aqueous solution, tetramethylammonium hydroxide aqueous solution, tetraethylammonium hydroxide aqueous solution, tetrabutylammonium hydroxide aqueous solution, and benzyltrimethylammonium hydroxide aqueous solution. In terms of cost, sodium hydroxide aqueous solution is preferred.
[0198] Next, the suspension is subjected to a physical defibration treatment to micronize the fine fiber raw material. There is no particular limitation on the physical defibration treatment method, and examples thereof include: high pressure homogenizer, ultra-high pressure homogenizer, ball mill, roller mill, shredder, planetary mill, jet mill, grinder, grinder, juicer mixer, homogenizing mixer, ultrasonic homogenizer, nano homogenizer, underwater collision and other mechanical treatments. By performing such a physical defibration treatment, the cellulose in the suspension of the cellulose raw material using the hydrophilic solvent 7 as the solvent can be micronized, so that a dispersion of micronized cellulose with at least one side of its structure reaching the nanometer level can be obtained. In addition, according to the time and number of physical defibration treatments at this time, the number average short axis diameter and the number average long axis diameter of the obtained fine fibers 3 can be adjusted.
[0199] As described above, a dispersion of microfibers (microfiber dispersion liquid) having micronized microfibers of which at least one side has reached the nanometer level is obtained. The obtained dispersion can be used directly as a stabilizer for the O / W type emulsion described later, or after dilution, concentration, etc., it can be used as a stabilizer for the O / W type emulsion described later.
[0200] In addition, within the scope of not impairing the effect of the present invention, as required, the dispersion of fine fibers may also contain other components other than cellulose and components for pH adjustment. As the above-mentioned other components, there is no particular limitation, and they can be appropriately selected from known additives according to the purpose of the composite particles 1. Specifically, they can include: organic metal compounds such as alkoxysilane or their hydrolyzates, inorganic layered compounds, inorganic needle-shaped minerals, defoamers, inorganic particles, organic particles, lubricants, antioxidants, antistatic agents, ultraviolet absorbers, stabilizers, magnetic materials, orientation promoters, plasticizers, crosslinking agents, drugs, pesticides, fragrances, adhesives, enzymes, colorants, deodorants, metals, metal oxides, inorganic oxides, preservatives, antibacterial agents, natural extracts, surfactants, etc.
[0201] Generally, since the fine fibers have a fiber shape derived from a microfibril structure, the fine fibers used in the manufacturing method of this embodiment preferably have a fiber shape within the range shown below. That is, the shape of the fine fibers is preferably fibrous. In addition, for the fibrous fine fibers, the number average short axis diameter in the short axis diameter can be 1 nm or more and 1000 nm or less, preferably 2 nm or more and 500 nm or less.
[0202] Here, when the number average minor axis diameter is less than 1 nm, a highly crystalline rigid fine fiber structure cannot be obtained, making it difficult to stabilize the emulsion and to form composite particles by implementing a polymerization reaction using the emulsion as a template or solidification of the polymer. On the other hand, when it exceeds 1000 nm, the size becomes too large during the process of stabilizing the emulsion, making it difficult to control the size and shape of the resulting composite particles.
[0203] The number average major axis diameter is not particularly limited, but may be preferably 5 times or more the number average minor axis diameter. When the number average major axis diameter is less than 5 times the number average minor axis diameter, it may be difficult to fully control the size and shape of the composite particles, which is not preferred.
[0204] It should be noted that the short axis diameter (minimum diameter) of 100 fibers was measured by transmission electron microscopy and atomic force microscopy, and the average value was calculated as the number average short axis diameter of the fine fibers. On the other hand, the long axis diameter (maximum diameter) of 100 fibers was measured by transmission electron microscopy and atomic force microscopy, and the average value was calculated as the number average long axis diameter of the fine fibers.
[0205] The type and crystal structure of cellulose that can be used as the cellulose raw material are not particularly limited. Specifically, as a raw material composed of cellulose type I crystals, for example, in addition to wood-based natural cellulose, non-wood-based natural cellulose such as cotton linter, bamboo, hemp, bagasse, kenaf, bacterial cellulose, sea squirt cellulose, and valence cellulose can also be used. In addition, regenerated cellulose represented by rayon fiber and cuprammonium fiber composed of cellulose type II crystals can also be used.
[0206] From the perspective of the availability of materials, it is preferred to use wood-based natural cellulose as a raw material. As wood-based natural cellulose, there is no particular limitation, and cellulose commonly used to manufacture cellulose nanofibers such as softwood pulp, hardwood pulp, and recycled paper pulp can be used. From the perspective of the ease of refining and micronization, softwood pulp is preferred.
[0207] Chitosan / chitin raw materials are polysaccharides with a linear structure used to support and protect the body of animals, such as crabs, shrimps and other crustaceans; insects, spiders and other arthropods; squid tendons, which have crystallinity (there are parts with regular molecular arrangement) and are partially bound to proteins. Chitosan is a polysaccharide with N-acetylglucosamine as the main constituent sugar.
[0208] When chitin and / or chitosan raw materials are separated / purified, purified chitin consisting of 100% N-acetylglucosamine is rarely obtained, but chitin and / or chitosan containing glucosamine as a component is obtained. For example, a raw material obtained by crushing the shell of king crab in a dry state to about 5 mm and a raw material obtained by crushing the soft shell of squid in a wet state to about 1 cm can be used as chitin and / or chitosan raw materials. The chitin / chitosan raw material is preferably purified in advance.
[0209] In addition, the microfiber raw material is preferably chemically modified. More specifically, it is preferred to introduce ionic functional groups on the crystal surface of the microfiber raw material. This is because, by introducing ionic functional groups on the crystal surface of the microfiber raw material, the solvent can easily penetrate between the crystals of the microfiber raw material due to the osmotic pressure effect, thereby easily miniaturizing the microfiber raw material. In addition, by having ionic functional groups, the droplet stabilization effect of the microfiber is improved. In addition, by adsorbing functional materials via ionic functional groups, functional materials can be loaded.
[0210] The type of ionic functional groups introduced into the crystal surface of the microfiber raw material is not particularly limited. For example, by having anionic functional groups, the microfibers can carry cationic functional materials. In addition, by coordinating metal ions with microfibers having anionic functional groups and reducing and precipitating them, metal particles as functional materials can be loaded. The type and introduction method of the anionic functional group are not particularly limited, but carboxyl groups or phosphate groups are preferred. When the microfiber raw material is cellulose, carboxyl groups are preferred because they are easy to selectively introduce into the surface of cellulose crystals.
[0211] The method for introducing carboxyl groups into the crystal surface of cellulose is not particularly limited. For example, carboxyl methylation can be carried out by reacting cellulose with monochloroacetic acid or sodium monochloroacetate in a high concentration alkaline aqueous solution. In addition, carboxyl groups can also be introduced by directly reacting carboxylic anhydride compounds such as maleic acid or phthalic acid vaporized in an autoclave with cellulose.
[0212] In addition, a method using a co-oxidant in the presence of an N-oxyl compound headed by TEMPO under relatively mild conditions in an aqueous system can also be used, wherein the N-oxyl compound headed by TEMPO has high selectivity for oxidation of primary carbons of alcohols while maintaining the structure as much as possible. For the selectivity of the carboxyl group introduction site and the reduction of environmental load, it is more preferable to use an N-oxyl compound for oxidation.
[0213] Here, as N-oxyl compounds, TEMPO (2,2,6,6-tetramethylpiperidinyl-1-oxyl radical), 2,2,6,6-tetramethyl-4-hydroxypiperidin-1-oxyl, 4-methoxy-2,2,6,6-tetramethylpiperidin-N-oxyl, 4-ethoxy-2,2,6,6-tetramethylpiperidin-N-oxyl, 4-acetylamino-2,2,6,6-tetramethylpiperidin-N-oxyl, etc. can be listed. Among these, TEMPO with high reactivity is preferred. The amount of N-oxyl compound used can be the amount used as a colorant, and is not particularly limited. Generally, it is 0.01% by mass or more and 5.0% by mass or less relative to the solid content of the wood-based natural cellulose subjected to oxidation treatment.
[0214] As a method for oxidation using an N-oxyl compound, for example, there can be cited a method in which wood-based natural cellulose is dispersed in water and subjected to oxidation treatment in the presence of an N-oxyl compound. In this case, it is preferred to use a co-oxidant together with the N-oxyl compound. In this case, in the reaction system, the N-oxyl compound is sequentially oxidized by the co-oxidant to produce an oxoammonium salt, and the cellulose is oxidized by the above-mentioned oxoammonium salt. According to this oxidation treatment, the oxidation reaction can be smoothly carried out even under mild conditions, and the introduction efficiency of the carboxyl group is improved. When the oxidation treatment is carried out under mild conditions, the crystal structure of the cellulose is easily maintained.
[0215] As the pro-oxidant, for example, any oxidant capable of promoting oxidation reaction, such as halogen, hypohalous acid, halogenous acid, perhalogen acid or their salts, halogen oxides, nitrogen oxides, peroxides, etc., can be used. In view of easy availability and reactivity, sodium hypochlorite is preferred. The amount of the above-mentioned pro-oxidant used is not particularly limited, as long as it is an amount capable of promoting oxidation reaction. Generally, it is about 1 to 200 mass % relative to the solid content of the wood-based natural cellulose to be oxidized.
[0216] In addition, together with the N-oxyl compound and the pro-oxidant, at least one compound selected from the group consisting of bromide and iodide can be further used. Thus, the oxidation reaction can be smoothly carried out and the efficiency of the introduction of the carboxyl group can be improved. As such a compound, sodium bromide or lithium bromide is preferred, and sodium bromide is more preferred from the perspective of cost and stability. The amount of the compound used is not particularly limited, as long as it is an amount that can promote the oxidation reaction. Generally, it is about 1 to 50% by mass relative to the solid content of the wood-based natural cellulose subjected to oxidation treatment.
[0217] The reaction temperature of the oxidation reaction is preferably 4°C to 80°C, more preferably 10°C to 70°C. When the reaction temperature of the oxidation reaction is lower than 4°C, the reactivity of the reagent decreases and the reaction time becomes longer. When it exceeds 80°C, side reactions are promoted, the molecular weight of the sample decreases, and the fiber structure of the highly crystalline rigid cellulose nanofibers is destroyed, making it difficult to use as a stabilizer for an O / W emulsion.
[0218] The reaction time of the oxidation treatment can be appropriately set in consideration of the reaction temperature, the required amount of carboxyl groups, etc., and is not particularly limited, but is usually 10 minutes to 5 hours.
[0219] The pH of the reaction system during the oxidation reaction is not particularly limited, but is preferably 9 or more and 11 or less. When the pH is 9 or more, the reaction can proceed effectively. When the pH exceeds 11, a side reaction may occur, which promotes the decomposition of the sample. In addition, in the oxidation treatment, as the oxidation proceeds, the pH in the system decreases due to the generation of carboxyl groups, so it is preferred to keep the pH of the reaction system at 9 or more and 11 or less in the oxidation treatment. As a method for keeping the pH of the reaction system at 9 or more and 11 or less, a method of adding an alkaline aqueous solution as the pH decreases can be cited.
[0220] Examples of the alkaline aqueous solution include organic bases such as sodium hydroxide aqueous solution, lithium hydroxide aqueous solution, potassium hydroxide aqueous solution, ammonia aqueous solution, tetramethylammonium hydroxide aqueous solution, tetraethylammonium hydroxide aqueous solution, tetrabutylammonium hydroxide aqueous solution, and benzyltrimethylammonium hydroxide aqueous solution. In terms of cost, sodium hydroxide aqueous solution is preferred.
[0221] By adding alcohol to the reaction system, the oxidation reaction caused by the N-oxyl compound can be stopped. At this time, the pH of the reaction system is preferably maintained within the above range. As the alcohol added, in order to quickly terminate the reaction, low molecular weight alcohols such as methanol, ethanol, and propanol are preferred. From the perspective of the safety of the by-products generated by the reaction, ethanol is particularly preferred.
[0222] The reaction solution after the oxidation treatment can be directly supplied to the micronization step, but in order to remove colorants such as N-oxyl compounds, impurities, etc., it is preferred to recover the oxidized cellulose contained in the reaction solution and wash it with a washing solution. The recovery of the oxidized cellulose can be carried out by a known method such as filtering using a glass filter or a nylon mesh with a pore size of 20 μm. Pure water is preferably used as the washing solution for washing the oxidized cellulose.
[0223] If the obtained TEMPO oxidized cellulose is subjected to a defibration treatment, TEMPO oxidized cellulose nanofibers (hereinafter also referred to as TEMPO oxidized CNF, cellulose single nanofibers, CSNF) having a uniform fiber width of 3 nm are obtained. When CSNF is used as a raw material for cellulose nanofibers of composite particles 1, it is easy to make the particle size of the obtained O / W type emulsion uniform due to its uniform structure.
[0224] As described above, the CSNF used in this embodiment can be obtained by the steps of oxidizing the cellulose raw material and the steps of refining and dispersing the cellulose raw material into liquid. In addition, the content of the carboxyl group introduced into the CSNF is preferably 0.1 mmol / g to 5.0 mmol / g, and more preferably 0.5 mmol / g to 2.0 mmol / g.
[0225] Here, when the amount of carboxyl groups is less than 0.1 mmol / g, it is difficult to micronize and uniformly disperse the cellulose because the solvent cannot enter between the cellulose microfibrils through the osmotic pressure effect. In addition, when the amount of carboxyl groups exceeds 5.0 mmol / g, the molecular weight of the cellulose microfibrils is reduced due to the side reactions caused by the accompanying chemical treatment, so that the fiber structure of the highly crystalline rigid cellulose nanofibers cannot be obtained, and it is difficult to use it as a stabilizer for O / W emulsions.
[0226] If necessary, in the dispersion of fine fibers, a functional material may be supported on the fine fibers to obtain a dispersion of fine fibers supported with a functional material. Composite particles can be obtained by using fine fibers supported with a functional material.
[0227] There is no particular limitation on the method of imparting the functional material to the microfibers, and a known method can be used. For example, a method of adding and mixing the functional material in the dispersion of the microfibers to make it adhere can be used. In addition, the functional material can be synthesized in the dispersion of the microfibers and loaded.
[0228] Here, as described above, when loading the functional material on the fine fiber, it is preferred to introduce anionic functional groups on the crystal surface of the fine fiber in advance. By adding and mixing the cationic functional material in the dispersion of the fine fiber having the anionic functional group, the functional material can be stably loaded on the fine fiber. In addition, by adjusting the pH of the dispersion, the loading or removal of the functional material can be controlled.
[0229] The concentration of the fine fibers when the functional material is loaded is not particularly limited, but is preferably 0.1% by mass or more and 20% by mass or less, and more preferably 0.5% by mass or more and 10% by mass or less. When the concentration of the fine fibers is less than 0.1%, it is difficult to effectively load the functional material. When the concentration of the fine fibers exceeds 20% by mass, the viscosity of the fine fibers is very high, and sufficient stirring cannot be performed, making it difficult to react uniformly.
[0230] The solvent of the dispersion of fine fibers is not particularly limited, but preferably a hydrophilic solvent. The hydrophilic solvent is not particularly limited, but preferably water; alcohols such as methanol, ethanol, and isopropanol; cyclic ethers such as tetrahydrofuran. It is particularly preferred that the dispersion contains 50% by mass or more of water. If the proportion of water in the suspension is less than 50% by mass, the dispersibility of the fine fibers may deteriorate. In addition, as the solvent contained other than water, the above-mentioned hydrophilic solvent is preferred.
[0231] If necessary, the pH of the suspension may be adjusted to improve the dispersibility of the fine fiber raw material and the fine fibers. Examples of the alkaline aqueous solution used for pH adjustment include organic bases such as sodium hydroxide aqueous solution, lithium hydroxide aqueous solution, potassium hydroxide aqueous solution, ammonia aqueous solution, tetramethylammonium hydroxide aqueous solution, tetraethylammonium hydroxide aqueous solution, tetrabutylammonium hydroxide aqueous solution, and benzyltrimethylammonium hydroxide aqueous solution. In terms of cost, sodium hydroxide aqueous solution is preferred.
[0232] The method of supporting the metal fine particles as the functional material on the cellulose nanofibers having anionic functional groups is not particularly limited, and the cellulose nanofibers can be produced, for example, by the following method.
[0233] The method comprises: a cellulose nanofiber dispersion liquid preparation step, in which a dispersion liquid containing at least one cellulose nanofiber is prepared; a metal salt and cellulose nanofiber containing liquid preparation step, in which a dispersion liquid containing at least one metal salt and at least one cellulose nanofiber is prepared; and a cellulose nanofiber dispersion liquid preparation step loaded with metal particles, in which metal ions in the metal salt and cellulose nanofiber containing liquid are reduced to load the metal particles.
[0234] If necessary, the fine fibers carrying the functional material may be washed by filtration, centrifugal separation or the like to remove free functional material.
[0235] (Step 2-i)
[0236] The step 2-i is a step of coating the surface of droplets containing a pore-forming agent and a core material in a dispersion of fine fibers with fine fibers to stabilize the droplets in the form of an emulsion.
[0237] Specifically, the process is as follows: adding a core material-containing liquid containing a pore-forming agent and a core material to the dispersion of fine fibers obtained in the first process, dispersing the core material in the dispersion of fine fibers in the form of droplets, and coating the surfaces of the droplets with fine fibers, thereby preparing an O / W type emulsion stabilized by fine fibers. The O / W type emulsion stabilized by fine fibers is referred to as an emulsion.
[0238] As the method for making O / W type emulsion, it is not particularly limited, common emulsification can be used, for example various homogenizers are used or mechanical stirring is used, specifically, mechanical treatments such as high pressure homogenizer, ultrahigh pressure homogenizer, universal homogenizer, ball mill, roller mill, cutter, planetary mill, jet mill, grinding machine, juicer mixer, homogenizing mixer, ultrasonic homogenizer, nano homogenizer, underwater collision, paint stirrer can be listed. In addition, multiple mechanical treatments can also be used in combination.
[0239] For example, when an ultrasonic homogenizer is used, the core material-containing liquid is added to the dispersion of the fine fibers to prepare a mixed solvent, and the front end of the ultrasonic homogenizer is inserted into the mixed solvent to perform ultrasonic treatment. The treatment conditions of the ultrasonic homogenizer are not particularly limited, for example, the frequency is usually 20 kHz or more, the power is usually 10 W / cm 2 The treatment time is not particularly limited, but is generally about 10 seconds to 1 hour.
[0240] By the ultrasonic treatment, the droplets containing the pore former and the core material are dispersed in the dispersion of the microfibers to be emulsified, and the microfibers are selectively adsorbed at the liquid / liquid interface between the droplets and the microfiber dispersion, so that the droplets are covered by the microfibers to form a structure that is stable as an O / W type emulsion. In this way, an emulsion that becomes stable by adsorbing a solid at the liquid / liquid interface is academically called a "Pickering emulsion."
[0241] As described above, the mechanism of formation of Pickering emulsion by microfibers is still uncertain, but it is believed that since cellulose has hydrophilic sites derived from hydroxyl groups and hydrophobic sites derived from hydrocarbon groups in its molecular structure, it exhibits amphiphilicity, and therefore, cellulose is adsorbed at the liquid / liquid interface between the hydrophobic monomer and the hydrophilic solvent due to its amphiphilicity.
[0242] As described above, when the droplets dispersed in the O / W type emulsion contain a hydrophobic non-polymerizable solvent as a pore-forming agent, oil droplets containing the non-polymerizable solvent are formed inside the core particles when the core material is solidified in step 3-i. By removing the non-polymerizable solvent, pores can be formed inside the core particles.
[0243] In addition, when the droplets dispersed in the O / W emulsion contain an excessive amount of surfactant, the hydrophilic solvent as the continuous phase is absorbed into the interior of the droplets and acts as a pore former, so that the core particles generated by solidifying the core material in step 3-i contain the hydrophilic solvent. By removing the hydrophilic solvent, pores can be formed inside the core particles.
[0244] The structure of the O / W emulsion can be confirmed by optical microscopic observation. The particle size of the O / W emulsion is not particularly limited, but the average particle size is preferably 0.1 μm or more and 1000 μm or less. The average particle size can be calculated by randomly measuring the diameters of 100 emulsions and taking the average value.
[0245] In the O / W type emulsion structure, the thickness of the coating layer (fine fiber layer) formed on the surface layer of the droplet containing the pore former and the core material is not particularly limited, and is preferably 3 nm or more and 1000 nm or less. Although not particularly limited, the particle size in the emulsion structure is the same as the particle size of the composite particles obtained in step 3-i. The thickness of the coating layer can be measured, for example, by using a cryo-TEM.
[0246] The weight ratio of the fine fiber dispersion to the core material used in step 2-i is not particularly limited, but the polymerizable monomer is preferably 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the fine fibers. When the polymerizable monomer is less than 1 part by mass, the yield of the composite particles decreases, which is not preferred, and when it exceeds 50 parts by mass, it is difficult to uniformly cover the droplets containing the pore-forming agent and the core material with the fine fibers, which is not preferred.
