A method for separating a photovoltaic module back sheet
By using alkaline alcohol solution to treat the photovoltaic laminate, efficient separation and recycling of the back plate of the photovoltaic module is achieved, the back plate separation problem in the prior art is solved, the cost and environmental pollution risks are reduced, and the operation process is simplified.
Patent Information
- Application Number
- CN202111287944.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-11-02
AI Technical Summary
The prior art is difficult to efficiently and greenly separate the back panel of photovoltaic modules, especially the toughness of the PET layer and the stability of the fluorine film, making it difficult for traditional methods to achieve effective recycling, and high temperature and high pressure treatment increases costs and environmental pollution risks.
The photovoltaic laminate is treated with alkaline alcohol solution (such as potassium hydroxide ethanol solution). Through alkaline hydrolysis and alcoholylation, the fluorine film floats on the upper layer of the solution, and the PET layer is dissolved in the solution to realize the back plate and other parts. The separation and reaction under normal pressure avoid the need for high temperature and high pressure.
It realizes efficient separation and recycling of the backplane, avoids the generation of harmful gases, reduces operating costs and environmental pollution, and simplifies the separation process.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic module recycling, and specifically relates to a photovoltaic module separation and recycling method, and in particular to a method for separating a photovoltaic module back plate. Background Art
[0002] The amount of scrapped photovoltaic modules increases year by year. The first difficulty encountered in the entire process of recycling the various parts of the modules is how to deal with the backsheet. The backsheet is generally made of a single or double layer of fluorine film bonded to a PET layer. The fluorine film has a stable chemical structure, and the usual landfill treatment method cannot degrade this component even within a thousand years; acid dissolution, organic solvent dissolution or heat treatment will produce toxic gases such as hydrogen fluoride. The existence of the backsheet means that if the above methods are applied to the recycling of modules, additional waste gas treatment measures are required, which increases the recycling cost and reduces the economic efficiency. Separating the fluorine-containing backsheet as the first step in recycling photovoltaic laminates can provide more method options for the subsequent recycling of silicon cells and glass parts, but how to efficiently and greenly separate the backsheet has become a problem that we urgently need to solve.
[0003] Patent document CN109092842A records a method for dismantling scrapped photovoltaic modules, which records that the fluorine film is removed in sequence by controlling the different pressures and angles of the fluid sprayed from the spray gun, and the backplane is separated from the silicon wafer, and then the silicon wafer, solder ribbon and glass are separated. However, due to the high toughness of the PET layer, it is very difficult to peel the backplane using the fluid sprayed from the spray gun.
[0004] Patent document CN110841786A describes a method for recycling waste photovoltaic modules, which describes the use of chemical treatment to directly degrade the backplane with alcohol (methanol\ethylene glycol) at 160-200°C to obtain fluorine-containing coatings for recycling. However, this method requires high temperature and high pressure (pressure of 2-4MPa) when using alcohol (methanol\ethylene glycol) for degradation, otherwise it cannot be achieved. Summary of the invention
[0005] In view of the deficiencies of the prior art, an object of the present invention is to provide a method for separating a photovoltaic module backplane.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions, including:
[0007] The present invention provides a method for separating a back sheet of a photovoltaic module, wherein the photovoltaic module comprises glass, a cell layer, a fluorine-containing back sheet and an aluminum frame junction box accessory device, and the method comprises:
[0008] Step 1, removing the aluminum frame and junction box of the photovoltaic module to obtain a photovoltaic laminate including glass, a battery layer and a fluorine-containing backsheet;
[0009] Step 2, adding the photovoltaic laminate into an alkaline alcohol solution for reaction, after the reaction is completed, the fluorine film in the fluorine-containing backsheet floats on the upper layer of the reaction solution, the PET layer in the fluorine-containing backsheet dissolves in the reaction solution, and the other parts of the photovoltaic laminate sink to the bottom of the solution, thereby separating the backsheet from other parts in the photovoltaic laminate;
[0010] Wherein, the reaction conditions of step 2 are: reaction temperature is 60-150° C., and reaction time is 0.15-24 h.