[0247] The core material containing liquid used can contain the core material and can form an O / W type emulsion. In order to stably form an O / W type emulsion, it is preferably hydrophobic. In addition, the core material is a material that is solidified by chemical changes or physicochemical changes to form core particles. There is no particular limitation on the core material, as long as droplets containing a pore-forming agent and a core material can be stably formed. As the core material, for example, a polymerizable monomer (monomer), a molten polymer, or a soluble polymer can be used.
[0248] The type of polymerizable monomer used in step 2-i is not particularly limited as long as it is a monomer of a polymer, has a polymerizable functional group in its structure, is liquid at room temperature, is incompatible with water, and can form a polymer (polymer) through a polymerization reaction. The polymerizable monomer has at least one polymerizable functional group. A polymerizable monomer having one polymerizable functional group is also called a monofunctional monomer. In addition, a polymerizable monomer having two or more polymerizable functional groups is also called a multifunctional monomer.
[0249] The type of polymerizable monomer is not particularly limited, and examples thereof include (meth) acrylic monomers, vinyl monomers, etc. In addition, polymerizable monomers having a cyclic ether structure such as an epoxy group or an oxetane structure (e.g., ε-caprolactone, etc.) may also be used. It should be noted that the expression "(meth)acrylate" means both "acrylate" and "methacrylate".
[0250] Examples of the monofunctional (meth)acrylic monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, and propylene glycol. isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, carbitol ethyl (meth)acrylate, (meth)acrylate phosphate, ethylene oxide modified (meth)acrylate phosphate, (meth)acrylate phenoxy, ethylene oxide modified (meth)acrylate phenoxy, propylene oxide modified (meth)acrylate phenoxy esters of ethylene oxide, nonylphenol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, propylene oxide-modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acrylic acid adamantane derivative mono(meth)acrylates such as adamantane acrylate having a monovalent mono(meth)acrylate derived from 2-adamantane and adamantanediol, and the like.
[0251] Examples of the bifunctional (meth)acrylic monomer include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and di(meth)acrylates such as hydroxypivalate neopentyl glycol di(meth)acrylate.
[0252] Examples of the trifunctional or higher (meth)acrylic monomer include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tri(meth)acrylate tri-2-hydroxyethyl isocyanurate, and glycerol tri(meth)acrylate; tri(meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Ester compounds; polyfunctional (meth)acrylate compounds having three or more functions such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate; and polyfunctional (meth)acrylate compounds obtained by substituting a part of these (meth)acrylates with alkyl or ε-caprolactone, etc.
[0253] As the monofunctional vinyl monomer, a liquid incompatible with water at room temperature is preferred, such as vinyl ethers, vinyl esters, aromatic vinyls, and particularly styrene and styrene-based monomers.
[0254] Examples of (meth)acrylates among the monofunctional vinyl monomers include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, alkyl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, aryl (meth)acrylate, diethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, heptafluorodecyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and tricyclodecanyl (meth)acrylate.
[0255] Examples of the monofunctional aromatic vinyl monomer include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, ethylstyrene, isopropenyltoluene, isobutyltoluene, tert-butylstyrene, vinylnaphthalene, vinylbiphenyl, and 1,1-diphenylethylene.
[0256] Examples of the polyfunctional vinyl monomer include polyfunctional monomers having an unsaturated bond such as divinylbenzene, etc. A liquid that is incompatible with water at room temperature is preferred.
[0257] For example, specific examples of the multifunctional vinyl monomers include: (1) divinyls such as divinylbenzene, 1,2,4-trivinylbenzene, and 1,3,5-trivinylbenzene; (2) dimethacrylates such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-propylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, and 2,2-bis(4-methacryloyloxydiethoxyphenyl)propane; (3) trimethacrylates such as trimethylolpropane trimethacrylate and triethylolethane trimethacrylate; 4) Diacrylates such as ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, 1,3-dipropylene glycol diacrylate, 1,4-dibutylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2-bis(4-acryloxypropoxyphenyl)propane, and 2,2-bis(4-acryloxydiethoxyphenyl)propane; (5) Triacrylates such as trimethylolpropane triacrylate and triethylolethane triacrylate; (6) Tetraacrylates such as tetramethylolmethane tetraacrylate; (7) Others, such as tetramethylenebis(ethyl fumarate), hexamethylenebis(acrylamide), triallyl cyanurate, and triallyl isocyanurate.
[0258] For example, specific examples of the polyfunctional styrene-based monomers include divinylbenzene, trivinylbenzene, divinyltoluene, divinylnaphthalene, divinylxylene, divinylbiphenyl, bis(vinylphenyl)methane, bis(vinylphenyl)ethane, bis(vinylphenyl)propane, and bis(vinylphenyl)butane.
[0259] In addition to these, polyether resins, polyester resins, polyurethane resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, etc. having at least one polymerizable functional group can also be used, without particular limitation.
[0260] The above polymerizable monomers may be used alone or in combination of two or more.
[0261] Furthermore, a polymerization initiator may be added to the polymerizable monomer. Examples of general polymerization initiators include free radical initiators such as organic peroxides and azo polymerization initiators.
[0262] Examples of the organic peroxide include peroxyketal, hydroperoxide, dialkyl peroxide, diacyl peroxide, peroxycarbonate, and peroxyester.
[0263] Examples of the azo polymerization initiator include 2,2-azobis(isobutyronitrile) (AIBN), 2,2-azobis(2-methylbutyronitrile) (AMBN), 2,2-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1-azobis(1-cyclohexanecarbonitrile) (ACHN), 2,2-azobisisobutyric acid dimethyl ester (MAIB), 4,4-azobis(4-cyanovaleric acid) (ACVA), 1,1-azobis(1-acetoxy-1-phenylethane), 2,2-azobis(2-methylbutyronitrile) (AMBN), 2,4-dimethylvaleronitrile (ADVN), 1,1-azobis(1-cyclohexanecarbonitrile) (ACHN), 2,2-azobisisobutyric acid dimethyl ester (MAIB), 4,4-azobis(4-cyanovaleric acid) (ACVA), 1,1-azobis(1-acetoxy-1-phenylethane), 2,2-azobis(2-methylbutyronitrile) ... Amide), 2,2-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2-azobis(2-methylamidinopropane) dihydrochloride, 2,2-azobis[2-(2-imidazolin-2-yl)propane], 2,2-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2-azobis(2,4,4-trimethylpentane), 2-cyano-2-propylazoformamide, 2,2-azobis(N-butyl-2-methylpropionamide), 2,2-azobis(N-cyclohexyl-2-methylpropionamide), etc.
[0264] If a core material containing liquid containing a polymerizable monomer and a polymerization initiator is used in the 2-i step, the polymerization initiator is contained in the droplets of the O / W type emulsion (droplets containing a pore former and a core material) in the later-described 3-i step, so that when the monomers inside the above-mentioned droplets of the emulsion are polymerized in the later-described 3-i step, the polymerization reaction proceeds easily.
[0265] The weight ratio of the polymerizable monomer and the polymerization initiator that can be used in step 2-i is not particularly limited. Generally, the polymerization initiator is preferably 0.1 parts by mass or more relative to 100 parts by mass of the polymerizable monomer. When the polymerization initiator is less than 0.1 parts by mass, the polymerization reaction cannot be fully carried out, and the yield of the composite particles is reduced, which is not preferred.
[0266] The polymer used to obtain the soluble polymer is not particularly limited, but is preferably one that is difficult to dissolve in a hydrophilic solvent. When the polymer is dissolved in a hydrophilic solvent, a stable emulsion cannot be formed.
[0267] Examples of the polymer for obtaining the soluble polymer include the following.
[0268] Cellulose acetate derivatives such as cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate; polysaccharides such as chitin and chitosan; polylactic acids such as polylactic acid and copolymers of lactic acid and other hydroxycarboxylic acids.
[0269] Dibasic acid polyesters such as polybutylene succinate, polyethylene succinate, and polybutylene adipate. Polycaprolactones such as copolymers of caprolactone and hydroxycarboxylic acid.
[0270] Polyhydroxybutyrates such as polyhydroxybutyrate and copolymers of polyhydroxybutyrate and hydroxycarboxylic acid.
[0271] Aliphatic polyesters such as polyhydroxybutyric acid and copolymers of polyhydroxybutyric acid and other hydroxycarboxylic acids.
[0272] Polyamino acids; polyester-polycarbonate; natural resins such as rosin, etc.
[0273] These may be used alone or in combination of two or more.
[0274] By dissolving the above polymer in a solvent, a soluble polymer can be obtained. As a solvent for dissolving the above polymer, a solvent with low compatibility with the dispersion of fine fibers is preferably used. When the solubility in a hydrophilic solvent is high, the solvent easily dissolves from the dispersed phase (droplets) to the continuous phase (hydrophilic solvent), so it is difficult to emulsify.
[0275] The boiling point of the solvent for dissolving the polymer is preferably 90° C. or lower. If the boiling point is higher than 90° C., the hydrophilic solvent of the dispersion of fine fibers evaporates before the solvent, making it difficult to obtain the composite particles 1 .
[0276] Specific examples of solvents that can be used include benzene, toluene, xylene, ethyl acetate, butyl acetate, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), isophorone, cellosolve acetate, isophorone, Solvesso 100, trichloroethylene, hexane, chloroform, methylene chloride, ethylene dichloride, isooctane, and nonane.
[0277] The weight ratio of the soluble polymer to the solvent is not particularly limited as long as the polymer can be dissolved. Preferably, the weight of the solvent is preferably 0.005 to 100 parts by mass, more preferably 0.1 to 80 parts by mass, relative to 100 parts by mass of the polymer.
[0278] As a method of obtaining a molten polymer by melting a polymer, for example, a solid polymer is melted at room temperature to become a liquid. Preferably, the molten polymer is added to a dispersion of fine fibers heated to a temperature capable of maintaining the polymer in a molten state while being mechanically treated with an ultrasonic homogenizer as described above, thereby stabilizing molten polymer droplets in the dispersion as an O / W type emulsion.
[0279] As the molten polymer, a polymer with low solubility in the hydrophilic solvent of the fine fibers is preferred. When the solubility in the hydrophilic solvent is high, the polymer easily dissolves from the dispersed phase (droplets) to the continuous phase (hydrophilic solvent), so it is difficult to emulsify. In addition, the melting point of the molten polymer is preferably below 90°C. When the melting point is higher than 90°C, the water in the dispersion of the fine fibers evaporates, making it difficult to emulsify.
[0280] As the polymer used for the melt polymer, specifically, pentaerythritol tetrastearate, pentaerythritol distearate, pentaerythritol tristearate, stearyl stearate, batyl stearate, stearyl stearate, myristyl myristate, cetyl palmitate, ethylene glycol distearate, behenyl alcohol, microcrystalline wax, paraffin wax, hydrocarbon wax, fatty acid alkyl ester, polyol fatty acid ester, a mixture of fatty acid ester and wax, a mixture of fatty acid ester, monopalmitin glyceryl ( / stearate monoglyceryl), mono / distearate glyceryl ( / stearate glyceryl), monoacetate monostearate glyceryl ( / glyceryl fatty acid ester), succinic aliphatic monoglyceryl ( / glyceryl fatty acid ester), citric acid saturated aliphatic monoglyceryl, sorbitan monostearate, sorbitan fatty acid ester, sorbitan tribehenate, propylene glycol monobehenate ( / propylene glycol fatty acid ester), pentaerythritol adipate Stearic acid esters of polymers, pentaerythritol tetrastearate, dipentaerythritol hexastearate, stearyl citric acid, pentaerythritol fatty acid esters, glycerol fatty acid esters, ultra-light-colored rosin, rosin-containing glycols, ultra-light-colored rosin metal salts, hydrogenated petroleum resins, rosin esters, hydrogenated rosin esters, special rosin esters, linear phenolic resins, crystalline poly-α-olefins, polyalkylene glycols, polyalkylene glycol esters, polyoxyalkylene ethers; polylactic acids such as polylactic acid and copolymers of lactic acid and other hydroxycarboxylic acids; dibasic acid polyesters such as polybutylene succinate, polyethylene succinate, polybutylene adipate; polycaprolactones such as copolymers of caprolactone and hydroxycarboxylic acids; polyhydroxybutyrates such as copolymers of polyhydroxybutyrate and hydroxycarboxylic acids; aliphatic polyesters such as polyhydroxybutyric acid and copolymers of polyhydroxybutyric acid and other hydroxycarboxylic acids; polyamino acids; polyester-polycarbonates; natural resins such as rosin, etc.
[0281] By using a liquid containing a pore former as the core material-containing liquid, core particles having pores can be obtained. As the pore former, a known pore former as described above can be used, and for example, a non-polymerizable solvent can be used.
[0282] Examples of the non-polymerizable solvent include aromatic compounds, acetate compounds, and aliphatic hydrocarbons. Examples of aromatic compounds include toluene and xylene, examples of acetate compounds include ethyl acetate and butyl acetate, and examples of aliphatic hydrocarbons include n-hexane, n-heptane, n-octane, and n-dodecane.
[0283] Although not particularly limited, the non-polymerizable solvent preferably dissolves the core material but does not dissolve the solidified core particles. From this viewpoint, acetate compounds and aliphatic hydrocarbons are preferably used as the non-polymerizable solvent, and among them, n-hexane and n-heptane are preferably used.
[0284] By using a non-polymerizable solvent that dissolves the core material but not the solidified core particles, in step 2-i, droplets are obtained in a state where the non-polymerizable solvent is dissolved in the core material. In step 3-i, when the core material is solidified, the non-polymerizable solvent precipitates in the form of oil droplets inside the generated core particles. In step 4, by removing the hydrophilic solvent, composite particles having porous or hollow core particles can be obtained.
[0285] There is no particular limitation on the weight ratio of the core material to the pore former used in the 2-i step, but the content of the pore former relative to the total mass of the core material and the pore former is, for example, 10% by mass to 90% by mass, preferably 20% by mass to 80% by mass, and more preferably 30% by mass to 80% by mass. When the content of the pore former is less than 10% by mass, sufficient pores cannot be formed inside the core particles, or the porosity (void ratio) of the core particles is reduced, which may make it impossible for the composite particles to obtain sufficient soft focus and good texture. On the other hand, when the content of the pore former exceeds 90% by mass, it is difficult to obtain spherical particles.
[0286] In order to obtain core particles having pores, the core material-containing liquid preferably contains an oil-soluble surfactant. By containing a large amount of an oil-soluble surfactant in the core material-containing liquid, the hydrophilic solvent as the continuous phase solvent in the 2-i step or the 3-i step is absorbed into the droplets, so that the hydrophilic solvent plays a role as a pore-forming agent. Therefore, when the solvent is removed in the 4th step, composite particles having porous or hollow core particles can be obtained.
[0287] The oil-soluble surfactant is not particularly limited as long as it can be dissolved in the core material. HLB (Hydrophilic-Lipophilic Balance) is preferably 8 or less. As the oil-soluble surfactant, it is preferred to use a nonionic surfactant, for example, sorbitan fatty acid esters, glycerol fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, etc. Among them, sorbitan fatty acid esters are preferably used, for example, sorbitan monooleate, sorbitan monostearate, sorbitan monopalmitate, sorbitan trioleate, etc. can be used.
[0288] There is no particular limitation on the weight ratio of the core material to the oil-soluble surfactant that can be used in step 2-i, but the oil-soluble surfactant is preferably at or above the critical micelle concentration. When the oil-soluble surfactant is at or above the critical micelle concentration, the hydrophilic solvent of the continuous phase is absorbed, and the hydrophilic solvent acts as a pore-forming agent, thereby preparing porous or hollow composite particles.
[0289] In addition, the droplets (droplets containing the core material and the pore-forming agent) dispersed in the dispersion of fine fibers in step 2-i may contain components other than the polymerization initiator in advance.
[0290] Specific examples of such ingredients include colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, deodorants, fragrances, flavors, anti-dandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials such as fats and waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), enzymes, etc.
[0291] When the liquid droplets including the core material and the pore-forming agent contain components other than the polymerization initiator in advance, the components can be contained inside the core particles when the composite particles are formed, thereby being able to exhibit functions suitable for the intended use.
[0292] Preferably, other components are easily dissolved or dispersed in the droplets containing the core material and the pore-forming agent but are difficult to dissolve or disperse in the hydrophilic solvent. By dissolving or dispersing other components in the droplets, other components are easily encapsulated in the emulsion droplets when forming an O / W type emulsion, so that composite particles encapsulating other components can be effectively obtained. In addition, the amount of other components encapsulated can be increased.
[0293] In addition, as the core material, a polymerizable monomer, a soluble polymer, and a molten polymer can be used together to form droplets containing a core material and a pore-forming agent and emulsified. In addition, when a biodegradable polymer (resin) is selected as the polymer type of the core particle of the composite particle, since the resulting composite particle is composed of the core particle composed of the biodegradable polymer and fine fibers, it can become a particle with high environmental friendliness of a biodegradable material.
[0294] (Step 2-ii)
[0295] Step 2-ii is a step in which droplets (hydrophilic) containing a pore-forming agent such as a hydrophilic solvent are dispersed in a core material to prepare a W / O type emulsion, and droplets (hydrophobic) containing the W / O type emulsion are dispersed in a fine fiber dispersion so that the surfaces of the droplets are covered with fine fibers to become stable as a W / O / W type emulsion.
[0296] Specifically, a stabilizer is dissolved or dispersed in a core material, and a hydrophilic solvent such as water is added as a pore-forming agent and dispersed to prepare a W / O type emulsion in which droplets (hydrophilic) are dispersed. Next, the W / O type emulsion is added to the fine fiber dispersion obtained in the first step, and is dispersed in the fine fiber dispersion in the form of droplets, and the surface of the droplets (hydrophobic) is covered with fine fibers, thereby preparing a W / O / W type emulsion stabilized by fine fibers.
[0297] It should be noted that, unless otherwise specified, the same materials and methods as those of the step 2-i were used in the step 2-ii.
[0298] As the method for making W / O type emulsion, it is not particularly limited, and common emulsification can be used, for example various homogenizers are used or mechanical stirring is used, specifically, mechanical treatments such as high pressure homogenizer, ultrahigh pressure homogenizer, universal homogenizer, ball mill, roller mill, chopper, planetary mill, jet mill, grinding machine, grinder, juice mixer, homogenizing mixer, ultrasonic homogenizer, nano homogenizer, underwater collision, paint stirrer can be listed. In addition, multiple mechanical treatments can also be used in combination.
[0299] For example, when using an ultrasonic homogenizer, a hydrophilic solvent such as water as a pore-forming agent is added to the core material-containing liquid containing a stabilizer to prepare a mixed solvent, and the front end of the ultrasonic homogenizer is inserted into the mixed solvent to perform ultrasonic treatment. The treatment conditions of the ultrasonic homogenizer are not particularly limited, for example, the frequency is usually 20kHz or more, the power is usually 10W / cm 2 The treatment time is not particularly limited, but is generally about 10 seconds to 1 hour.
[0300] Through the above-mentioned ultrasonic treatment, droplets containing a hydrophilic solvent as a pore former are dispersed in the core material-containing liquid for emulsification. In addition, the stabilizer is selectively adsorbed at the liquid / liquid interface between the droplets and the core material phase to form a structure stable as a W / O type emulsion.
[0301] The hydrophilic solvent of the pore former contained in the hydrophilic droplets may be any solvent that is difficult to dissolve in the core material. For example, the same hydrophilic solvent as that used for the continuous phase may be used.
[0302] In order to disperse the droplets containing the hydrophilic solvent as a pore former in the core material to prepare the W / O type emulsion, a stabilizer may be used. The stabilizer is not particularly limited as long as it can stabilize the droplets, and for example, an oil-soluble surfactant or a solid material may be used.
[0303] As the oil-soluble surfactant, the nonionic surfactant described above can be used. For example, sorbitan fatty acid esters, glycerol fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, etc. can be cited. Among them, sorbitan fatty acid esters are preferably used, for example, sorbitan monooleate, sorbitan monostearate, sorbitan monopalmitate, sorbitan trioleate, etc. can be used.
[0304] As a solid material, any material that can stabilize the droplets may be used, for example, clay, carbon black, silica particles, titanium oxide particles, and fine fibers. When fine fibers are used, it is preferred to introduce hydrophobic functional groups on the fiber surface. There is no particular limitation on the method for introducing the hydrophobic functional groups, and the hydrophobic functional groups may be introduced by ionic bonds, covalent bonds, and the like. When fine fibers having ionic functional groups are used as the fine fibers, organic onium ions and the like may be used to introduce the hydrophobic functional groups by ionic bonds.
[0305] By dispersing the obtained W / O type emulsion in the form of droplets in the fine fiber dispersion in the same manner as in step 2-i, the surface of the droplets can be covered with the fine fibers to stabilize the W / O / W type emulsion.
[0306] In a W / O / W type emulsion, by solidifying the core material in step 3-i, core particles containing droplets of a hydrophilic solvent coated with fine fibers can be obtained. By removing the hydrophilic solvent, composite particles having porous or hollow core particles coated with fine fibers can be obtained.
[0307] (Step 3-i)
[0308] This is a step of solidifying the core material inside the liquid droplets to obtain a dispersion of particles in which the surfaces of the core particles are covered with fine fibers.
[0309] There is no particular limitation on the method for solidifying the core material. When a polymerizable monomer is used as the core material, the core material can be solidified by polymerizing the polymerizable monomer to form a polymer. When a soluble polymer is used as the core material, the core material can be solidified by removing the solvent from the soluble polymer by diffusing the solvent inside the droplet into a hydrophilic solvent or by evaporating the solvent. When a molten polymer is used as the core material, the core material can be solidified by cooling and solidifying the molten polymer.
[0310] In the manufacturing method 1, when the droplets contained in the O / W type emulsion formed in the 2-i step are composed of a liquid in which a hydrophobic non-polymerizable solvent is dissolved in the core material, the non-polymerizable solvent is precipitated as oil droplets in the 3-i step, thereby forming core particles containing oil droplets. In addition, when the core material contains an oil-soluble surfactant, the hydrophilic solvent of the continuous phase is absorbed by the droplets, thereby forming core particles containing the hydrophilic solvent.
[0311] In the production method II, the core material inside the droplets contained in the W / O / W type emulsion formed in the step 2-ii is solidified in the step 3-i, thereby forming core particles containing droplets containing a hydrophilic solvent.
[0312] For example, the core material is solidified by heating while stirring the O / W type emulsion to polymerize the polymerizable monomer, wherein the O / W type emulsion is stabilized by being coated with fine fibers by droplets containing the polymerizable monomer and polymerization initiator as the core material produced by the 2-i step and the 2-ii step. The stirring method is not particularly limited, and a known method can be used, specifically, a disperser or a stirrer can be used. In addition, it is also possible to perform heat treatment without stirring.
[0313] In addition, the temperature conditions during heating can be appropriately set according to the type of polymerizable monomer and the type of polymerization initiator, preferably above 20°C and below 150°C. When it is less than 20°C, the rate of polymerization reaction decreases, so it is not preferred; when it exceeds 150°C, the fine fibers may be modified, so it is not preferred. The time required for the polymerization reaction can be appropriately set according to the type of polymerizable monomer and the type of polymerization initiator, usually about 1 hour to 24 hours. In addition, the polymerization reaction can also be carried out by ultraviolet irradiation treatment as a type of electromagnetic wave. In addition, in addition to electromagnetic waves, particle beams such as electron beams can also be used.
[0314] As a method for evaporating the solvent of the soluble polymer, specifically, the solvent can be evaporated and removed by heating and / or drying under reduced pressure. When the boiling point of the organic solvent is lower than that of water, the organic solvent can be selectively removed. Although not particularly limited, the solvent can be effectively removed by heating under reduced pressure. The heating temperature is preferably 20° C. to 100° C., and the pressure is preferably 600 mmHg to 750 mmHg.
[0315] The method of diffusing the solvent of the soluble polymer is, specifically, to further add a solvent or a salt to the O / W type emulsion to diffuse the solvent inside the droplets. By diffusing the solvent with low solubility in the hydrophilic solvent into the hydrophilic solvent phase over time, the soluble polymer can be precipitated and solidified in the form of particles.
[0316] As a method of solidifying the molten polymer, the molten polymer can be solidified by cooling the O / W type emulsion.
[0317] (Step 4)
[0318] The fourth step is a step of recovering the core particles containing the pore-forming agent inside and covered with fine fibers on the surface from the dispersion obtained in the third step i, and generating pores inside the core particles by removing the pore-forming agent contained inside the core particles. As a recovery method, for example, a centrifugal separation method can be used.
[0319] The state of the dispersion obtained in step 3-i is such that the particles covered with fine fibers, a large amount of water, and free fine fibers that do not contribute to the formation of the coating layer are mixed together immediately after the particles covered with fine fibers are generated. Therefore, it is necessary to recover / clean the particles covered with fine fibers from the dispersion in this state, and as a method for recovering / cleaning, washing by centrifugation or washing by filtration is preferred.
[0320] As a cleaning method using centrifugal separation, a known method can be used. Specifically, the particles coated with fine fibers are repeatedly precipitated by centrifugal separation, the supernatant is removed, and the particles are redispersed in a water / methanol mixed solvent, and the residual solvent is removed from the precipitate finally obtained by centrifugal separation, thereby recovering the particles coated with fine fibers.
[0321] For filtration and washing, a known method can also be used, such as using a PTFE membrane filter with a pore size of 0.1 μm and repeatedly filtering with water and methanol to further remove the residual solvent from the slurry finally remaining on the membrane filter, thereby recovering the composite particles.
[0322] The method for removing the pore-forming agent is not particularly limited, and the drying can be carried out at normal pressure, reduced pressure, room temperature or heating, depending on the solvent to be removed. The dry solid material containing the composite particles thus obtained is not in the form of a film or aggregate as described above, but is obtained in the form of a fine powder.
[0323] If necessary, the composite particles may be dispersed in a solvent, and the functional material may be supported on fine fibers on the surface of the composite particles in the dispersion of the composite particles.
[0324] There is no particular limitation on the method for loading the functional material on the composite particles, and a known method can be used. For example, the following method can be used: the composite particles are redispersed in a hydrophilic solvent such as water or alcohol to prepare a dispersion of the composite particles, and the functional material is added and mixed into the dispersion of the composite particles to make it adhere. In addition, the functional material can be synthesized in the dispersion of the composite particles and loaded.
[0325] The method of supporting metal fine particles as a functional material on composite particles of cellulose nanofibers covered with cellulose nanofibers having anionic functional groups as fine fibers is not particularly limited, but examples thereof include the following methods.
[0326] The method comprises: a step of preparing a dispersion containing at least one of the above-mentioned composite particles; a step of preparing a dispersion containing at least one metal salt and composite particles; and a step of reducing metal ions in the dispersion containing the metal salt and composite particles to prepare a dispersion of composite particles loaded with metal microparticles.
[0327] If necessary, the composite particles loaded with the functional material may be separated by filtration, centrifugal separation or the like to remove free functional material.
[0328] The composite particles of this embodiment may have the functional components impregnated or enclosed in their pores. The inclusion of the functional components enables the functions to be exhibited.
[0329] The dry powder of the composite particles of this embodiment can be used as a light diffusion film, a heat insulating material, a home care product, or a personal care product. In particular, it is preferably used as personal care particles used for personal care applications.
[0330] Personal care products refer to cosmetics, toiletries, and other products that keep human skin clean, modify or beautify the appearance. They are related products of hair care, oral care, odor care, nail care, body care, skin care, and cosmetics, such as toothpaste, perfume, nail polish, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair gel, hair spray, shampoo, conditioner, hair toner, body lotion, face cream, and soap, etc.
[0331] The composite particles of this embodiment can be mixed or dispersed in other cosmetic raw materials and used in personal care products such as cosmetics. In addition, the composite particles 1 of this embodiment can be dispersed in a solvent containing cosmetic raw materials and used as a personal care composition.
[0332] Examples of cosmetic raw materials include colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, deodorant ingredients, fragrances, flavors, antidandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials such as fats and waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), etc.
[0333] (Effect of composite particles)
[0334] The composite particles of the first aspect of the present invention are novel composite particles having fine fibers, which solve the problem of excessive solvent in fine fibers such as cellulose nanofibers and chitin nanofibers and can be produced by a simple method.
[0335] Since the composite particles of the first mode of the present invention are covered with fine fibers with high safety, high hydrophilicity, high strength and large specific surface area, even if the composite particles are porous, they have high strength and good dispersion stability. They are composite particles with good skin affinity that can exert various functions such as high moisturizing, pore correction, and soft focus, and can be manufactured by a simple method.
[0336] Furthermore, the composite particles of the first embodiment of the present invention are porous particles with high porosity and large specific surface area or hollow particles with high porosity, and they will not break during the production process, and stable composite particles can be obtained.
[0337] By impregnating the pores of the composite particles of the first embodiment of the present invention with functional components, composite particles that exhibit various functions can be obtained.
[0338] In the first mode of composite particles of the present invention, when fine fibers such as cellulose nanofibers or chitin nanofibers are composed of cellulose or chitin / chitosan which are biodegradable polymers, and the core particles are also composed of a material containing a biodegradable polymer, it can be expected that the load on the environment will be reduced, which will help solve the problem of microplastics.
[0339] According to the production methods of the second and third aspects of the present invention, the composite particles of the first aspect of the present invention can be produced.
[0340] The composite particles of the first embodiment of the present invention can be used for personal care applications. That is, the composite particles of the first embodiment of the present invention can be included in personal care products and personal care compositions.
[0341] The composite particles of the first embodiment of the present invention can be used, for example, in products related to hair care, oral care, odor care, body care, skin care, and cosmetics, specifically, toothpaste, perfume, nail polish, beauty serum, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair gel, hair spray, shampoo, conditioner, hair tonic, body lotion, face cream, and soap.
[0342] [Second Embodiment]
[0343] like Figure 4 As shown, the personal care particle 1A of this embodiment is composed of the following: a core particle 2A formed of a material containing a polymer, a fine fiber 3 bound to the surface of the core particle 2A and in an inseparable state, and a functional material 40 that exerts a personal care function. The fine fiber 3 is any one of cellulose nanofibers and chitin nanofibers. The functional material 40 is supported on the fine fiber 3. The fine fiber 3 may also include both cellulose nanofibers and chitin nanofibers.
[0344] In the present embodiment, the fine fibers 3 are formed as a coating layer covering the surface of the core particle 2A.
[0345] The method for producing the personal care particles 1A is not particularly limited, and a known method can be used, and a chemical production method or a physicochemical production method can be used.
[0346] Examples of the chemical preparation method include polymerization granulation methods (emulsion polymerization method, suspension polymerization method, seed polymerization method, radiation polymerization method, etc.) in which particles are formed from polymerizable monomers during polymerization.
[0347] Examples of the physicochemical preparation method include a dispersion granulation method (spray drying method, liquid solidification method, solvent evaporation method, phase separation method, solvent dispersion cooling method, etc.) in which particles are formed from a polymer solution in the form of microdroplets.
[0348] For example, by forming an O / W Pickering emulsion using fine fibers 3 and solidifying the core material inside the droplets to produce particles in which the surface of the core particles 2A is coated with fine fibers 3, personal care particles 1A can be obtained in which the core particles 2A and the fine fibers 3 are bound together and inseparable. By using the fine fibers 3 without using additives such as surfactants, stable droplets can be formed, thereby obtaining personal care particles 1A with high dispersibility, high effects brought about by functional materials, good smoothness, and good skin affinity.
[0349] The core material may be any material that forms the core particle 2A after solidification, and may be, for example, a polymerizable monomer, a molten polymer, or a soluble polymer.
[0350] The method for solidifying the core material is not particularly limited, and the core material can be solidified by polymerizing the polymerizable monomer, solidifying the molten polymer, and removing the solvent from the soluble polymer.
[0351] Personal care products refer to cosmetics, toiletries, and other products that keep human skin clean, modify or beautify the appearance. They are related products of hair care, oral care, odor care, nail care, body care, skin care, and cosmetics, such as toothpaste, perfume, nail polish, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair gel, hair spray, shampoo, conditioner, hair toner, body lotion, face cream, and soap, etc.
[0352] The personal care particles 1A of this embodiment can be used Figure 5 and Figure 6 The manufacturing method shown is used to manufacture.
[0353] Figure 5 The manufacturing method shown is equivalent to the manufacturing method of the fifth embodiment (manufacturing method III), and includes a first step, a 2-iii step, a 2-iv step, and a 3-ii step.
[0354] like Figure 5 As shown in (a), the first step is a step of defibrillating a cellulose raw material or a chitin / chitosan raw material in a hydrophilic solvent 7 to obtain a dispersion 11A of fine fibers 3A which are either unloaded cellulose nanofibers or chitin nanofibers. The second step-iii is a step of loading a functional material 40 that exerts a personal care function on the fine fibers 3A in the dispersion 11A of the unloaded fine fibers 3A, such as Figure 5 As shown in (b), a dispersion 11B of fine fibers 3B carrying the functional material 40 is obtained.
[0355] like Figure 5 As shown in (c), step 2-iv is a step of dispersing the droplet 6A containing the core material in the dispersion 11B of the fine fibers 3B carrying the functional material so that the surface of the droplet 6A is covered with the fine fibers 3B carrying the functional material.
[0356] Step 3-ii is a step of solidifying the core material inside the droplet 6A. Figure 5 As shown in (d), through this step, personal care particles (particles in which the surface of the core particle 2A is covered with the fine fibers 3 carrying the functional material 40) 1A can be obtained.
[0357] Then, from Figure 5 The personal care particles 1A are separated and recovered from the dispersion in the state shown in (d).
[0358] That is, in the manufacturing method III, the O / W type Pickering emulsion is stabilized by adsorbing the fine fibers 3B loaded with the functional material to the interface of the droplets 6A dispersed in the hydrophilic solvent 7. Then, the core material inside the droplets 6A of the emulsion is solidified while maintaining the stabilized state, thereby obtaining the personal care particles 1A.
[0359] Figure 6 The manufacturing method shown corresponds to the manufacturing method of the sixth embodiment (manufacturing method IV), and includes a first step, a second-iv step, a third-ii step, and a fifth step.
[0360] like Figure 6 As shown in (a), the first step is a step of defibrillating a cellulose raw material or a chitin / chitosan raw material in a hydrophilic solvent 7 to obtain a dispersion 11A of fine fibers 3A which are either unsupported cellulose nanofibers or chitin nanofibers.
[0361] like Figure 6 As shown in (b), step 2-iv is a step of dispersing the liquid droplet 6A containing the core material in the dispersion liquid 11A of the unsupported fine fibers 3A so that the surface of the liquid droplet 6A is covered with the unsupported fine fibers 3A.
[0362] like Figure 6 As shown in (c), step 3-ii is a step of solidifying the core material inside the droplet 6A to obtain a dispersion 12A of particles 10A in which the surfaces of the core particles 2A are covered with the unsupported fine fibers 3A.
[0363] like Figure 6 As shown in (d), the fifth step is a step of loading the functional material 40 that performs the personal care function on the fine fibers 3A on the surface of the particles 10A in the dispersion 12A. Through this step, personal care particles (particles in which the surface of the core particles 2A is covered with the fine fibers 3 loaded with the functional material 40) 1A can be obtained. It should be noted that in this step, the functional material 40 is also loaded on the unloaded fine fibers 3A that exist independently in the dispersion 12A, thereby forming fine fibers 3B loaded with the functional material.
[0364] Then, from Figure 6 The personal care particles 1A are separated and recovered from the dispersion in the state shown in (d).
[0365] That is, in the manufacturing method IV, the O / W type Pickering emulsion is stabilized by adsorbing the fine fibers 3A at the interface of the droplets 6A dispersed in the hydrophilic solvent 7 and containing the core material. Then, the core material inside the emulsion is solidified while maintaining the stabilized state, thereby obtaining a particle 10A in which the surface of the core particle 2A is coated with the fine fibers 3A. Then, by loading the functional material 40 on the fine fibers 3A on the surface of the particle 10 coated with the fine fibers, the personal care particle 1A can be obtained.
[0366] The term "inseparable" as used herein means that the core particles and the fine fibers are not separated and the core particles are kept covered with the fine fibers even after repeated operations of centrifuging the dispersion containing the personal care particles and removing the supernatant, further adding a solvent for redispersion, thereby recovering and washing the personal care particles, or washing with a solvent by filtering and washing using a membrane filter. The coating state can be confirmed by observing the surface of the personal care particles using a scanning electron microscope.
[0367] In the above-mentioned manufacturing method, when obtaining the personal care particles of the present embodiment, the bonding mechanism between the fine fibers and the core particles is still uncertain, but it can be inferred as follows: since the personal care particles are made using the O / W type emulsion stabilized by the fine fibers as a template, when the fine fibers are in contact with the core material inside the emulsion droplets, the core material is solidified to form core particles, so the fine fibers are physically fixed to the surface of the core particles, and finally the core particles and the fine fibers reach an inseparable state.
[0368] Here, the O / W emulsion is also referred to as an oil-in-water emulsion, that is, water is used as a continuous phase, and oil is dispersed in the form of oil droplets (oil particles).
[0369] Although not particularly limited, when personal care particles are prepared using an O / W emulsion stabilized by fine fibers as a template, true spherical personal care particles derived from the O / W emulsion can be obtained because the O / W emulsion becomes stable. Specifically, a pattern in which a coating layer composed of fine fibers is formed on the surface of a true spherical core particle with a relatively uniform thickness is preferred.
[0370] The particle size of the personal care particles can be confirmed by optical microscopic observation. The average particle size can be calculated by measuring 100 points at random and averaging the particle diameters. The average particle size is not particularly limited, but is preferably 0.1 μm or more and 1000 μm or less.
[0371] From the viewpoint of dispersion stability, the fine fibers preferably form a coating layer on the surface of the core particle. The coating layer preferably covers the entire surface of the core particle, but it does not necessarily have to cover the entire surface.
[0372] The thickness of the coating layer composed of fine fibers is not particularly limited, but is preferably 3 nm to 1000 nm.
[0373] The average thickness of the coating layer can be obtained by the following method: using a microtome to cut the material obtained by fixing the personal care particles with the embedding resin, and observing it under a scanning electron microscope, the thickness of the coating layer in the cross-sectional image of the personal care particles in the image is measured at 100 random points on the image, and the average value is taken.
[0374] In addition, it is preferred that the personal care particles are uniformly coated with a coating layer having a relatively uniform thickness. When the thickness of the coating layer is uniform, the dispersion stability is high. Specifically, the coefficient of variation of the value of the thickness of the coating layer is preferably 0.5 or less, more preferably 0.4 or less.
[0375] The fine fibers constituting the personal care particles of the present embodiment are cellulose nanofibers and / or chitin nanofibers, similarly to the fine fibers constituting the composite particles of the first embodiment.
[0376] It should be noted that the crystal surface of the fine fiber constituting the personal care particles of the present embodiment preferably has an ionic functional group. By having an ionic functional group, the aggregation of the personal care particles can be suppressed, thereby effectively exerting the function of the functional material, and a personal care product with good skin affinity can be obtained. In addition, by utilizing the ionic functional group to load the functional material, the detachment of the functional material can be suppressed or controlled. For example, if it is a fine fiber with an anionic functional group, a cationic functional material can be loaded, and if it is a fine fiber with a cationic functional group, an anionic functional material is easily loaded.
[0377] The type of ionic functional group is not particularly limited, but preferably an anionic functional group. By having an anionic functional group, for example, in the case of loading metal particles, the metal ions are coordinated with the anionic functional groups of the microfibers and reduced and precipitated, so that the metal particles can be effectively loaded. In addition, the microfibers have the function of being a dispersion stabilizer, so that the shape and particle size of the generated metal particles can be controlled. In addition, in the personal care particles, the metal particles can be inhibited from detaching from the microfibers. In addition, usually, when the metal particles are dried, aggregation occurs, so the optical properties caused by the local surface plasmon resonance (LSPR) described later cannot be shown, but when the personal care particles are made into dry powders, the metal particles will not aggregate, so even dry powders can show optical properties.
[0378] The anionic functional group is not particularly limited, and examples thereof include a carboxyl group, a phosphoric acid group, and a sulfonic acid group. Among them, a carboxyl group and a phosphoric acid group are preferred, and a carboxyl group is preferred because it can be selectively introduced easily onto the surface of cellulose crystals.
[0379] The content of the ionic functional group is preferably 0.1 mmol or more and 5.0 mmol or less per 1 g of the fine fiber raw material and / or fine fiber. When it is less than 0.1 mmol, the dispersion stability of the personal care particles may deteriorate; when it exceeds 5.0 mmol, it may be difficult to stably load the functional material.
[0380] In addition, the fine fibers constituting the personal care particles of the present embodiment preferably have a fiber shape derived from a microfibril structure. Specifically, it is preferred that the fine fibers are fibrous, the number average minor axis diameter is 1 nm or more and 1000 nm or less, the number average major axis diameter is 50 nm or more, and the number average major axis diameter is 5 times or more of the number average minor axis diameter. In addition, the crystallinity of the fine fibers is preferably 50% or more. The crystal structure of the cellulose nanofibers is preferably cellulose type I. The crystal structure of the chitin nanofibers may be any of α-chitin and β-chitin, but is preferably α-chitin.
[0381] In the personal care particles of the present embodiment, the microfibers loaded with the functional material are coated on the surface of the core particles, and the dispersion stability of the functional material is improved, so that its function can be effectively exerted. The functional material is "loaded" on the microfibers means: physically or chemically, reversibly or irreversibly bound or adsorbed. In the personal care particles of the present invention, the functional material can be loaded by a known method.
[0382] In the personal care particles of the present embodiment, the functional material and the fine fibers are in an "inseparable" state. The "inseparability" of the fine fibers and the functional material means that the fine fibers and the functional material are not separated even after repeated operations of recovering and washing the personal care particles by centrifuging the dispersion containing the personal care particles and removing the supernatant, and further adding a solvent for redispersion, or repeatedly washing with a solvent by filtering and washing using a membrane filter.
[0383] The functional material constituting the personal care particles of this embodiment is a material that exerts its function in personal care products, and a known functional material can be used. Examples of the functional material include the materials exemplified in the first embodiment.
[0384] When colorants are used as functional materials, organic synthetic pigments or natural pigments are used to impart color to hair dyes, lotions, and beauty serums, and inorganic pigments and organic pigments are used in cosmetics to control the hue, chroma, and brightness of foundation or to control concealer power. In lipsticks and nail polishes, pigments are sometimes formulated in combination with dyes.