[0011] Preferably, in step 2, the reaction conditions further include: accelerating the reaction rate by a combination of one or more of physical stirring, ultrasonic stirring, and crushing the photovoltaic laminate before the reaction;
[0012] Preferably, the particle size of the photovoltaic laminate obtained after the crushing process is less than or equal to 2 cm*2 cm.
[0013] Preferably, in step 2, after the photovoltaic laminate is added to the alkaline alcohol solution, the mass volume ratio of the photovoltaic laminate to the alkaline alcohol solution is 50-850 g:1 L.
[0014] Preferably, the mass volume ratio of the photovoltaic laminate to the alkaline alcohol solution is 60-110 g:1 L.
[0015] Preferably, in step 2, the alkali in the alkaline alcohol solution includes at least one of NaOH, KOH, sodium carbonate and sodium bicarbonate.
[0016] Preferably, in step 2, the alcohol in the alkaline alcohol solution includes at least one of ethanol and ethylene glycol.
[0017] Preferably, the alkaline alcohol solution is a potassium hydroxide ethanol solution.
[0018] Preferably, in the alkaline alcohol solution, the concentration of the alkali is greater than or equal to 0.05 mol / L.
[0019] Preferably, the concentration of the alkali in the alkaline alcohol solution is 0.2-0.8 mol / L.
[0020] Preferably, in step 2, the reaction heating temperature is 90-120° C., and the reaction time is 0.5-8 h.
[0021] Preferably, in the reaction, the alcohol solution can be reused through a condensation reflux device.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The fluorine film in the back sheet separated and recovered by the present invention is not decomposed, so no fluorine-containing harmful gas is generated;
[0024] 2) The present invention uses an alkaline alcohol solution to allow the reaction to be carried out under normal pressure, requiring a relatively low heating temperature. After the reaction, the fluorine film floats in the solution, and the PET layer dissolves in the solution. The operation is simple, and separation and further recovery are easily achieved.
[0025] 3) The present invention can achieve the purpose of efficiently dissolving the PET layer through the synergistic effect of alkali and alcohol. DETAILED DESCRIPTION
[0026] Unless otherwise defined, technical terms or scientific terms used in this specification and claims shall have the ordinary meanings understood by persons with ordinary skills in the technical field to which this application belongs. All values from the lowest value to the highest value listed herein refer to all values obtained by incrementing the lowest value to the highest value by one unit when the difference between the lowest value and the highest value is more than two units.
[0027] The specific implementation methods of the present application will be described below. It should be noted that in the specific description of these implementation methods, in order to provide a concise description, it is impossible for this specification to provide a detailed description of all the features of the actual implementation methods. Without departing from the spirit and scope of the present application, those skilled in the art may modify and replace the implementation methods of the present application, and the resulting implementation methods are also within the scope of protection of the present application.
[0028] A method for separating a photovoltaic module back sheet is provided in a specific embodiment of the present invention. The photovoltaic module includes glass, a cell layer, a fluorine-containing back sheet and an aluminum frame junction box accessory device. The method includes:
[0029] Step 1, removing the aluminum frame and junction box of the photovoltaic module to obtain a photovoltaic laminate including glass, a battery layer and a fluorine-containing backsheet;
[0030] Step 2, adding the photovoltaic laminate into an alkaline alcohol solution for reaction, after the reaction is completed, the fluorine film in the fluorine-containing backsheet floats on the upper layer of the reaction solution, the PET layer in the fluorine-containing backsheet dissolves in the reaction solution, and the other parts of the photovoltaic laminate sink to the bottom of the solution, thereby separating the backsheet from other parts in the photovoltaic laminate;
[0031] The reaction conditions in step 2 are as follows: reaction temperature is 60-150° C., and reaction time is 0.5-24 h.