[0385] Dyes are substances that are dissolved in solvents such as water, oil, and alcohol, and exist in a dissolved state in a cosmetic base to color. There are water-soluble dyes that are soluble in water, and oil-soluble dyes that are soluble in oil or alcohol. Examples of dyes include azo dyes, xanthene dyes, and quinoline dyes. Although not particularly limited, dyes are preferably cationic dyes with cations or anionic dyes with anions. For example, if it is a cationic dye, it can be adsorbed on microfibers with anionic functional groups; if it is an anionic dye, it can be adsorbed on microfibers with cationic functional groups.
[0386] Lakes are metal salts of water-soluble dyes.
[0387] An organic pigment is a colored powder that has no soluble group in its structure and is insoluble in water, oil, etc. Examples of the organic pigment include azo pigments, indigo pigments, and phthalocyanine pigments.
[0388] Natural pigments are pigments derived from animals, plants, and microorganisms. Examples include yellow-orange-red carotenoid pigments found in carrots, tomatoes, and red salmon, and yellow-red-purple flavonoid pigments found in hibiscus and safflower.
[0389] Examples of the inorganic pigment include extender pigments, color pigments, white pigments, and pearlescent pigments.
[0390] Extender pigments are used to adjust the gloss and feel of use, and examples include: talc (hydrated magnesium silicate, talc), kaolin (hydrated aluminum silicate, white clay), mica (mica, hydrated potassium aluminum silicate), silica (silicic anhydride), calcium carbonate (CaCO3), magnesium carbonate (MgCO3), etc.
[0391] Examples of the color pigment include iron oxide, ultramarine blue, Prussian blue, chromium oxide, chromium hydroxide, manganese violet, and carbon black.
[0392] White pigments are used not only to adjust the color but also to cover blemishes and freckles and protect against ultraviolet rays. Examples of white pigments include titanium oxide and zinc oxide.
[0393] Examples of pearlescent pigments include titanium oxide-coated mica (mica titanium), bismuth oxychloride, etc. Various interference colors are expressed by changing the film thickness of titanium oxide coated on mica.
[0394] Examples of polymer powders include powders obtained by alternately laminating polymers having different refractive indices, nylon powders, and polymethyl methacrylate powders.
[0395] Metal particles can be used as colorants or light shielding agents. Metal particles have properties that bulk metals do not have. For example, when the particles become smaller, the total surface area of the particles becomes larger, so the catalytic performance of the particles improves. When the particles reach nanometer size, the melting point decreases, so the particles can be fired at low temperatures. In addition, depending on the size of the particles, the optical properties of the particles will also change greatly. When oxides with a small refractive index reach a size of less than 1 / 10 of the visible light wavelength region, the scattering of light becomes very small, so they are evenly dispersed in liquids and become transparent.
[0396] Based on localized surface plasmon resonance, nano-sized metal particles have the property of absorbing light of specific wavelengths depending on their elements, particle size, and shape. The free electrons on the surface of metal particles will vibrate collectively due to external electric fields such as light. Electrons are charged particles, so when electrons vibrate, they generate an electric field around them. The phenomenon in which the electric field generated by the vibration of free electrons resonates with the external electric field (light, etc.) is called localized surface plasmon resonance (LSPR). The LSPR causes absorption or reflection of light in a specific wavelength region, thereby enabling light shielding.
[0397] In addition, if the wavelength of light absorbed or reflected is in the visible light region, it functions as a colorant. The wavelength of light absorbed or scattered varies depending on the type of metal, particle size, and shape that constitute the metal particles. Compared with organic pigments that are generally used as colorants, metal particles have the characteristics of high stability and long-term stable absorption or scattering of specific wavelength regions.
[0398] The metal element constituting the metal microparticles is not particularly limited, but preferably contains at least one of rubidium (Ru), iron (Fe), cobalt (Co), rhodium (Rh), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), and zinc (Zn). The elements constituting the metal microparticles may be one or more.
[0399] Among them, it is preferred to contain one or more metals or metal compounds selected from nickel (Ni), palladium (Pd), silver (Ag), and gold (Au), but it is not particularly limited thereto. In addition, by using silver (Ag), antibacterial properties can be imparted.
[0400] When a plurality of metals are used, for example, the precipitated silver (Ag) fine particles may be coated with a metal more noble than silver or a metal oxide such as silicon dioxide, thereby improving the stability of the silver (Ag) fine particles.
[0401] Furthermore, the metal fine particles may contain components other than metals.
[0402] The average particle size of the metal particles is not particularly limited, but is preferably 500 nm or less. When the average particle size exceeds 500 nm, it is difficult to load on the fine fibers. More preferably, it is 0.1 nm or more and 50 nm or less. Since the color tone changes due to the average particle size of the metal particles, it is important to control the shape of the metal particles. The shape of the metal particles is not particularly limited. For example, spherical, flat, and rod-shaped can be listed.
[0403] In particular, in the case of flat metal particles or rod-shaped metal particles having anisotropic shapes such as flat or rod-shaped, the wavelength derived from LSPR absorption or scattering varies greatly depending on the aspect ratio. Among the metal particles having anisotropic shapes, flat silver particles or rod-shaped gold particles are particularly expected to be used.
[0404] For example, it is known that spherical silver nanoparticles with a particle size of several nm to tens of nm have absorption near a wavelength of 400 nm due to the above-mentioned LSPR, and therefore appear light yellow. However, anisotropically grown silver particles are not limited to this. For example, it is known that the absorption peak of planar silver particles is red-shifted. At this time, it can be confirmed that the larger the aspect ratio (i.e., particle size / particle thickness) of the planar silver particles, the more the absorption / scattering peak moves toward the longer wave side. That is, planar silver particles can be used as optical materials that absorb / scatter any wavelength. In addition, if the absorption / scattering wavelength is controlled in the visible light region, planar silver particles that present bright tones such as red and blue in addition to yellow can be obtained, thereby playing a role as a colorant.
[0405] Furthermore, depending on the aspect ratio of the tabular silver microparticles, the absorption peak can be shifted to the near infrared region outside the visible light region, thereby functioning as a near infrared light shielding agent.
[0406] Furthermore, the absorption / reflection peaks of the rod-shaped gold particles shift depending on the aspect ratio (major axis / minor axis).
[0407] It should be noted that in this embodiment, visible light refers to electromagnetic waves with a wavelength range of approximately 400nm to 700nm; near infrared light refers to electromagnetic waves with a wavelength range (approximately 700nm to 2500nm) close to visible light in infrared light.
[0408] In the present embodiment, the "fine particles" in the metal fine particles refer to particles having a volume particle size of 10 μm or less. In addition, the tabular silver fine particles are tabular silver fine particles, and the rod-shaped gold fine particles are rod-shaped gold fine particles.
[0409] Here, the thickness of the plate-like metal particles is set to h, the diameter is set to d (equivalent circle diameter), and the diameter d of the plate-like metal particles relative to the thickness h is set to aspect ratio (d / h). The "plate-like" of the plate-like metal particles means that the particles are plate-like, and the plate-like means (for example) that the average value of the aspect ratio (d / h) is greater than 1.1.
[0410] It should be noted that the shape of the surface and back of the plate-like metal particles is not particularly limited, but is generally a polygon such as a hexagon or a triangle. When the surface and back are polygonal or elliptical, the diameter d (circle equivalent diameter) is calculated by assuming the diameter of a circle equal to the area of the surface or back.
[0411] In addition, either the front surface or the back surface of the plate-like metal fine particles may have a larger area, and the two surfaces may not be parallel.
[0412] From the viewpoint of controlling optical properties, it is preferred that the shape of the tabular metal fine particles is tabular, and the particle diameter d, thickness h, and aspect ratio thereof are within the following ranges.
[0413] The average value of the particle diameter d of the plate-like metal fine particles is preferably from 2 nm to 1000 nm, more preferably from 20 nm to 500 nm, and even more preferably from 20 nm to 400 nm.
[0414] The average value of the thickness h of the plate-like metal fine particles, that is, the average value of the distance h between the front surface and the back surface, is preferably from 1 nm to 100 nm, and more preferably from 5 nm to 50 nm.
[0415] In addition, the said average value is calculated|required by measuring 100 particles, for example.
[0416] The average aspect ratio (average value of d / average value of h) of the plate-like metal fine particles is 1.1 or more, preferably 2.0 or more, more preferably 2.0 or more and 100 or less, and further preferably 2.0 or more and 50 or less. By arbitrarily changing the average value of the particle diameter d to control the average aspect ratio, the color tone can be changed.
[0417] The shape and size of the tabular metal fine particles can be evaluated using a scanning electron microscope, a transmission electron microscope, or a scanning transmission electron microscope.
[0418] Examples of a method for measuring the particle diameter d and thickness h of the plate-like metal fine particles and a method for calculating the aspect ratio include the following methods.
[0419] (1) Particle size measurement method
[0420] The dried powder of the personal care particles was observed by scanning transmission electron microscopy to obtain a scanning transmission electron microscope image. The diameter of the flat metal particles in the scanning transmission electron microscope image when they are approximately circular was calculated as the particle size in the plane direction. The above average value was obtained by measuring 100 particles.
[0421] (2)Method for measuring average thickness
[0422] The determination can be carried out by the following method: the dry powder of the personal care particles fixed by the embedding resin is cut in the cross-sectional direction by a microtome and observed by a transmission electron microscope. The thickness h of the flat metal particles in the transmission electron microscope is calculated as the thickness perpendicular to the plane direction. The average value (average thickness) of the thickness h is obtained by measuring 100 particles.
[0423] (3) Calculation method of average aspect ratio
[0424] The average value of the diameter d (equivalent circle diameter) of the tabular metal fine particles determined by the above method relative to the average value of the thickness h was calculated as the average aspect ratio of the tabular metal fine particles (average value of d / average value of h).
[0425] The method for measuring the particle size d and thickness h of the tabular metal fine particles and the method for calculating the average aspect ratio are examples, and the method for measuring the particle size and thickness of the tabular metal fine particles and the method for calculating the aspect ratio are not limited thereto.
[0426] The metal or metal compound constituting the flat metal particles is not particularly limited, and any metal or metal compound can be used. As the metal or metal compound constituting the flat metal particles, for example, metals, metal salts, metal complexes, and alloys or oxides and composite oxides thereof such as gold, silver, copper, aluminum, iron, platinum, zinc, palladium, ruthenium, iridium, rhodium, osmium, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum can be listed. Among them, it is preferred to include at least any one of gold, silver, and copper, and in particular, when at least silver is included, the flat metal particles can shield light with wavelengths from the visible light region to the near infrared region, thereby imparting antibacterial properties.
[0427] The ratio of the metal contained in the plate-like metal fine particles is not particularly limited.
[0428] exist Figure 5 In the method shown (manufacturing method III), first, the functional material 40 is loaded on the unloaded fine fiber 3A to produce the fine fiber 3B loaded with the functional material. Then, the fine fiber 3B loaded with the functional material is used to prepare an O / W type Pickering emulsion having a droplet 6A containing a core material. Next, the core material inside the droplet 6A of the emulsion is solidified, so that particles (personal care particles 1A) in which the core particles 2A are coated with the fine fiber 3B loaded with the functional material can be produced.
[0429] exist Figure 6 In the method shown (manufacturing method IV), first, an O / W type Pickering emulsion having a droplet 6A containing a core material is prepared using unloaded fine fibers 3A. Next, the core material inside the droplet 6A of the emulsion is solidified to prepare a particle 10A coated with the fine fibers 3A. Next, a functional material 40 is loaded on the fine fibers 3A on the surface of the particle 10A, thereby preparing a particle (personal care particle 1A) coated with the fine fibers 3B loaded with the functional material 40.
[0430] The method of supporting the functional material on the fine fibers is not particularly limited. For example, a commercially available or pre-made functional material may be added and mixed into a dispersion of fine fibers or a dispersion of particles coated with fine fibers to allow the functional material to adhere.
[0431] As a method for loading the functional material on the fine fibers, a method of loading the functional material in a dispersion of the fine fibers or in a dispersion of particles coated with the fine fibers is preferred. By loading the functional material in a dispersion of the fine fibers or in a dispersion of particles coated with the fine fibers, the functional material can be stably loaded on the fine fibers, thereby suppressing aggregation of the functional material.
[0432] The core particles constituting the personal care particles of the present embodiment are formed of materials containing one or more polymers. The polymer can use a known polymer, or a polymer obtained by polymerizing a polymerizable monomer by a known method. That is, as the material forming the core particles of the personal care particles of the present embodiment, the polymers exemplified in the first embodiment can be used.
[0433] The core particles constituting the personal care particles of the present embodiment may also contain other components such as functional components other than the polymer. For example, colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoamers, antistatic agents, adhesives, bleaching agents, chelating agents, deodorizing ingredients, aromatics, fragrances, antidandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials headed by fats and waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), etc. can be listed.
[0434] The functional component may be in any form of solid, gas, or liquid. The content of the functional component in the personal care particles is not particularly limited, but is preferably within a range that allows the personal care particles to stably maintain their form. When the content of the functional component is 100 parts by mass, the functional component is preferably 0.001 parts by mass or more and 80 parts by mass or less.
[0435] <About the manufacturing method of the granules for personal care>
[0436] As described above, the personal care particles of the embodiment can be Figure 5 and Figure 6 The method shown (manufacturing method III and manufacturing method IV) is used for manufacturing.
[0437] In the production method III and the production method IV, a dispersion containing personal care particles can be obtained. In addition, by removing the solvent from the dispersion, the personal care particles are obtained in the form of a dry solid substance. The method for removing the solvent is not particularly limited, and for example, the excess water can be removed by centrifugation or filtration, and then heat-dried in an oven to obtain the dry solid substance. In this case, the obtained dry solid substance is not in the form of a film or aggregate, but is obtained in the form of a fine and smooth powder.
[0438] In contrast, it is known that in conventional methods different from the production method III and the production method IV, when the solvent is removed from the dispersion liquid of the microfine fibers, the microfine fibers are strongly aggregated to form a film.
[0439] In the dispersion containing the personal care particles obtained by manufacturing method III and manufacturing method IV, the personal care particles are true spheres with fine fibers fixed on the surface, so even if the solvent is removed, the fine fibers will not aggregate with each other, and the personal care particles are only in contact with each other in a point-to-point manner. Therefore, it is believed that the dry solid material is obtained in the form of a fine powder. Thus, the personal care particles will not aggregate with each other, so that a smooth and skin-friendly cosmetic can be obtained in a powdered cosmetic. In addition, the aggregation of functional materials can be suppressed, so that a uniform powdered cosmetic can be obtained.
[0440] It should be noted that the dry powder of the personal care particles is a dry solid material that contains almost no solvent and can be further redispersed in a solvent. Specifically, the solid content of the dry powder of the personal care particles can be set to 80% or more, 90% or more, or 95% or more. From the viewpoints of reducing transportation costs, preventing decay, increasing the addition rate, and improving the kneading efficiency with the resin, personal care particles from which the solvent is almost removed are preferred.
[0441] Since the fine fibers existing on the surface of the personal care particles have high hydrophilicity, the dry powder of the personal care particles has the characteristics of absorbing moisture such as sweat or showing high moisturizing properties.
[0442] In addition, the personal care particles obtained in the form of dry powder are also easily redispersed in a solvent, and after redispersion, the dispersion stability derived from the fine fibers bonded to the surface of the personal care particles is also exhibited. Therefore, the dry powder of the personal care particles can be included in beauty essences, emulsions, creams, etc.
[0443] Hereinafter, each step will be described in detail.
[0444] As described above, the manufacturing method III includes the first step, the second-iii step, the second-iv step, and the third-ii step, and the manufacturing method IV includes the first step, the second-iv step, the third-ii step, and the fifth step.
[0445] (1st step)
[0446] The first step is to defibrate the fine fiber raw material in a solvent to obtain a dispersion of fine fibers. The fine fiber raw material refers to a raw material for cellulose nanofibers and / or chitin nanofibers, i.e., a cellulose raw material and a chitin / chitosan raw material. That is, the first step of this embodiment is the same as the first step of the first embodiment.
[0447] (Step 2-iii)
[0448] The step 2-iii is a step of supporting a functional material on fine fibers in a dispersion of fine fibers to obtain a dispersion of fine fibers supporting the functional material.
[0449] There is no particular limitation on the method of imparting the functional material to the microfibers, and a known method can be used. For example, a method of adding and mixing the functional material in the dispersion of the microfibers to make them adhere can be used. In addition, the functional material can be synthesized in the dispersion of the microfibers and loaded.
[0450] Here, as described above, when loading the functional material on the fine fiber, it is preferred to introduce anionic functional groups on the crystal surface of the fine fiber in advance. By adding and mixing the cationic functional material in the dispersion of the fine fiber having the anionic functional group, the functional material can be stably loaded on the fine fiber. In addition, by adjusting the pH of the dispersion, the loading or removal of the functional material can be controlled.
[0451] The concentration of the fine fibers when the functional material is loaded is not particularly limited, but is preferably 0.1% by mass or more and 20% by mass or less, and more preferably 0.5% by mass or more and 10% by mass or less. When the concentration of the fine fibers is less than 0.1%, it is difficult to effectively load the functional material. When the concentration of the fine fibers exceeds 20% by mass, the viscosity of the fine fibers is very high, and sufficient stirring cannot be performed, making it difficult to react uniformly.
[0452] The solvent of the dispersion liquid of fine fibers is not particularly limited, but the hydrophilic solvent 7 is preferable.
[0453] The hydrophilic solvent 7 is not particularly limited, but is preferably water; alcohols such as methanol, ethanol, and isopropanol; or cyclic ethers such as tetrahydrofuran.
[0454] It is particularly preferred that 50% by mass or more of water is contained. When the proportion of water in the suspension is less than 50% by mass, the dispersibility of the fine fibers may be deteriorated. In addition, as a solvent contained other than water, the above-mentioned hydrophilic solvent is preferred.
[0455] If necessary, the pH of the suspension may be adjusted to improve the dispersibility of the fine fiber raw material and the fine fibers. Examples of the alkaline aqueous solution used for pH adjustment include organic bases such as sodium hydroxide aqueous solution, lithium hydroxide aqueous solution, potassium hydroxide aqueous solution, ammonia aqueous solution, tetramethylammonium hydroxide aqueous solution, tetraethylammonium hydroxide aqueous solution, tetrabutylammonium hydroxide aqueous solution, and benzyltrimethylammonium hydroxide aqueous solution. In terms of cost, sodium hydroxide aqueous solution is preferred.
[0456] The method for supporting metal fine particles as a functional material on cellulose nanofibers having anionic functional groups is not particularly limited, but the cellulose nanofibers can be produced, for example, by the following method: The method includes step ia, step ib, and step ic in order.
[0457] Step ia: a cellulose nanofiber dispersion preparation step of preparing a dispersion containing at least one type of cellulose nanofibers.
[0458] Step ib: a step of preparing a liquid containing a metal salt and cellulose nanofibers, in which a dispersion liquid containing at least one metal salt and at least one cellulose nanofiber is prepared.
[0459] Step ic: a step of preparing a cellulose nanofiber dispersion liquid loaded with metal particles, wherein metal ions in a metal salt and a cellulose nanofiber-containing liquid are reduced to load the metal particles.
[0460] (Step ia: Cellulose nanofiber dispersion preparation step)
[0461] In step ia of the method for supporting metal fine particles on cellulose nanofibers, at least one cellulose nanofiber dispersion is prepared.
[0462] First, a cellulose nanofiber dispersion is prepared. The solid content concentration of the cellulose nanofiber dispersion is not particularly limited, but is preferably 0.1 mass % to 20 mass %, and more preferably 0.5 mass % to 10 mass %.
[0463] When the solid content concentration of the cellulose nanofiber dispersion is less than 0.1% by mass, it is difficult to control the particle size of the metal particles. On the other hand, when the solid content concentration of the cellulose nanofiber dispersion exceeds 20% by mass, the viscosity of the cellulose nanofiber dispersion becomes high, and it is difficult to uniformly mix the metal salt and the cellulose nanofibers in step ib (metal salt and cellulose nanofiber-containing liquid preparation step), and further, the reduction reaction cannot be uniformly performed in step ic (metal particle-loaded cellulose nanofiber dispersion preparation step).
[0464] The solvent for dispersing the cellulose nanofibers is not particularly limited as long as the cellulose nanofibers can be sufficiently dissolved or dispersed. From the viewpoint of environmental load, water is preferably used as the solvent.
[0465] From the viewpoint of dispersibility of metal fine particles and cellulose nanofibers, water or a hydrophilic solvent is preferably used as the solvent. The hydrophilic solvent is not particularly limited, but alcohols such as methanol, ethanol, and isopropanol are preferred.
[0466] The pH of at least one cellulose nanofiber dispersion is not particularly limited, but is preferably pH 2 or more and pH 12 or less.
[0467] (Step ib: Step of preparing a liquid containing a metal salt and cellulose nanofibers)
[0468] In step ib of the method for supporting metal fine particles on cellulose nanofibers, a dispersion liquid containing at least one metal salt and at least one cellulose nanofiber is prepared to prepare a metal salt and cellulose nanofiber-containing liquid.
[0469] The method for preparing a solution or dispersion containing at least one metal salt and at least one cellulose nanofiber is not particularly limited. For example, a dispersion containing at least one cellulose nanofiber (cellulose nanofiber dispersion) and a solution containing at least one metal salt (metal salt containing solution) are prepared, and the metal salt containing solution is added to the cellulose nanofiber dispersion while stirring the cellulose nanofiber dispersion. In addition, a solid metal salt may be directly added to the cellulose nanofiber dispersion, or the cellulose nanofiber dispersion may be added to the metal salt containing solution.
[0470] As the metal salt, at least one selected from the group consisting of silver nitrate, silver chloride, silver oxide, silver sulfate, silver acetate, silver nitrite, silver chlorate, chloroauric acid, sodium gold chloride, potassium gold chloride, platinum chloride, and platinum oxide is preferred. These metal salts may be used alone or in combination of two or more.
[0471] When the metal salt-containing solution is prepared, the solvent used in the metal salt-containing solution is not particularly limited as long as the metal salt is sufficiently dispersed or dissolved.
[0472] From the viewpoint of environmental load, it is preferred to use water as the solvent.
[0473] From the viewpoint of the solubility of the metal salt, water or a hydrophilic solvent is preferably used as the solvent. The hydrophilic solvent is not particularly limited, but alcohols such as methanol, ethanol, and isopropanol are preferred.
[0474] Furthermore, the concentration of the metal salt in the metal salt-containing solution is not particularly limited.
[0475] The concentration of the metal salt in the metal salt and cellulose nanofiber dispersion is not particularly limited, but is preferably 0.002 mmol / L or more and 20.0 mmol / L or less. In particular, when using cellulose nanofibers having anionic functional groups, metal ions coordinate with the anionic functional groups, so it is preferred to prepare in a manner that the concentration of the metal salt (the concentration of the metal ions) is less than the amount of the anionic functional groups. When the concentration of the metal salt (the concentration of the metal ions) exceeds the amount of the anionic functional groups of the cellulose nanofibers, the cellulose nanofibers may aggregate.
[0476] The solvent used in the liquid containing the metal salt and cellulose nanofibers is not particularly limited as long as the cellulose nanofibers can be sufficiently dispersed or dissolved.
[0477] From the viewpoint of environmental load, it is preferred to use water as the solvent.
[0478] From the viewpoint of dispersibility of cellulose nanofibers, water or a hydrophilic solvent is preferably used as the solvent. The hydrophilic solvent is not particularly limited, but alcohols such as methanol, ethanol, and isopropanol are preferred.
[0479] The solid content concentration of the cellulose nanofibers in the metal salt and cellulose nanofiber dispersion is not particularly limited, but is preferably 0.1 mass % to 20 mass %, and more preferably 0.1 mass % to 50 mass %.
[0480] When the solid content concentration of the cellulose nanofibers is less than 0.1% by mass, it is difficult to control the particle size of the metal particles. On the other hand, when the solid content concentration of the cellulose nanofibers exceeds 20% by mass, the viscosity of the cellulose nanofiber dispersion becomes high, making it difficult to uniformly mix the metal salt and the cellulose nanofibers in step ib, and further, the reduction reaction cannot be uniformly performed in step ic.
[0481] The solvent of the metal salt and the cellulose nanofiber-containing liquid is not particularly limited as long as the cellulose nanofibers are sufficiently dissolved or dispersed.
[0482] From the viewpoint of environmental load, it is preferred to use water as the solvent.
[0483] From the viewpoint of dispersibility of metal fine particles and cellulose nanofibers, water or a hydrophilic solvent is preferably used as the solvent. The hydrophilic solvent is not particularly limited, but alcohols such as methanol, ethanol, and isopropanol are preferred.
[0484] The pH of the liquid containing the metal salt and cellulose nanofibers is not particularly limited, but is preferably pH 2 or more and pH 12 or less.
[0485] The temperature of the liquid containing the metal salt and cellulose nanofibers is not particularly limited, but is preferably 4° C. or higher and 100° C. or lower when water is used as the solvent.
[0486] (Step ic: Step of preparing a cellulose nanofiber dispersion liquid carrying metal fine particles)
[0487] In step ic of the method for supporting metal fine particles on cellulose nanofibers, metal ions in a metal salt and a cellulose nanofiber-containing liquid are reduced, metal fine particles are precipitated by reaction, and the shape is controlled to obtain cellulose nanofibers supporting metal fine particles of a desired shape.
[0488] The method for reducing the metal ions in the metal salt and cellulose nanofiber-containing liquid is not particularly limited, and a known method can be used. For example, a method using a reducing agent, ultraviolet rays, electron beams, immersion plasma, etc. can be used. As a reducing agent for reducing the metal ions, a known reducing agent can be used.
[0489] Examples of the reducing agent include metal hydride, borohydride, borane, silane, hydrazine, and hydrazide reducing agents. Generally, in the liquid phase reduction method, sodium borohydride, dimethylamine borane, sodium citrate, ascorbic acid, alkali metal salts of ascorbic acid, hydrazine, and the like can be used as the reducing agent.
[0490] The amount of reducing agent added to the liquid containing metal salt and cellulose nanofibers (concentration of reducing agent) is not particularly limited, but is preferably equal to or higher than the concentration of the metal salt in the liquid containing metal salt and cellulose nanofibers, more preferably 0.002 mmol / L to 2000 mmol / L.
[0491] When the concentration of the reducing agent in the liquid containing the metal salt and cellulose nanofibers is lower than the concentration of the metal salt in the liquid containing the metal salt and cellulose nanofibers, unreduced metal ions remain in the liquid containing the metal salt and cellulose nanofibers.
[0492] When a reducing agent is used to reduce metal ions in a liquid containing metal salt and cellulose nanofibers, the method of adding the reducing agent is not particularly limited, but the reducing agent may be dissolved or dispersed in a solvent such as water in advance, and then the solution or dispersion may be added to the liquid containing metal salt and cellulose nanofibers.
[0493] The rate of adding the reducing agent to the metal salt and the cellulose nanofiber-containing liquid is not particularly limited, but the reducing agent is preferably added by a method that allows the reduction reaction to proceed uniformly.
[0494] It should be noted that the method for supporting metal fine particles on cellulose nanofibers is not particularly limited, but preferably includes at least the above-mentioned step ia, step ib, and step ic. Other steps may be inserted between the steps.
[0495] As required, at least a portion of the surface of the metal particles can be coated with a semiconductor or metal and its metal oxide. The semiconductor or metal and its oxide used for coating are not particularly limited, but for example, metals such as gold, silver, copper, aluminum, iron, platinum, zinc, palladium, ruthenium, iridium, rhodium, osmium, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, aluminum, metal salts, metal complexes and their alloys or oxides, composite oxides, silicon dioxide, etc. can be listed. In particular, from the viewpoint of stability and versatility, it is preferred to coat gold and silicon dioxide.
[0496] If necessary, the cellulose nanofibers loaded with the functional material may be washed by filtration, centrifugal separation or the like to remove free functional material.
[0497] (Step 2-iv)
[0498] Step 2-iv is to prepare the microfiber (in the manufacturing method III, as Figure 5 As shown, the microfiber 3B loaded with the functional material 40; in the manufacturing method IV, as Figure 6 As shown, in a dispersion of fine fibers 3A not carrying a functional material 40, the surface of a liquid droplet including a core material is covered with the fine fibers to stabilize the dispersion as an emulsion.
[0499] Specifically, in the production method III, the dispersion of fine fibers 3B loaded with a functional material obtained in the step 2-iii ( Figure 5In the manufacturing method IV, in the first step obtained in the dispersion of fine fibers 3A ( Figure 6 In the dispersion 11A), a core material-containing liquid is added so that the core material is dispersed in the dispersion in the form of droplets 6A, and the surface of the droplets 6A is covered with fine fibers to produce an O / W type emulsion stabilized by fine fibers. It should be noted that in the following description, the O / W type emulsion stabilized by fine fibers is sometimes referred to as an "emulsion".
[0500] The method for preparing the O / W emulsion is not particularly limited, and the method exemplified in the first embodiment can be adopted.
[0501] By ultrasonic treatment, the droplets containing the core material are dispersed in the dispersion of the microfibers to be emulsified, and the microfibers are selectively adsorbed at the liquid / liquid interface between the droplets and the microfiber dispersion, so that the droplets are covered by the microfibers, forming a structure that is stable as an O / W type emulsion. In this way, an emulsion that becomes stable by adsorbing solids at the liquid / liquid interface is academically called a "Pickering emulsion."
[0502] As described above, the mechanism of formation of Pickering emulsion by microfibers is still uncertain, but it is believed that since cellulose has hydrophilic sites derived from hydroxyl groups and hydrophobic sites derived from hydrocarbon groups in its molecular structure, it exhibits amphiphilicity, and therefore, cellulose is adsorbed at the liquid / liquid interface between the hydrophobic monomer and the hydrophilic solvent due to its amphiphilicity.
[0503] The structure of the O / W emulsion can be confirmed by optical microscopic observation. The particle size of the O / W emulsion is not particularly limited, but the average particle size is preferably 0.1 μm or more and 1000 μm or less. The average particle size can be calculated by randomly measuring the diameters of 100 emulsions and taking the average value.
[0504] In the O / W type emulsion structure, the thickness of the coating layer of the fine fibers formed on the surface of the droplet containing the core material is not particularly limited, but is preferably 3 nm or more and 1000 nm or less. Although not particularly limited, the particle size in the emulsion structure is the same as the particle size of the personal care particles obtained in step 3-ii. The thickness of the coating layer can be measured, for example, by using a cryo-TEM.
[0505] The weight ratio of the fine fiber dispersion to the core material used in step 2-iv is not particularly limited, but the polymerizable monomer is preferably 1 part by mass or more and 50 parts by mass or less relative to 100 parts by mass of the fine fibers. When the polymerizable monomer is less than 1 part by mass, the yield of the personal care particles decreases, which is not preferred, and when it exceeds 50 parts by mass, it is difficult to evenly cover the droplets with the fine fibers, which is not preferred.
[0506] The core material containing liquid used can form an O / W emulsion as long as it contains a core material. In order to stably form an O / W emulsion, it is preferably hydrophobic. In addition, the core material is a material that is solidified to form core particles 2A through chemical changes or physicochemical changes. The core material is not particularly limited, but is not particularly limited as long as it can stably form droplets. As the core material, for example, a polymerizable monomer (monomer), a molten polymer, a soluble polymer can be used.
[0507] The polymerizable monomer used in the step 2-iv is not particularly limited, and the monomers exemplified as the polymerizable monomer used in the step 2-i of the first embodiment can be used.
[0508] Furthermore, the polymerization initiator exemplified in the first embodiment may be added to the polymerizable monomer.
[0509] If a core material containing liquid containing a polymerizable monomer and a polymerization initiator is used in step 2-iv, the droplets of the O / W type emulsion in the later step 3-ii contain a polymerization initiator, so when the monomers inside the droplets of the emulsion are polymerized in the later step 3-ii, the polymerization reaction proceeds easily.
[0510] The weight ratio of the polymerizable monomer to the polymerization initiator used in step 2-iv is not particularly limited, but generally, the polymerization initiator is preferably 0.1 parts by mass or more relative to 100 parts by mass of the polymerizable monomer. When the polymerization initiator is less than 0.1 parts by mass, the polymerization reaction cannot be fully carried out, and the yield of the personal care particles is reduced, which is not preferred.
[0511] The core material containing liquid may also contain a solvent. Although not particularly limited, in order to stabilize the emulsion in step 2-iv, an organic solvent is preferably used. For example, toluene, xylene, ethyl acetate, butyl acetate, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), isophorone, cellosolve acetate, isophorone, Solvesso 100, trichloroethylene, hexane, chloroform, dichloromethane, dichloroethane, isooctane, nonane, etc. can be used.
[0512] The weight ratio of the polymerizable monomer to the solvent used in step 2-iv is not particularly limited, but the amount of the solvent is preferably 80 parts by mass or less relative to 100 parts by mass of the polymerizable monomer.
[0513] As the polymer for obtaining the soluble polymer, the polymers exemplified in the first embodiment can be used.
[0514] As a method for obtaining a molten polymer by melting a polymer, the method exemplified in the first embodiment can be adopted. In addition, as a polymer used for the molten polymer, the polymer exemplified in the first embodiment can be used.
[0515] In addition, the droplets containing the core material may contain functional components other than the polymerization initiator in advance. Specifically, the functional components include: colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoamers, antistatic agents, adhesives, bleaching agents, chelating agents, deodorants, fragrances, fragrances, anti-dandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials headed by fats or waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), enzymes, etc.
[0516] When the polymerizable monomer contains functional components other than the polymerization initiator in advance, the functional components can be contained inside the core particles when the particles are formed into personal care particles, thereby being able to exhibit functions suitable for the intended use.
[0517] Preferably, the functional component is easily dissolved or dispersed in the droplets but is difficult to be dissolved or dispersed in the hydrophilic solvent. By dissolving or dispersing in the droplets, when forming an O / W type emulsion, the functional component is easily encapsulated in the droplets of the emulsion, thereby effectively obtaining personal care particles encapsulated with the functional component. In addition, the amount of the encapsulated functional component can be increased.
[0518] In addition, as the core material, a polymerizable monomer, a soluble polymer, and a molten polymer can be used together to form droplets and emulsify. In addition, when a biodegradable polymer (resin) is selected as the polymer type of the core particle of the personal care particles, since the obtained personal care particles are composed of core particles composed of biodegradable polymers and fine fibers, they become particles with high environmental friendliness of biodegradable materials.
[0519] (Step 3-ii)
[0520] Step 3-ii is to solidify the core material inside the droplet to obtain a core particle with fine fibers (such as in the production method III) coated on the surface. Figure 5 As shown, the microfiber 3B loaded with the functional material 40; in the manufacturing method IV, as Figure 6 As shown, the process of preparing a dispersion liquid of particles of fine fibers 3A) not carrying the functional material 40.
[0521] There is no particular limitation on the method for solidifying the core material. When a polymerizable monomer is used as the core material, it can be solidified by polymerizing the polymerizable monomer to form a polymer. When a soluble polymer is used as the core material, the polymer can be solidified by diffusing the solvent inside the droplet into a hydrophilic solvent or by evaporating the solvent to remove the solvent. When a molten polymer is used as the core material, it can be solidified by cooling and solidifying the molten polymer.
[0522] For example, the core material is solidified by heating while stirring an O / W emulsion to polymerize the polymerizable monomer, wherein the O / W emulsion is stabilized by being coated with fine fibers by droplets made by the 2-iv step and containing the polymerizable monomer as the core material and the polymerization initiator. The stirring method is not particularly limited, and a known method can be used, specifically, a disperser or a stirrer can be used. In addition, it is also possible to perform heat treatment only without stirring.
[0523] In addition, the temperature conditions during heating can be appropriately set according to the type of polymerizable monomer and the type of polymerization initiator, but it is preferably above 20°C and below 150°C. When it is less than 20°C, the polymerization reaction rate decreases, so it is not preferred. When it exceeds 150°C, the fine fibers may be modified, so it is not preferred. The time required for the polymerization reaction can be appropriately set according to the type of polymerizable monomer and the type of polymerization initiator, but it is usually about 1 hour to 24 hours. In addition, the polymerization reaction can also be carried out by ultraviolet irradiation treatment, which is a kind of electromagnetic wave. In addition, in addition to electromagnetic waves, particle beams such as electron beams can also be used.
[0524] As a method for evaporating the solvent of the soluble polymer, specifically, a method of evaporating and removing the solvent by heating and / or drying under reduced pressure can be cited. When an organic solvent having a lower boiling point than water is used, the organic solvent can be selectively removed. Although not particularly limited, the solvent can be effectively removed by heating under reduced pressure. The heating temperature is preferably 20° C. to 100° C., and the pressure is preferably 600 mmHg to 750 mmHg.
[0525] As a method for diffusing the solvent of the soluble polymer, specifically, a method of diffusing the solvent inside the droplets by further adding a solvent or a salt to the above-mentioned O / W type emulsion can be cited. By diffusing a solvent with low solubility in the hydrophilic solvent into the hydrophilic solvent phase over time, the soluble polymer can be precipitated and solidified in the form of particles.
[0526] As a method for solidifying the molten polymer, there is a method of cooling the above-mentioned O / W type emulsion.
[0527] Through the above steps, particles in which the core particles are covered with fine fibers can be obtained (in the production method III, Figure 5 (d) the personal care particles 1A shown; in the manufacturing method IV, Figure 6 (c) is a dispersion of particles 10A) coated with fine fibers.
[0528] It should be noted that in the manufacturing method III, a state is such that just after the personal care particles 1A are generated, a large amount of water and free fine fibers that do not contribute to the formation of the coating layer are mixed in the dispersion of the personal care particles 1A. Therefore, it is necessary to recycle / clean the personal care particles 1A. In addition, in the manufacturing method IV, a state is such that just after the particles 10A covered with fine fibers are generated, a large amount of water and free fine fibers that do not contribute to the formation of the coating layer are mixed in the dispersion of the particles 10A. Therefore, it is necessary to recycle / clean the particles 10A.
[0529] As a recovery / cleaning method, washing by centrifugation or washing by filtration is preferred. In addition, the residual solvent may be removed.
[0530] As a washing method using centrifugal separation, a known method can be used. Specifically, the personal care particles 1A or particles 10A are repeatedly precipitated by centrifugal separation, the supernatant is removed, and the particles are redispersed in a mixed solvent of water / methanol, and the residual solvent is removed from the precipitate obtained by the final centrifugal separation, thereby recovering the personal care particles 1A or particles 10A. For filtration washing, a known method can also be used, for example, a PTFE membrane filter with a pore size of 0.1 μm is used and water and methanol are repeatedly filtered, and the residual solvent is further removed from the slurry finally remaining on the membrane filter, thereby recovering the personal care particles 1A or particles 10A.
[0531] The method for removing the residual solvent is not particularly limited, and the method may be air-drying or heat-drying in an oven. The dry solid material including the personal care particles 1A thus obtained is not in the form of a film or aggregate as described above, but is obtained in the form of a fine powder.
[0532] (5th step)
[0533] In the manufacturing method IV, the fifth step is Figure 6 (c) is a step of supporting the functional material 40 on the fine fibers 3A on the surface of the particles 10A in the dispersion of the particles 10A covered with the fine fibers 3A.
[0534] There is no particular limitation on the method for loading the functional material on the fine fibers 3A on the surface of the particle 10A, and a known method can be used. For example, the following method can be used: the particles coated with fine fibers are dispersed in a hydrophilic solvent such as water or alcohol to prepare a dispersion of the particles, and the functional material is added and mixed in the dispersion to make it adhere. In addition, the functional material can be loaded on the particles coated with fine fibers by synthesizing the functional material in the dispersion of the particles coated with fine fibers.
[0535] Here, as described above, when the functional material is loaded on the particles coated with fine fibers, it is preferred to introduce anionic functional groups on the crystal surface of the fine fibers in advance. By adding and mixing cationic functional materials in the dispersion of the particles coated with fine fibers having anionic functional groups, the functional material can be stably loaded on the fine fibers on the surface of the particles coated with fine fibers. In addition, by adjusting the pH of the dispersion of the particles coated with fine fibers, the loading or detachment of the functional material can be controlled.
[0536] The concentration of the particles coated with fine fibers in the dispersion used when loading the functional material is not particularly limited, but is preferably 0.1% by mass to 50% by mass, and more preferably 0.5% by mass to 20% by mass. When the concentration is less than 0.1%, it is difficult to effectively load the functional material. When the concentration exceeds 50% by mass, the dispersibility of the particles coated with fine fibers deteriorates, making it difficult to react uniformly.
[0537] The solvent of the dispersion of the particles coated with fine fibers is not particularly limited, but a hydrophilic solvent is preferred.
[0538] The hydrophilic solvent is not particularly limited, but is preferably water; alcohols such as methanol, ethanol, and isopropanol; and cyclic ethers such as tetrahydrofuran.
[0539] It is particularly preferred that 50% by mass or more of water is contained. When the proportion of water in the suspension is less than 50% by mass, the dispersibility of the particles coated with fine fibers may deteriorate. In addition, as a solvent contained other than water, the above-mentioned hydrophilic solvent is preferred.
[0540] If necessary, the pH of the suspension may be adjusted to improve the dispersibility of the particles coated with fine fibers. Examples of alkaline aqueous solutions used for pH adjustment include organic bases such as sodium hydroxide aqueous solution, lithium hydroxide aqueous solution, potassium hydroxide aqueous solution, ammonia aqueous solution, tetramethylammonium hydroxide aqueous solution, tetraethylammonium hydroxide aqueous solution, tetrabutylammonium hydroxide aqueous solution, and benzyltrimethylammonium hydroxide aqueous solution. In terms of cost, sodium hydroxide aqueous solution is preferred.
[0541] The method for loading metal microparticles as functional materials on particles covered with fine fibers using cellulose nanofibers having anionic functional groups as fine fibers is not particularly limited, but can be produced, for example, by the following method. The method sequentially includes steps iia, iib, and iic.
[0542] Step iia: a cellulose nanofiber-covered particle dispersion preparation step of preparing a dispersion containing at least one type of cellulose nanofiber-covered particles.
[0543] Step iib: a step of preparing a liquid containing a metal salt and cellulose nanofiber-covered particles, in which a dispersion liquid containing at least one metal salt and at least one cellulose nanofiber-covered particles is prepared.
[0544] Step iic: a step of preparing a dispersion of cellulose nanofiber-covered particles carrying metal fine particles, wherein the metal ions in the liquid containing the metal salt and cellulose nanofiber-covered particles are reduced to prepare a reaction liquid.
[0545] (Step iia: Cellulose Nanofiber-Coated Particle Dispersion Liquid Preparation Step)
[0546] In step iia of the method for supporting metal fine particles on cellulose nanofiber-coated particles, at least one dispersion of cellulose nanofiber-coated particles is prepared.
[0547] First, a dispersion of cellulose nanofiber-coated particles is prepared. The solid content concentration of the dispersion of cellulose nanofiber-coated particles is not particularly limited, but is preferably 0.1% by mass to 50% by mass, and more preferably 0.5% by mass to 20% by mass.
[0548] When the solid content concentration of the dispersion of the cellulose nanofiber coated particles is less than 0.1% by mass, it is difficult to control the particle size of the metal particles. On the other hand, when the solid content concentration of the dispersion of the cellulose nanofiber coated particles exceeds 50% by mass, the dispersibility of the cellulose nanofiber coated particles deteriorates, and it is difficult to uniformly mix the metal salt and the cellulose nanofiber coated particles in step iib (metal salt and cellulose nanofiber containing liquid preparation step), and further in step iic (cellulose nanofiber coated particle dispersion preparation step loaded with metal particles), the reduction reaction cannot be uniformly performed.
[0549] The solvent and pH for dispersing the cellulose nanofiber-coated particles are the same as those in step ia.
[0550] (Step iib: Step of Preparing a Liquid Containing a Metal Salt and Cellulose Nanofiber-Coated Particles)
[0551] In step iib of the method for supporting metal fine particles on cellulose nanofiber-covered particles, a dispersion containing at least one metal salt and at least one cellulose nanofiber-covered particles is prepared.
[0552] The method for preparing a dispersion containing at least one metal salt and at least one cellulose nanofiber coated particle is not particularly limited. For example, at least one cellulose nanofiber coated particle dispersion and a solution containing at least one metal salt (metal salt containing solution) are prepared, and the metal salt containing solution is added to the cellulose nanofiber coated particle dispersion while stirring the cellulose nanofiber coated particle dispersion to prepare. In addition, a solid metal salt can be directly added to the dispersion of the cellulose nanofiber coated particles, or a dispersion of the cellulose nanofiber coated particles can be added to the metal salt containing solution.
[0553] The metal salt and the metal salt-containing liquid can be prepared in the same manner as in step ib.
[0554] The concentration of the metal salt in the dispersion of the metal salt and the cellulose nanofiber coated particles is not particularly limited, but is preferably 0.002 mmol / L or more and 20.0 mmol / L or less. In particular, when using cellulose nanofiber coated particles having anionic functional groups, since the metal ions are coordinated with the anionic functional groups, it is preferred to prepare the particles in such a manner that the concentration of the metal salt (the concentration of the metal ions) is less than the amount of the anionic functional groups. When the concentration of the metal salt (the concentration of the metal ions) exceeds the amount of the anionic functional groups of the cellulose nanofiber coated particles, the cellulose nanofiber coated particles may aggregate.
[0555] The solvent used in the liquid containing the metal salt and the cellulose nanofiber-covered particles can be the same as that used in step 2-iii.
[0556] The solid content concentration of the cellulose nanofiber-covered particles in the dispersion of the metal salt and the cellulose nanofiber-covered particles is not particularly limited, but is preferably 0.1 mass % to 50 mass %, and more preferably 0.1 mass % to 20 mass %.
[0557] When the solid content concentration of the cellulose nanofiber coated particles is less than 0.1% by mass, it is difficult to control the particle size of the metal particles. On the other hand, when the solid content concentration of the cellulose nanofiber coated particles exceeds 50% by mass, the dispersibility of the cellulose nanofiber coated particles deteriorates, and it is difficult to uniformly mix the metal salt and the cellulose nanofiber coated particles in step iib, and further, the reduction reaction cannot be uniformly performed in step iic.
[0558] As the solvent of the liquid containing the metal salt and the cellulose nanofiber-covered particles, the same solvent as in step ib can be used. The pH and temperature can also be the same as in step 2-iii.
[0559] (Step iic: Step of preparing a dispersion of cellulose nanofiber-coated particles carrying metal fine particles)
[0560] In step iic of the method for loading metal microparticles on cellulose nanofiber-coated particles, metal ions in a liquid containing metal salt and cellulose nanofiber-coated particles are reduced to generate a reaction liquid, and metal microparticles are precipitated while controlling their shape, thereby obtaining cellulose nanofiber-coated particles loaded with metal microparticles.
[0561] The method for reducing the metal ions in the liquid containing the metal salt and the cellulose nanofiber-covered particles can be the same method as in step ic, and the same reducing agent can be used.
[0562] The amount of reducing agent added to the liquid containing metal salt and cellulose nanofiber coated particles (concentration of reducing agent) is not specifically limited, but is preferably equal to or higher than the concentration of metal salt in the liquid containing metal salt and cellulose nanofiber coated particles, and more preferably is above 0.002 mmol / L and below 2000 mmol / L.
[0563] When the concentration of the reducing agent in the liquid containing the metal salt and the cellulose nanofiber-covered particles is lower than the concentration of the metal salt in the liquid containing the metal salt and the cellulose nanofiber-covered particles, unreduced metal ions remain in the liquid containing the metal salt and the cellulose nanofiber-covered particles.
[0564] When a reducing agent is used to reduce metal ions in a liquid containing metal salts and cellulose nanofiber-coated particles, the method of adding the reducing agent is not particularly limited, but the reducing agent can be pre-dissolved or dispersed in a solvent such as water, and then the solution or dispersion can be added to the liquid containing metal salts and cellulose nanofiber-coated particles.
[0565] The rate of adding the reducing agent to the liquid containing the metal salt and the cellulose nanofiber-covered particles is not particularly limited, but it is preferably added by a method that allows the reduction reaction to proceed uniformly.
[0566] The method for supporting metal fine particles on the cellulose nanofiber-coated particles is not particularly limited, but preferably includes at least the above-mentioned step iia, step iib, and step iic. Other steps may be inserted between the steps.
[0567] As required, at least a portion of the surface of the metal particles can be coated with a semiconductor or metal and its metal oxide. The semiconductor or metal and its oxide used for coating are not particularly limited, but for example, metals such as gold, silver, copper, aluminum, iron, platinum, zinc, palladium, ruthenium, iridium, rhodium, osmium, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, aluminum, metal salts, metal complexes and their alloys or oxides, composite oxides, silicon dioxide, etc. can be listed. In particular, from the viewpoint of stability and versatility, it is preferred to coat gold and silicon dioxide.
[0568] If necessary, the cellulose nanofiber-coated particles carrying the functional material may be washed by filtration, centrifugal separation or the like to remove free functional material.
[0569] In addition, unless otherwise stated, in the fifth step, cellulose nanofiber-coated particles may be used instead of the cellulose nanofibers in the second-iii step, and the same conditions may be applied.
[0570] The dry powder of the personal care particles of this embodiment can be mixed or dispersed in other cosmetic raw materials to be used in personal care products such as cosmetic products. In addition, the personal care particles can be dispersed in a solvent containing cosmetic raw materials and the like to be used as a personal care composition.
[0571] Examples of cosmetic raw materials include colorants, oil absorbents, sunscreens (ultraviolet absorbers, ultraviolet scatterers, etc.), antibacterial agents, antioxidants, antiperspirants, defoaming agents, antistatic agents, adhesives, bleaching agents, chelating agents, deodorant ingredients, fragrances, flavors, antidandruff active substances, skin softeners, insect repellents, preservatives, natural extracts, beauty ingredients, pH adjusters, vitamins, amino acids, hormones, oily raw materials such as fats and waxes, surfactants, inorganic particles (titanium oxide, silica, clay, etc.), etc.
[0572] (Effects of personal care particles)
[0573] According to one embodiment of the personal care particles of the present invention, there is provided a novel personal care particle having fine fibers which solves the problem of excessive solvent in fine fibers such as cellulose nanofibers and chitin nanofibers and can be produced by a simple method.
[0574] Furthermore, by coating the fine fibers with high safety, high hydrophilicity and high specific surface area, the particles do not aggregate with each other, thereby providing personal care particles with good smoothness and skin affinity and excellent moisturizing properties.
[0575] In addition, since the functional material is loaded on fine fibers with a high specific surface area, the dispersion stability of the functional material is maintained, thereby providing personal care particles that can effectively exert the functions of functional materials such as UV protection (absorption and / or scattering), color development, and antibacterial.
[0576] The cellulose nanofibers or chitin nanofibers are composed of cellulose or chitin / chitosan, which are biodegradable polymers. Therefore, the core particles are also composed of a material containing a biodegradable polymer, thereby providing personal care particles with reduced environmental load.
[0577] Although the embodiments of the present invention are described in detail above, the specific configuration is not limited to the present embodiment, and may also include design changes within the scope of the present invention. In addition, it is possible to appropriately combine the constituent elements shown in the above embodiments. For example, other components other than polymers and functional components may also be contained in the core particles.
[0578] Example
[0579] Hereinafter, the present invention will be described in detail based on examples, but the technical scope of the present invention is not limited to these examples. In the following examples, "%" means mass % (w / w %) unless otherwise specified.
[0580] [Examples 1 to 11, Comparative Examples 1 to 6]
[0581] <Example 1>
[0582] (First step: step of obtaining a cellulose nanofiber dispersion)
[0583] {TEMPO Oxidation of Wood Cellulose}
[0584] 70 g of softwood kraft pulp was suspended in 3500 g of distilled water, and a solution obtained by dissolving 0.7 g of TEMPO and 7 g of sodium bromide in 350 g of distilled water was added, and then cooled to 20°C. 450 g of a 2 mol / L sodium hypochlorite aqueous solution with a density of 1.15 g / mL was added dropwise thereto to start the oxidation reaction. The temperature in the system was kept constant at 20°C, and a 0.5 N sodium hydroxide aqueous solution was added as the pH decreased during the reaction so that the pH continued to be maintained at 10. When the total amount of sodium hydroxide added reached 3.0 mmol / g relative to the weight of cellulose, about 100 mL of ethanol was added to stop the reaction. Subsequently, a glass filter was used and the filtration and washing were repeated with distilled water to obtain an oxidized pulp (oxidized cellulose).
[0585] {Determination of the amount of carboxyl groups in oxidized cellulose}
[0586] The oxidized pulp and reoxidized pulp obtained by TEMPO oxidation were dispersed in water at a concentration of 1% with a solid content of 0.1 g, and hydrochloric acid was added to adjust the pH to 2.5. Then, the carboxyl group content (mmol / g) was determined by conductometric titration using a 0.5 M sodium hydroxide aqueous solution.
[0587] {Fibrillation of oxidized cellulose and preparation of aqueous dispersion}
[0588] 0.5 g of the oxidized cellulose obtained by TEMPO oxidation was dispersed in 99.5 g of distilled water and subjected to a micronization treatment using a juicer mixer for 30 minutes to obtain a cellulose nanofiber aqueous dispersion having a concentration of 0.5%. This was used as a continuous phase.
[0589] {Evaluation of cellulose nanofibers}
[0590] As described below, the carboxyl group content, crystallinity, number average diameter of the major axis, light transmittance, and rheology of the obtained oxidized cellulose and cellulose nanofibers were measured and calculated.
[0591] {Determination of the amount of carboxyl groups}
[0592] The carboxyl group content of the oxidized cellulose before the dispersion treatment was calculated by the following method.
[0593] In a beaker, 0.2 g of oxidized cellulose was weighed in terms of dry weight, and 80 mL of ion exchange water was added. 5 mL of 0.01 mol / L sodium chloride aqueous solution was added thereto, and 0.1 mol / L hydrochloric acid was added while stirring to adjust the overall pH to 2.8. An automatic titrator (trade name: AUT-701, manufactured by "Toadie Keke" Co., Ltd.) was used to drip 0.1 mol / L sodium hydroxide aqueous solution at 0.05 mL / 30 seconds, and the conductivity and pH value were measured every 30 seconds, and the measurement was continued until the pH reached 11. Based on the obtained conductivity curve, the titration amount of sodium hydroxide was determined, thereby calculating the content of carboxyl groups. The results are shown in Table 1.
[0594] {Calculation of crystallinity}
[0595] The crystallinity of TEMPO-oxidized cellulose was calculated by the following method.
[0596] For TEMPO-oxidized cellulose, an X-ray diffraction pattern was measured in the range of 5°≤2θ≤35° using a sample horizontal multifunctional X-ray diffractometer (trade name: Ultima III, manufactured by Rigaku Corporation) under the conditions of X-ray output: (40 kV, 40 mA). Since the obtained X-ray diffraction pattern is derived from the cellulose I-type crystal structure, the crystallinity of TEMPO-oxidized cellulose was calculated using the following formula (2) and the method shown below. The results are shown in Table 1.
[0597] Crystallinity (%) = [(I22.6-I18.5) / I22.6] × 100 (2)
[0598] Here, I22.6 represents the diffraction intensity of the grating plane (002 plane) (diffraction angle 2θ=22.6°) in X-ray diffraction, and I18.5 represents the diffraction intensity of the amorphous part (diffraction angle 2θ=18.5°).
[0599] {Calculation of the number average diameters of the major and minor axes of cellulose nanofibers}
[0600] Using an atomic force microscope, the number average diameters of the major axis and the minor axis of the cellulose nanofibers were calculated by the following method.
[0601] First, a 0.5% cellulose nanofiber aqueous dispersion was diluted to 0.001%, and 20 μL was dripped onto a mica plate and air-dried. After drying, an atomic force microscope (trade name: AFM5400L, manufactured by Hitachi High-Tech Norodomics) was used to observe the shape of the cellulose nanofibers in DFM mode.
[0602] The long axis diameter (maximum diameter) of 100 fibers was measured according to the observation image of atomic force microscopy, and the average value was taken to obtain the number average diameter of the long axis of cellulose nanofibers. The short axis diameter (minimum diameter) of 100 fibers was measured according to the observation image of atomic force microscopy, and the average value was taken to obtain the number average diameter of the short axis of cellulose nanofibers. The results are shown in Table 1.
[0603] {Measurement of light transmittance of cellulose nanofiber aqueous dispersion}
[0604] The light transmittance of a cellulose nanofiber aqueous dispersion having a concentration of 0.5% by mass was measured by the following method.
[0605] Water was added to one quartz sample cell as a reference, and a cellulose nanofiber aqueous dispersion was added to another cell without mixing bubbles. The transmittance from wavelength 220nm to 800nm in an optical path length of 1cm was measured using a spectrophotometer (trade name: NRS-100, manufactured by JASCO Corporation). The results are shown in Table 1. Figure 7shown.
[0606] {Rheological determination}
[0607] The rheology of a cellulose nanofiber aqueous dispersion with a concentration of 0.5% by mass was studied by using a rheometer for steady-state viscoelasticity measurement. Specifically, the measurement was performed using a rheometer (trade name: AR 2000ex, manufactured by Thermo Instruments) with a cone plate having an inclination angle of 1°. The measurement section was set to 25°C and the rheology was measured at 0.01 s -1 Up to 1000s -1 The shear viscosity is measured continuously at a shear rate of Figure 8 As shown. The shear rate is 10s -1 and 100s -1 The shear viscosity at 100 °C is shown in Table 1.
[0608] [Table 1]
[0609]
[0610] As shown in Table 1, the cellulose nanofibers (TEMPO-oxidized CNF) contained in the cellulose nanofiber aqueous dispersion had a number average minor axis diameter of 3 nm and a number average major axis diameter of 831 nm.
[0611] In addition, from Figure 7 It can be clearly seen that the cellulose nanofiber aqueous dispersion exhibits high transparency. Figure 8 It can be clearly seen that the cellulose nanofiber dispersion exhibits thixotropy.
[0612] (Step 2-i: Step of preparing O / W type emulsion)
[0613] Next, 5 g of n-heptane, a non-polymerizable solvent, as a pore-forming agent, and 1 g of 2,2-azobis-2,4-dimethylvaleronitrile (hereinafter referred to as ADVN) as a polymerization initiator were dissolved in 5 g of divinylbenzene (hereinafter referred to as DVB) as a polymerizable monomer to prepare a polymerizable monomer mixed solution. This was used as a dispersed phase. In the polymerizable monomer mixed solution, the content of the non-polymerizable solvent as a pore-forming agent was 50% by mass relative to the total mass of the polymerizable monomer (DVB) as a core material and the non-polymerizable solvent as a pore-forming agent.
[0614] When the entirety of the obtained polymerizable monomer mixed solution was added to 40 g of the cellulose nanofiber aqueous dispersion obtained in the first step, the polymerizable monomer mixed solution and the cellulose nanofiber aqueous dispersion were separated into separate phases (two phases).
[0615] Next, the shaft of the ultrasonic homogenizer was inserted from the liquid surface of the upper phase in the mixed solution in the state of separation into two phases, and the ultrasonic homogenizer treatment was performed for 3 minutes under the conditions of frequency 24kHz and power 400W. The appearance of the mixed solution after the ultrasonic homogenizer treatment was in the form of a turbid emulsion. A drop of the mixed solution was dropped on a slide, covered with a cover glass and observed with an optical microscope, and then it was confirmed that countless emulsion droplets of about several μm were generated, and the O / W type emulsion with the cellulose nanofiber aqueous dispersion as the continuous phase and the polymerizable monomer mixed solution as the dispersed phase had dispersion stability.
[0616] (Step 3-i: Step of solidifying the core material)
[0617] The O / W type emulsion dispersion was placed in a hot water bath at 70°C using a water bath, and treated for 8 hours while being stirred by a stirrer to perform a polymerization reaction. After the treatment for 8 hours, the dispersion was cooled to room temperature. The appearance of the dispersion did not change before and after the polymerization reaction.
[0618] (Step 4: Step of recovering, washing and removing the pore-forming agent)
[0619] The obtained dispersion was placed in a centrifugal separator and treated at a centrifugal force of 75,000 g for 5 minutes to obtain a precipitate. The supernatant was removed by decantation to recover the precipitate, which was then washed twice alternately with pure water and methanol using a PTFE membrane filter having a pore size of 0.1 μm.
[0620] The thus obtained washed / recovered product was redispersed at a concentration of 1%, and the particle size was evaluated using a particle size distribution meter (NANOTRAC UPA-EX150, "Nikkiso Co., Ltd."). Next, the washed / recovered product was air-dried and vacuum-dried at room temperature of 25°C for 24 hours to obtain a fine dry powder.
[0621] <Example 2>
[0622] In the step 2-i, a dry powder was obtained in the same manner as in Example 1 except that 7 g of DVB and 3 g of n-heptane were used.
[0623] <Example 3>
[0624] In the step 2-i, a dry powder was obtained in the same manner as in Example 1 except that 3 g of DVB and 7 g of n-heptane were used.
[0625] <Example 4>
[0626] In the step 2-i, a dry powder was obtained in the same manner as in Example 1 except that n-hexane was used instead of n-heptane.
[0627] <Example 5>
[0628] In step 2-i, a dry powder was obtained in the same manner as in Example 1 except that n-dodecane was used instead of n-heptane.
[0629] <Example 6>
[0630] In step 2-i of Example 1, 7 g of DVB was used, and 3 g of sorbitan monooleate (Span 80) as an oil-soluble surfactant was used instead of n-heptane, and distilled water as a continuous phase solvent was absorbed into the interior of the emulsion droplets to serve as a pore-forming agent. A dry powder was obtained in the same manner as in Example 1 except for this.
[0631] The amount of distilled water absorbed into the interior of the emulsion droplets is unknown, and therefore the content of distilled water as a pore former relative to the total mass of the polymerizable monomer (DVB) as a core material and distilled water as a pore former is unknown.
[0632] <Example 7>
[0633] In step 2-i, 1 mass % of acetylated CNF was dispersed in 7 g of DVB as a polymerizable monomer, and then 1 g of 2,2-azobis-2,4-dimethylvaleronitrile (hereinafter also referred to as ADVN) as a polymerization initiator was dissolved to prepare a polymerizable monomer mixed solution.
[0634] When 3 g of pure water as a pore former was added to the obtained polymerizable monomer mixed solution, the polymerizable monomer mixed solution and the distilled water were separated into respective phases (two phases). Then, ultrasonic homogenization was performed to prepare a W / O type emulsion. The ratio (content) of the pore former in the total mass of the polymerizable monomer (DVB) as the core material and the distilled water as the pore former was 30% by mass.
[0635] The entire amount of the obtained W / O type emulsion was added to 40 g of the cellulose nanofiber aqueous dispersion.
[0636] A dry powder was prepared in the same manner as in Example 1 except for the above-mentioned points.
[0637] <Example 8>
[0638] In Example 1, a dry powder was prepared in the same manner as in Example 1 except that a chitosan nanofiber (also referred to as chitosan NF) dispersion prepared according to Patent Document 6 cited as a prior art document was used instead of TEMPO-oxidized CNF.
[0639] <Example 9>
[0640] In Example 1, a CM-treated CNF dispersion obtained by carboxymethylation (hereinafter also referred to as CM-treatment) according to Patent Document 2 cited as a prior art document was used instead of TEMPO oxidation. Dry powder was prepared in the same manner as in Example 1 except for the above.
[0641] <Example 10>
[0642] In Example 1, a phosphated CNF dispersion obtained by phosphated treatment according to Non-Patent Document 1 cited as a prior art document was used instead of TEMPO oxidation. Dry powder was prepared in the same manner as in Example 1 except for the above.
[0643] <Example 11>
[0644] In step 2-i of Example 1, 10 g of a molten polymer obtained by heating 5 g of poly-ε-caprolactone (PCL, manufactured by Wako Junka) was used instead of DVB as a polymerizable monomer. A dry powder was prepared in the same manner as in Example 1 except for this.
[0645] <Comparative Example 1>
[0646] In Example 1, granules were produced by spray drying without performing Step 2-i and Step 3-i. Each step was performed in the same manner as in Example 1 except for the above.
[0647] <Comparative Example 2>
[0648] In step 2-i of Example 1, n-heptane as a non-polymerizable solvent was not added to 10 g of DVB as a polymerizable monomer. Each step was performed in the same manner as in Example 1 except for this.
[0649] <Comparative Example 3>
[0650] In Example 1, each step was performed in the same manner as in Example 1 except that a carboxymethyl cellulose (hereinafter also referred to as CMC) aqueous solution was used instead of the TEMPO-oxidized CNF dispersion.
[0651] <Comparative Example 4>
[0652] In step 2-i of Example 11, an aqueous solution obtained by dissolving 8 parts by mass of polyvinyl alcohol (PVA) and 0.5 parts by mass of polyglyceryl laurate-10 (PGLE ML10) in 500 g of pure water was added to the polymerizable monomer mixed solution instead of the cellulose nanofiber aqueous dispersion to prepare an emulsion dispersion. Other steps were performed in the same manner as in Example 11.
[0653] <Comparative Example 5>
[0654] In step 2-i of Example 11, each step was performed in the same manner as in Example 11 except that a CMC aqueous solution was added to the polymerizable monomer mixed solution instead of the TEMPO-oxidized CNF dispersion to prepare an emulsion dispersion.
[0655] <Comparative Example 6>
[0656] As a conventional example, commercially available styrene-divinylbenzene copolymer microbeads (particle size 4.5 μm, Technochemikar) were prepared.
[0657] <Evaluation Method>
[0658] (Evaluation of particle structure)
[0659] The obtained dry powders of each embodiment and comparative examples 1 to 5 and the prepared dry powder of comparative example 6 were observed using a scanning electron microscope. In addition, the obtained dry powder was embedded in a resin and the cross section was observed using an SEM. Based on these observations, the particle structure of each dry powder was evaluated. The evaluation was judged by "0" and "×" shown below.
[0660] ○: The inside of the particle has pores, and the surface of the particle is covered with fine fibers (cellulose nanofibers or chitin nanofibers).
[0661] ×: The above-mentioned particles were not obtained.
[0662] (Evaluation of true sphericity)
[0663] Each dry powder was placed in a particle shape image analyzer "PITA-04" of Seishin Corporation, and the average circularity was calculated based on the average circularity of more than 1,000 particles, and the true sphericity was evaluated based on the following evaluation criteria. It should be noted that when the image area of the particle is set to S and the perimeter is set to L, the calculation is performed using the formula "circularity = 4πS / L2".
[0664] ○: The average circularity is 0.6 or more.
[0665] ×: The average circularity is less than 0.6.
[0666] (Evaluation of oil absorption)
[0667] The oil absorption is measured by the method of JISK 5101-13-1. The powder is placed on the measuring plate and the refined linseed oil is gradually added by dropping 4 or 5 drops from the burette each time. Each time the refined linseed oil is added, a palette knife is used to knead the refined linseed oil into the sample. Repeat this operation until a block of the refined linseed oil and the sample can be formed. Then, the operation is repeated by dropping drop by drop and kneading thoroughly until the slurry has a smooth hardness.
[0668] The oil absorption was evaluated by judging by the following "○", "△", and "×".
[0669] ○: Oil absorption is 30 ml / 100 g or more.
[0670] △: The oil absorption is 20 ml / 100 g or more and less than 30 ml / 100 g.
[0671] ×: Oil absorption is less than 20 ml / 100 g.
[0672] (Evaluation of light diffusion)
[0673] The light diffusion property was evaluated by the following method using a spectral variable color difference meter GC5000 manufactured by Nippon Denshoku Industries. First, a glass plate containing each dry powder was placed on the GC5000, and the spectral reflectivity R1 when receiving incident light at an angle of -45° at a wavelength of 400nm to 700nm at a 0° angle, and the spectral reflectivity R2 when receiving incident light at an angle of -45° at a 45° angle. Then, based on the measurement results, the ratio of R1 to R2 at a wavelength of 600nm was calculated as the light diffusion index. The closer the light diffusion index is to 1, the lower the angle dependence and the higher the soft focus. The evaluation of light diffusion is judged by the following "0", "△", and "×".
[0674] ○: Light diffusion index is 0.9 or more.
[0675] △: The light diffusion index is 0.6 or more and less than 0.9.
[0676] ×: The light diffusion index is less than 0.6.
[0677] (Evaluation of Dispersibility)
[0678] The dry powder was added to pure water at a concentration of 1% by mass, and dispersed with a stirring bar for 24 hours, and the aggregation was visually confirmed. The evaluation was judged by the following "0" or "×".
[0679] ○: No aggregates were observed visually.
[0680] ×: Aggregates were visually observed.
[0681] (Evaluation of user experience)
[0682] In a room with a temperature of 20°C and a humidity of 40% RH, each dry powder of the embodiment and the comparative example was applied to the inner side of the lower arm of the test subject (female in her 30s). Specifically, 0.1 g of each dry powder was applied with fingers into a circle with a diameter of about 5 cm. The feeling of use when applied to the skin was judged by the following "0" and "×".
[0683] ○: Good affinity to the skin and little irritation to the skin.
[0684] ×: Poor affinity to skin and irritating to skin.
[0685] (Evaluation of Moisturizing Properties)
[0686] In a room with an air temperature of 20°C and a humidity of 40%RH, each dry powder of the embodiment and the comparative example was applied to the inner side of the lower arm of the subject (30-year-old female). Specifically, 0.1 g of each dry powder was applied with fingers into a circle with a diameter of about 5 cm. After 30 minutes after application, the moisture content of the skin where the dry powder was applied was measured using a moisture detector MY-707S (Skara Co., Ltd.). The evaluation was judged by the "○" and "×" shown below.
[0687] ○: The water content is 60% or more.
[0688] ×: The moisture content is less than 60%.
[0689] The evaluation results of the above Examples 1 to 11 and Comparative Examples 1 to 6 are summarized in Table 2 below. The emulsion stabilizer in Table 2 refers to cellulose nanofibers or emulsion stabilizers used to replace cellulose nanofibers. In addition, Table 2 shows the polymer constituting the core particles and the pore former used in the manufacturing method and its content (the ratio of the pore former to the total mass of the core material and the pore former). It should be noted that the manufacturing method used in Examples 1 to 11 is Figure 2 Manufacturing method I shown.
[0690] [Table 2]
[0691]
[0692] When the dry powder obtained in Example 1 was observed using a scanning electron microscope (SEM), it was confirmed that the polymerization reaction was carried out using the O / W type emulsion droplets as a template, and there were countless spherical particles of the shape derived from the emulsion droplets. In addition, it was confirmed that the surface was uniformly covered with cellulose nanofibers having a width of several nm. In addition, despite repeated cleaning by filtration and cleaning, the surface of the particles was still uniformly covered with cellulose nanofibers, indicating that the core particles were combined with the cellulose nanofibers and were in an inseparable state. In addition, it was confirmed that fine pores were formed on the surface of the particles.
[0693] Furthermore, when the dry powder obtained in Example 1 was embedded in a resin and the cross section was observed by SEM, it was confirmed that a large number of fine pores were present in the dry powder. That is, it was confirmed that the dry powder obtained in Example 1 was the composite particle of the first embodiment.
[0694] In addition, when the dry powder obtained in Example 1 was added to pure water at a concentration of 1% by mass and stirred for 24 hours with a stirrer for redispersion, it was easily redispersed, and no aggregation was observed by visual observation. In addition, when the particle size was evaluated using a particle size distribution meter, the average particle size was the same as before drying, and there was no signal indicating aggregation in the data of the particle size distribution meter.
[0695] The above shows that even if the surface of the dry powder (composite particles of the first embodiment) obtained in Example 1 is covered with cellulose nanofibers, it does not form a film during drying but is obtained as a powder and has good redispersibility.
[0696] Similarly, when the surfaces and cross sections of the dry powders obtained in Examples 2 to 11 were observed by SEM, it was confirmed that the particles constituting the dry powders were spherical composite particles having pores inside and fine fibers covering the surfaces.
[0697] Thus, it can be confirmed that by adopting manufacturing method I, regardless of the type of fine fiber (TEMPO oxidation CNF, CMized CNF, phosphated CNF, chitin NF), spherical composite particles having pores inside the core particles composed of various polymers such as polymers of various monomers or biodegradable polymers and covered with fine fibers on the surface can be prepared. In addition, it can be confirmed that regardless of the type of pore former and the amount of pore former added, spherical composite particles having pores inside the core particles and covered with fine fibers on the surface can be prepared.
[0698] In addition, similarly to Example 1, it was confirmed that the dry powders obtained in Examples 2 to 4, 6, 8 to 11 also had portions where the particle surfaces were covered with fine fibers and portions where pores were formed. In other words, it was confirmed that porous composite particles were obtained in Examples 1 to 4, 6, 8 to 11. The dry powders obtained in these examples had very high oil absorption and exhibited excellent light diffusivity.
[0699] In the dry powders obtained in Examples 5 and 7, no pores were observed on the particle surface, but by observing the cross section, it was confirmed that they were hollow composite particles. The dry powders obtained in these examples had relatively high oil absorption and exhibited excellent light diffusion.
[0700] All the dry powders obtained in Examples 1 to 11 have good redispersibility and exhibit excellent skin affinity and moisturizing properties.
[0701] Furthermore, by impregnating the dried powder (composite particles) obtained in Example 1 with a vitamin C derivative as a functional ingredient, personal care particles having a whitening component can be obtained.
[0702] On the other hand, the dry powders of Comparative Examples 1, 2, and 6 were neither porous particles nor hollow particles, and had poor oil absorption and light diffusion properties. In addition, the dry powders of Comparative Examples 3 to 5 were porous particles, and had good oil absorption properties, but were not spherical (low true sphericity), and had poor feel during use. In addition, since they were not coated with fine fibers, they had poor dispersibility and moisture retention properties.
[0703] [Examples 21 to 30, Comparative Examples 21 to 29]
[0704] <Example 21>
[0705] (First step: step of obtaining a cellulose nanofiber dispersion)
[0706] In the same manner as in the first step of Example 1, an aqueous dispersion of cellulose nanofibers having a concentration of 0.5% by mass was obtained.
[0707] (Step 2-iii: Step of loading functional materials)
[0708] {Step ia: Preparation of cellulose nanofiber dispersion}
[0709] 50 g of a 0.5 mass % aqueous dispersion of cellulose nanofibers was prepared.
[0710] {Step ib: Preparation of silver nitrate aqueous solution and cellulose nanofiber-containing solution}
[0711] A 100 mM silver (I) nitrate aqueous solution was prepared and 1.0 g of the 100 mM silver nitrate aqueous solution was added to 50 g of a 0.5 mass % aqueous dispersion of cellulose nanofibers while stirring with a stirring bar while maintaining a constant temperature (25° C.), and stirring was continued for 30 minutes.
[0712] {Process ic: Reduction precipitation}
[0713] Sodium borohydride was dissolved in distilled water to prepare a 100 mM sodium borohydride aqueous solution. While maintaining a constant temperature (25°C), 1.0 g of a 100 mM sodium borohydride aqueous solution was added to the silver nitrate aqueous solution and the cellulose nanofiber-containing solution using a stirring bar, and stirring was continued for 60 minutes to prepare a dispersion of cellulose nanofibers loaded with silver particles. The resulting dispersion exhibited a yellow color derived from the silver particles, indicating that silver particles were generated.
[0714] (Step 2-iv: Step of preparing O / W type emulsion)
[0715] Next, 1 g of 2,2-azobis-2,4-dimethylvaleronitrile (hereinafter also referred to as ADVN) as a polymerization initiator was dissolved in 10 g of divinylbenzene (hereinafter also referred to as DVB) as a polymerizable monomer. When the entirety of the resulting polymerizable monomer mixture was added to 40 g of the cellulose nanofiber dispersion loaded with silver particles, the polymerizable monomer mixture and the cellulose nanofiber dispersion were separated into respective phases (two phases).
[0716] Next, the shaft of the ultrasonic homogenizer was inserted from the liquid surface of the upper phase in the mixed solution in the state of separation into two phases, and the ultrasonic homogenizer treatment was performed for 3 minutes under the conditions of frequency 24kHz and power 400W. The appearance of the mixed solution after the ultrasonic homogenizer treatment was in the form of a turbid emulsion. When a drop of the mixed solution was dropped on a slide, a cover glass was covered and observed with an optical microscope, it was confirmed that countless emulsion droplets of about several μm were generated, and the emulsion droplets had dispersion stability as an O / W type emulsion.
[0717] (Step 3-ii: Step of solidifying the core material)
[0718] The O / W type emulsion dispersion was placed in a hot water bath at 70°C using a water bath, and treated for 8 hours while being stirred by a stirrer to perform a polymerization reaction. After the treatment for 8 hours, the dispersion was cooled to room temperature. The appearance of the dispersion did not change before and after the polymerization reaction.
[0719] (Washing and drying process)
[0720] The obtained dispersion was placed in a centrifugal separator and treated at a centrifugal force of 75,000 g for 5 minutes to obtain a precipitate. The supernatant was removed by decantation to recover the precipitate, which was then washed twice alternately with pure water and methanol using a PTFE membrane filter having a pore size of 0.1 μm.
[0721] The thus obtained washed / recovered product was redispersed at a concentration of 1%, and the particle size was evaluated using a particle size distribution meter (NANOTRAC UPA-EX150, "Nikkiso Co., Ltd."). Next, the washed / recovered product was air-dried and then vacuum-dried at room temperature of 25°C for 24 hours to obtain a yellow, fine-textured dry powder derived from the LSPR of spherical silver particles.
[0722] (Shape observation by scanning electron microscope)
[0723] The obtained dry powder was observed by scanning electron microscopy (SEM). Fig. 9 As shown. It can be confirmed that countless true spherical particles derived from the shape of the emulsion droplets are formed by polymerization reaction using the O / W type emulsion droplets as a template, and it can be confirmed that the surface is uniformly covered with cellulose nanofibers with a width of several nm. Although the particles are repeatedly washed by filtration and washing, the surface of the particles is still evenly covered with cellulose nanofibers, indicating that the core particles and the cellulose nanofibers are combined and are in an inseparable state.
[0724] In addition, despite repeated cleaning by filtration and washing, spherical silver particles of about several to 10 nm still exist on the surface of the cellulose nanofibers. The cellulose nanofibers on the surface of the particles are loaded with spherical silver particles as functional materials, which indicates that the cellulose nanofibers and the spherical silver particles are inseparable.
[0725] Furthermore, when the obtained dry powder was embedded in a resin and cut with a microtome, and then observed using a scanning electron microscope, it was confirmed that a uniform coating layer was formed on the surface of the core particles.
[0726] In this way, despite repeated washing by filtration and washing, the surfaces of the personal care particles were still evenly covered with cellulose nanofibers. Since the surfaces of the cellulose nanofibers were loaded with spherical silver particles as a functional material, it was confirmed that the obtained dry powder was the personal care particles of the second embodiment.
[0727] (Evaluation of Dispersibility)
[0728] When the dry powder is added to pure water at a concentration of 1% by mass and stirred for 24 hours with a stirrer for redispersion, it is easy to redisperse, and no aggregation is observed by visual inspection. In addition, when a particle size distribution meter is used to evaluate the particle size, the average particle size is the same as before drying, and there is no signal indicating aggregation in the data of the particle size distribution meter. As shown above, even if the surface of the personal care particles is coated with cellulose nanofibers, it will not form a film due to drying, but will be obtained in the form of a powder, and it also has good redispersibility.
[0729] <Example 22>
[0730] In step ic of step 2-iii of Example 21, personal care particles were obtained under the same conditions as in Example 21 except that oxygen was blown in. The obtained dry powder of the personal care particles was observed using a scanning electron microscope (SEM). The SEM image is as follows: Fig.10 shown.
[0731] <Example 23>
[0732] In Example 21, personal care particles were prepared under the same conditions as in Example 21 except that a chitosan nanofiber (also referred to as "chitosan NF") dispersion prepared according to Patent Document 6 cited as a prior art document was used instead of TEMPO-oxidized CNF.
[0733] <Example 24>
[0734] In Example 21, a CM-modified CNF dispersion obtained by carboxymethylation (hereinafter also referred to as CM-modification) treatment according to Patent Document 2 cited as a prior art document was used instead of TEMPO oxidation. Personal care particles were prepared under the same conditions as in Example 21 except for the above.
[0735] <Example 25>
[0736] In Example 21, a phosphated CNF dispersion obtained by phosphate esterification treatment according to Non-Patent Document 1 cited as a prior art document was used instead of TEMPO oxidation. Personal care particles were prepared under the same conditions as in Example 21 except for the above.
[0737] <Example 26>
[0738] (First step: step of obtaining a cellulose nanofiber dispersion)
[0739] Under the same conditions as in Example 21, a cellulose nanofiber dispersion was obtained.
[0740] (Step 2-iii: Functional material loading step)
[0741] Under the same conditions as in Example 21, a cellulose nanofiber dispersion carrying spherical silver particles was obtained.
[0742] (Step 2-iv: Step of preparing O / W type emulsion)
[0743] Next, 10 g of polylactic acid (PLA) was dissolved and mixed in 100 g of ethylene dichloride, thereby preparing a soluble polymer.
[0744] When all of the soluble polymer was added to 500 g of a 0.5 mass % dispersion of cellulose nanofibers supporting spherical silver particles, the soluble polymer and the dispersion of cellulose nanofibers supporting spherical silver particles were separated into separate phases (two phases).
[0745] Next, an ultrasonic homogenizer was used to treat the upper liquid surface of the mixed liquid in a two-phase separated state in the same manner as in step 2-iv of Example 21. It was confirmed by an optical microscope that numerous emulsion droplets of about 1 to several tens of μm were generated and that the emulsion droplets had dispersion stability as an O / W type emulsion.
[0746] (Step 3-ii: Step of solidifying the core material)
[0747] The O / W type emulsion was dried under reduced pressure of 700 mmHg at 40°C for 3 hours to completely volatilize the ethylene dichloride. The appearance of the dispersion did not change before and after the evaporation of the ethylene dichloride.
[0748] When the obtained dispersion is separated and washed under the same conditions as in Example 21, personal care particles having a particle size of about 1 to several tens of μm can be obtained. When the recovered product is dried under the same conditions as in Example 21, a yellow fine-textured dry powder derived from the LSPR of the spherical silver particles can be obtained.
[0749] <Example 27>
[0750] First, the cellulose nanofibers loaded with spherical silver particles were prepared by performing the first step and the second step-iii in the same manner as in Example 26. Next, 10 g of poly-ε-caprolactone (PCL, manufactured by "Wako Junko") was dissolved in 200 g of ethyl acetate to prepare a soluble polymer. In addition, an O / W type emulsion was prepared in the same manner as in the second step-iv of Example 26. Next, the obtained O / W type emulsion was dried under reduced pressure at 40°C for 5 hours under reduced pressure conditions of 700 mmHg to completely volatilize the ethyl acetate (third step-ii).
[0751] When the obtained dispersion is separated and washed under the same conditions as in Example 21, personal care particles having a particle size of about 1 to several tens of μm can be obtained. When the recovered product is dried under the same conditions as in Example 21, a yellow fine-textured dry powder derived from the LSPR of the spherical silver particles can be obtained.
[0752] <Example 28>
[0753] After the first step was performed under the same conditions as in Example 21, the second step was not performed but the second step was performed under the same conditions as in Example 21, and then the washing and drying steps were performed to obtain cellulose nanofiber-coated particles. Next, the following fifth step was performed using the obtained cellulose nanofiber-coated particles, and then the particles were washed and dried by the following method.
[0754] (The fifth step: functional material loading step)
[0755] {Step iia: Preparation of cellulose nanofiber-coated particle dispersion}
[0756] The cellulose nanofiber-covered particles were dispersed in pure water to prepare 50 g of a 0.5 mass % dispersion of the cellulose nanofiber-covered particles.
[0757] {Step iib: Preparation of a silver nitrate aqueous solution and a cellulose nanofiber-coated particle-containing solution}
[0758] A 100 mM silver (I) nitrate aqueous solution was prepared and 1.0 g of the 100 mM silver nitrate aqueous solution was added to 50 g of the 0.5 mass % dispersion of cellulose nanofiber-coated particles while stirring with a stirring bar while maintaining a constant temperature (25° C.), and stirring was continued for 30 minutes.
[0759] {Process iic: Reduction precipitation}
[0760] Sodium borohydride was dissolved in distilled water to prepare a 100 mM sodium borohydride aqueous solution. While maintaining a constant temperature (25°C), 1.0 g of a 100 mM sodium borohydride aqueous solution was added to the silver nitrate aqueous solution and the cellulose nanofiber coated particle containing liquid while stirring with a stirrer, and stirring was continued for 60 minutes to prepare a dispersion of cellulose nanofiber coated particles loaded with spherical silver particles. The resulting dispersion exhibited a yellow color derived from the spherical silver particles, indicating that spherical silver particles were generated.
[0761] (Washing and drying process)
[0762] The obtained dispersion was placed in a centrifugal separator and treated at a centrifugal force of 75,000 g for 5 minutes to obtain a precipitate. The supernatant was removed by decantation to recover the precipitate, and then the precipitate was washed 4 times with pure water using a PTFE membrane filter with a pore size of 0.1 μm. The washed / recovered product thus obtained was redispersed at a concentration of 1%, and the particle size was evaluated using a particle size distribution meter (NANOTRACUPA-EX150, "Nikkiso Co., Ltd.").
[0763] Next, the washed / recovered product was air-dried and then vacuum-dried at room temperature of 25° C. for 24 hours, thereby obtaining a fine dry powder having a yellow color derived from the spherical silver particles.
[0764] <Example 29>
[0765] In step 2-iii of Example 21, an aqueous solution of sodium tetrachloroaurate (III) was used instead of an aqueous silver nitrate solution. Other than this, each step was carried out in the same manner as in Example 21 to obtain a dry powder. The obtained dry powder was observed using a scanning electron microscope (SEM). The SEM image is as follows: Fig.11 shown.
[0766] <Example 30>
[0767] In Example 21, after step 1, step 2-iii was not performed, but step 2-iv, step 3-ii, and washing and drying were performed to obtain cellulose nanofiber-coated particles. Next, the following step 5 was performed using the obtained cellulose nanofiber-coated particles, and then washing and drying were performed by the following method.
[0768] (The fifth step: functional material loading step)
[0769] The cellulose nanofiber coated particles were dispersed in pure water to prepare a 10 g dispersion of 5 mass % cellulose nanofiber coated particles. Next, Rhodamine B, a cationic dye, was dissolved in pure water to prepare a 10 g 5 mass % Rhodamine B aqueous solution. While stirring the Rhodamine B aqueous solution, the dispersion of the cellulose nanofiber coated particles was added and stirred for a while. In this way, a dispersion of cellulose nanofiber coated particles loaded with Rhodamine B was prepared.
[0770] (Washing and drying process)
[0771] The obtained dispersion was placed in a centrifugal separator and treated at a centrifugal force of 75,000 g for 5 minutes to obtain a precipitate. The supernatant was removed by decantation to recover the precipitate, and then the precipitate was washed 4 times with pure water using a PTFE membrane filter with a pore size of 0.1 μm. The washed / recovered product thus obtained was redispersed at a concentration of 1%, and the particle size was evaluated using a particle size distribution meter (NANOTRACUPA-EX150, "Nikkiso Co., Ltd.").
[0772] Next, the washed / recovered product was air-dried and then vacuum-dried at room temperature of 25° C. for 24 hours, thereby obtaining a fine dry powder (personal care particles) having a red color derived from rhodamine B.
[0773] <Comparative Example 21>
[0774] In Example 21, step 2-iv and step 3-ii were not performed. Other steps were carried out in the same manner as in Example 21.
[0775] <Comparative Example 22>
[0776] In Example 21, pure water was used instead of the TEMPO-oxidized CNF dispersion. Each step was carried out in the same manner as in Example 21 except for the above.
[0777] <Comparative Example 23>
[0778] In Example 21, each step was carried out in the same manner as in Example 21 except that a carboxymethyl cellulose (hereinafter also referred to as CMC) aqueous solution was used instead of the TEMPO-oxidized CNF dispersion.
[0779] <Comparative Example 24>
[0780] First, an aqueous solution was prepared by dissolving 8 parts by mass of polyvinyl alcohol (PVA) and 0.5 parts by mass of polyglyceryl laurate-10 (PGLE ML10) in 500 g of pure water. This solution was used instead of the cellulose nanofiber dispersion to prepare a dispersion of "PVA / PGLE ML10" loaded with silver particles in the same manner as in step 2-iii of Example 21. Next, this dispersion was used instead of the cellulose nanofiber dispersion loaded with silver particles to prepare an O / W type emulsion in the same manner as in step 2-iv of Example 26. Next, the obtained O / W type emulsion was spray-dried at a drying temperature of 100°C using a spray dryer.
[0781] <Comparative Example 25>
[0782] In Comparative Example 24, polyglyceryl laurate-10 (PGLE ML10) was not added. Each step was carried out in the same manner as in Comparative Example 24 except for the above.
[0783] <Comparative Example 26>
[0784] In Example 28, each step was carried out in the same manner as in Example 28 except that a carboxymethyl cellulose (hereinafter also referred to as CMC) aqueous solution was used instead of the TEMPO-oxidized CNF dispersion.
[0785] <Comparative Example 27>
[0786] In Comparative Example 21, each step was carried out in the same manner as in Comparative Example 21 except that an aqueous solution of sodium tetrachloroaurate (III) was used instead of an aqueous silver nitrate solution.
[0787] <Comparative Example 28>
[0788] In step ic of step 2-iii in Comparative Example 21, oxygen gas was blown in. Each step was carried out in the same manner as in Comparative Example 21 except for the above.
[0789] <Comparative Example 29>
[0790] As a conventional example, a dry powder obtained by mixing commercially available styrene-divinylbenzene copolymer microbeads (particle size 4.5 μm, Technochemica) and spherical silver microparticles (particle size 10 nm, Sigmar Dolic) was prepared.
[0791] <Evaluation Method>
[0792] (Evaluation of particle structure)
[0793] The obtained dry powders of each of Examples and Comparative Examples 21 to 28 and the prepared dry powder of Comparative Example 29 were observed using a scanning electron microscope to evaluate the particle structure. The evaluation was determined by "0" or "×" as shown below.
[0794] ○: True spherical particles can be obtained, the surface of which is covered with fine fibers (cellulose nanofibers or chitin nanofibers), and the functional material is supported on the fine fibers.
[0795] ×: The above-mentioned particles were not obtained.
[0796] (Evaluation of whether it can be recycled)
[0797] The dispersion obtained in step 3-ii or step 5 was placed in a centrifugal separator and treated at a centrifugal force of 75,000 g for 5 minutes, the supernatant was removed by decantation to recover the precipitate, and then the precipitate was washed twice alternately with pure water and methanol using a PTFE membrane filter with a pore size of 0.1 μm. The evaluation was judged by "0" and "×" shown below.
[0798] ○: The precipitate can be recovered by centrifugal separation, and the sample can be recovered on the membrane filter.
[0799] ×: The precipitate could not be recovered by centrifugation. Or the sample could not be recovered on the membrane filter.
[0800] (Evaluation of Dispersibility)
[0801] Each dry powder of the example and the comparative example was added to pure water at a concentration of 1 mass %, and dispersed with stirring using a stirrer for 24 hours. Whether or not the powder aggregated was visually confirmed, and the result was judged by "0" or "×" as shown below.
[0802] ○: No aggregates were observed visually.
[0803] ×: Aggregates were visually observed.
[0804] (Evaluation of user experience)
[0805] In a room with a temperature of 20°C and a humidity of 40% RH, each dry powder of the embodiment and the comparative example was applied to the inner side of the lower arm of the test subject (female in her 30s). Specifically, 0.1 g of each dry powder was applied with fingers into a circle with a diameter of about 5 cm. The feeling of use when applied to the skin was judged by the following "0" and "×".
[0806] ○: Good affinity with skin and little irritation to skin.
[0807] ×: Poor affinity with skin and irritating to skin.
[0808] (Evaluation of Moisturizing Properties)
[0809] In a room with an air temperature of 20°C and a humidity of 40%RH, each dry powder of the embodiment and the comparative example was applied to the inner side of the lower arm of the subject (30-year-old female). Specifically, 0.1 g of each dry powder was applied with fingers into a circle with a diameter of about 5 cm. After 30 minutes after application, the moisture content of the skin where the dry powder was applied was measured using a moisture detector MY-707S (Skara Co., Ltd.). The evaluation was judged by the "○" and "×" shown below.
[0810] ○: The water content is 60% or more.
[0811] ×: The moisture content is less than 60%.
[0812] (Evaluation of colorability)
[0813] In a room with a temperature of 20°C and a humidity of 40%RH, each dry powder of the embodiment and the comparative example was applied to the inner side of the lower arm of the test subject (female in her 30s). Specifically, 0.1 g of each dry powder was applied with fingers into a circle with a diameter of about 5 cm. The evaluation was judged by the following "○" and "×".
[0814] ○: Coloring is visually uniform.
[0815] ×: Coloring is visually uneven.
[0816] In addition, the color of the dry powder was visually confirmed.
[0817] The evaluation results of Examples 21 to 30 and Comparative Examples 21 to 29 are summarized in Table 3 below. The emulsion stabilizer in Table 3 refers to cellulose nanofibers or emulsion stabilizers used to replace cellulose nanofibers. In addition, Table 3 shows the polymer constituting the core particles and the functional components (support materials) contained in the core particles. In addition, Table 3 shows the manufacturing method used in each example. Figure 5 The manufacturing method III shown is still Figure 6 Manufacturing method IV is shown.
[0818] [Table 3]
[0819]
[0820] "-" in Table 3 means that the results were not implemented or could not be evaluated and therefore were not implemented.
[0821] From the evaluation results of Examples 21 to 30 shown in Table 3, it can be clearly confirmed that by adopting the manufacturing method III or the manufacturing method IV, personal care particles having core particles of polymers containing various monomers or biodegradable polymers can be produced regardless of the type of fine fibers (TEMPO-oxidized CNF, CM-treated CNF, phosphate-esterified CNF, chitin NF). In addition, it can be confirmed that personal care particles loaded with silver, gold microparticles and dyes of various shapes can be produced.
[0822] like Fig. 9 As shown in FIG. 21, it can be confirmed that the spherical silver particles are supported on the surface of the cellulose nanofiber-coated particles. Fig.10 As shown in FIG. 22, it can be confirmed that the flat microparticles are supported on the surface of the cellulose nanofiber-coated particles. Fig.11As shown, it was confirmed that in Example 29, spherical gold microparticles were supported on the surface of the cellulose nanofiber-coated particles.
[0823] When the personal care particles (dry powder) were observed, they showed optical properties derived from the LSPR of various metal particles, showing yellow in Example 21 and Examples 23 to 28, blue in Example 22, and red in Example 29. In Example 30, red was shown derived from rhodamine B.
[0824] The personal care particles obtained in Examples 21 to 30 can be filtered and washed, have good redispersibility even after drying, and exhibit excellent skin affinity, moisturizing properties, and uniform colorability.
[0825] On the other hand, in Comparative Examples 21, 27, and 28, metal fine particles of various shapes and metal types were supported on cellulose nanofibers to prepare dispersions of cellulose nanofibers supporting metal fine particles.
[0826] In Comparative Examples 21, 27, and 28, attempts were made to wash the obtained metal particle-loaded cellulose nanofiber dispersion by centrifugal separation, but this was not achieved. Therefore, the obtained dispersion was made into powder by freeze drying and freeze crushing, and evaluated in the same manner. As a result, the obtained powder had excellent moisture retention and colorability, but poor redispersibility and skin affinity.
[0827] In Comparative Examples 22 and 25, step 2-iv could not be performed. Specifically, even if an ultrasonic homogenizer treatment was performed, the monomer phase or the soluble polymer phase and the cellulose nanofiber dispersion phase remained in a two-phase separation state, or even if an emulsion could be formed, the emulsion would immediately break, so that a stable O / W type emulsion could not be prepared.
[0828] In addition, in Comparative Example 23, Comparative Example 24, and Comparative Example 26, an O / W emulsion can be formed in the 2-iv process. It is believed that this is because CMC and PGLE ML10 exhibit amphiphilicity in the same manner as cellulose nanofibers, and therefore play a role as a stabilizer for the emulsion. However, when the core material is solidified by removing the solvent from the polymerization of the polymerizable monomer or the soluble polymer in the subsequent 3-ii process, the emulsion breaks, and therefore personal care particles using the O / W emulsion as a template cannot be obtained. The reason is still uncertain, but CMC and PGLE ML10 are water-soluble, so the coating layer used to maintain the shape of the emulsion during the solidification of the core material is likely to be fragile. Therefore, it can be considered that the emulsion has broken during the solidification of the core material.
[0829] In Comparative Examples 22 to 26, samples were recovered when filtration and washing were performed. However, when the redispersibility of the dried powder was evaluated, aggregates were visually confirmed in all Comparative Examples 22 to 26, and the dispersibility was poor.
[0830] The evaluation results of the dry powders of Comparative Examples 22 to 26 showed that the skin affinity was poor, the moisturizing amount was low, and the coloring was uneven by visual observation. It is believed that since the dry powders of Comparative Examples 22 to 26 did not include cellulose nanofibers, the moisturizing effect and dispersion effect brought by the cellulose nanofibers could not be obtained, resulting in poor use feeling and coloring.
[0831] The dry powder of Comparative Example 29 was excellent in feel during use, but was inferior in dispersibility in water, moisture retention, and colorability.
[0832] Industrial Applicability
[0833] The composite particles involved in the first embodiment of the present invention can be used for: paint additives such as paints and matting agents, films such as light diffusion films, additives for molded products such as automobiles and building materials, paper such as recording paper, personal care products such as cosmetics, toiletries and home care products, medical products, etc.
[0834] When the composite particles according to the first embodiment of the present invention are used in personal care products, they can be used, for example, in products related to hair care, oral care, odor care, body care, skin care, and cosmetics. Specifically, toothpaste, perfume, nail polish, beauty serum, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair gel, hair spray, shampoo, conditioner, hair tonic, body lotion, face cream, and soap, etc.
[0835] According to a fourth aspect of the present invention, there is provided novel personal care particles having fine fibers, which solve the problem that fine fibers such as cellulose nanofibers and chitin nanofibers contain too much solvent and can be produced by a simple method.
[0836] Furthermore, by coating with fine fibers having high safety, high hydrophilicity, and a high specific surface area, personal care particles having a good touch and excellent moisturizing properties can be provided.
[0837] In addition, since the functional material is loaded on fine fibers with a high specific surface area, the dispersion stability of the functional material is maintained, thereby providing personal care particles that effectively exert the functions of functional materials such as shielding ultraviolet rays (absorption and / or scattering), coloring, antibacterial, and deodorizing.
[0838] Microfibers such as cellulose nanofibers and chitin nanofibers are composed of cellulose or chitin / chitosan, which are biodegradable polymers. Therefore, by making the core particles also composed of a material containing a biodegradable polymer, it is possible to provide personal care particles that reduce the environmental load and solve the problem of microplastics.
[0839] In addition, the personal care particles of the fourth embodiment can be included in personal care products and personal care compositions. That is, the personal care particles of the fourth embodiment can be used in, for example, hair care, oral care, odor care, body care, skin care, and cosmetics related products. Specifically, toothpaste, perfume, nail polish, beauty essence, lotion, emulsion, makeup remover, eye shadow, eyeliner, foundation, blush, hair spray, hair spray, shampoo, conditioner, hair tonic, lotion, face cream, and soap, etc.
[0840] Explanation of symbols
[0841] 1 Composite particles
[0842] 1A Personal Care Granules
[0843] 2A Core Particles
[0844] 2 core particles
[0845] 3. Fine fibers (fine fibers of at least one of cellulose nanofibers and chitin nanofibers)
[0846] 3A Unloaded microfibers
[0847] 3B Microfibers loaded with functional materials
[0848] 4. Stoma
[0849] 6 Droplets containing core material and pore former (droplets of W / O emulsion, hydrophobicity)
[0850] 6A Droplet containing core material
[0851] 7 Hydrophilic solvents
[0852] 8 Stabilizer
[0853] 9 Droplets containing pore formers (hydrophilic)
[0854] 10 Particles coated with microfibers (including pore formers)
[0855] 10A Particles coated with microfibers (without pore formers)
[0856] 11A Dispersion of unloaded microfibers
[0857] 11B Dispersion of microfibers loaded with functional materials
[0858] 12 Dispersion of core particles containing a pore former and covered with fine fibers
[0859] 12A Dispersion of core particles (without pore-forming agent) with microfibers coated on the surface
[0860] 13 W / O type emulsion
[0861] 14 W / O / W emulsion
[0862] 40 Functional Materials
Claims
1. A method for producing composite particles, comprising: A step of defibrillating a chitin / chitosan raw material in a solvent to obtain a dispersion of fine fibers as chitin nanofibers; A step of dispersing droplets containing a pore-forming agent which is removed to generate pores in a core material which becomes core particles after solidification to prepare a W / O type emulsion, and dispersing the droplets containing the W / O type emulsion in a dispersion of fine fibers so that the surfaces of the droplets containing the W / O type emulsion are covered with the fine fibers, thereby preparing a W / O / W type emulsion; A step of solidifying the core material inside the droplets of the W / O / W type emulsion to obtain a dispersion liquid containing droplets containing the pore former and core particles whose surfaces are covered with the fine fibers; as well as A step of recovering the core particles from the dispersion of the core particles and removing the pore former from the inside of the recovered core particles to generate pores inside the core particles.
2. The manufacturing method according to claim 1, wherein: As the core material, at least any one of a polymerizable monomer, a soluble polymer, and a molten polymer is used.
3. A composite particle produced by the method for producing a composite particle according to claim 1, comprising: a core particle having pores; and Fine fibers composed of chitosan nanofibers are bonded to the surface of the core particle and are inseparable.
4. The composite particles according to claim 3, wherein The core particle is formed of a material containing a polymer.
5. The composite particles according to claim 4, wherein The polymer comprises a biodegradable polymer.
6. The composite particle according to any one of claims 3 to 5, wherein The core particles are porous particles or hollow particles.
7. The composite particle according to any one of claims 3 to 5, wherein The light diffusion index of the composite particles is 0.6 or more.
8. The composite particle according to any one of claims 3 to 5, wherein At least one of an ultraviolet absorber, an ultraviolet scatterer, a fragrance, a deodorant component, a whitening component, an anti-inflammatory component, an exfoliant, and a colorant enters into the pores.
9. The composite particle according to any one of claims 3 to 5, wherein The fine fibers have ionic functional groups.
10. A personal care product comprising the composite particles according to any one of claims 3 to 9.
11. A method for producing particles for personal care, comprising: A step of defibrillating a chitin / chitosan raw material in a solvent to obtain a dispersion of fine fibers as chitin nanofibers; A step of loading a functional material that exerts a personal care function on the fine fibers in the fine fiber dispersion to obtain a fine fiber dispersion loaded with the functional material; A step of dispersing a liquid droplet containing a core material in a dispersion liquid of fine fibers carrying the functional material so that the surface of the liquid droplet is covered with the fine fibers carrying the functional material; as well as A step of solidifying the core material inside the liquid droplet covered with fine fibers carrying the functional material.
12. A method for producing particles for personal care, comprising: A step of defibrillating a chitin / chitosan raw material in a solvent to obtain a dispersion of fine fibers as chitin nanofibers; A step of dispersing droplets containing a core material in the dispersion so that the surfaces of the droplets are covered with the fine fibers; A step of solidifying the core material inside the liquid droplets to obtain a dispersion of particles in which the surfaces of the core particles are covered with the fine fibers; as well as A step of supporting a functional material that exerts a personal care function on the surface of the fine fiber-coated particles in a dispersion of the fine fiber-coated particles.
13. The manufacturing method according to claim 11 or claim 12, wherein: As the core material, at least any one of a polymerizable monomer, a soluble polymer, and a molten polymer is used.
14. A personal care particle produced by the method for producing the personal care particle according to claim 11 or 12, having: a core particle formed from a material comprising a polymer; Fine fibers composed of chitosan nanofibers that are inseparable and bonded to the surface of the core particle; and A functional material is supported on the microfibers and performs a personal care function.
15. The personal care particles according to claim 14, wherein The functional material is at least any one of an ultraviolet absorber, an ultraviolet scatterer, a fragrance, a deodorant component, a whitening component, an anti-inflammatory component, an exfoliant, and a colorant.
16. The personal care particles according to claim 15, wherein The colorant is at least any one of an organic synthetic colorant, a natural colorant, and an inorganic pigment.
17. The personal care particles according to claim 15, wherein The colorant is metal particles.
18. The personal care particles according to claim 17, wherein The metal particles are composed of a material containing at least any one element of Ru, Fe, Co, Rh, Ni, Pd, Pt, Cu, Ag, Au, and Zn.
19. The personal care particles according to claim 17, wherein The metal fine particles are in the form of a plate having an average particle diameter of 2 nm to 1000 nm and an average thickness of 1 nm to 100 nm.
20. The personal care particle according to any one of claims 14 to 19, wherein The chitosan nanofibers have ionic functional groups.
21. The personal care particle according to any one of claims 14 to 19, wherein The polymer comprises a biodegradable polymer.
22. A personal care product comprising the personal care particles according to any one of claims 14 to 21.
23. A personal care composition comprising the personal care particles of any one of claims 14 to 21.