[0032] In one specific embodiment, in step 2, the reaction conditions further include: accelerating the reaction rate by a combination of one or more of physical stirring, ultrasonic stirring, and crushing the photovoltaic laminate before the reaction;
[0033] The particle size of the photovoltaic laminate obtained after the crushing process is less than or equal to 2cm*2cm.
[0034] The specific method and parameter conditions of the physical stirring and ultrasonic stirring used in the present invention are not particularly limited, as long as they can accelerate the reaction rate.
[0035] The present invention does not impose any particular limitation on the method and equipment for crushing the photovoltaic laminate, and it is only necessary to crush the photovoltaic laminate into particles of a certain size.
[0036] In a specific embodiment, in step 2, after the photovoltaic laminate is added to the alkaline alcohol solution, the mass volume ratio of the photovoltaic laminate to the alkaline alcohol solution is 50-850 g:1 L.
[0037] In a specific embodiment, the mass volume ratio of the photovoltaic laminate to the alkaline alcohol solution is 60-110 g:1L.
[0038] In a specific embodiment, in step 2, the base in the alkaline alcohol solution includes at least one of NaOH, KOH, sodium carbonate, and sodium bicarbonate.
[0039] In a specific embodiment, in step 2, the alcohol in the alkaline alcohol solution includes at least one of ethanol and ethylene glycol.
[0040] In a specific embodiment, the alkaline alcohol solution is a potassium hydroxide ethanol solution, which can achieve the best dissolution effect.
[0041] In a specific embodiment, the concentration of the alkali in the alkaline alcohol solution is greater than or equal to 0.05 mol / L.
[0042] In a specific embodiment, the concentration of the alkali in the alkaline alcohol solution is 0.2-0.8 mol / L. Within this range, there is a good balance between the alkali consumption and the backing plate separation rate.
[0043] In a specific embodiment, in step 2, the reaction heating temperature is 90-120° C., and the reaction time is 0.5-8 h.
[0044] The method of the present invention uses an alkaline alcohol solution as a reaction solvent to treat the photovoltaic laminate, which promotes the alkaline hydrolysis and alcoholysis of the PET layer in the back plate. Through the synergistic effect of the base and the alcohol, the purpose of efficiently dissolving the PET layer can be achieved without high temperature and high pressure.
[0045] In one specific embodiment, in the reaction, the alcohol solution can be reused through a condensation reflux device.
[0046] Example
[0047] The embodiments of the present application will be described in detail below. This embodiment is implemented on the premise of the technical solution of the present application, and a detailed implementation method and a specific operation process are given, but the protection scope of the present application is not limited to the following embodiments.
[0048] Example 1
[0049] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0050] Step 1: Take a photovoltaic module (263*143mm), mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate, and measure its mass to be 302.32g.
[0051] Step 2: Add the photovoltaic laminate to a 0.3 mol / l potassium hydroxide ethanol solution for reaction. The volume of the potassium hydroxide ethanol solution is 3 L and the heating temperature is 150°C. After 8 hours of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0052] Finally, a total of 1.12 g of fluorine film and 294.29 g of bottom precipitate were recovered.
[0053] Example 2
[0054] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0055] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a laminate;
[0056] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.3mol / l potassium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 1.5h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0057] Finally, a total of 0.21 g of fluorine film and 58.41 g of bottom precipitate were recovered.
[0058] Example 3
[0059] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0060] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0061] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.3mol / l sodium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 2.5h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0062] Finally, a total of 0.24 g of fluorine film and 58.56 g of bottom precipitate were recovered.
[0063] Example 4
[0064] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0065] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0066] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.05mol / l sodium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 6h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0067] Finally, a total of 0.20 g of fluorine film and 58.57 g of bottom precipitate were recovered.
[0068] Example 5
[0069] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0070] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0071] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.2mol / l sodium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 3h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0072] Finally, a total of 0.25 g of fluorine film and 58.58 g of bottom precipitate were recovered.
[0073] Example 6
[0074] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0075] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0076] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.8mol / l sodium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 2h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0077] Finally, a total of 0.25 g of fluorine film and 58.57 g of bottom precipitate were recovered.
[0078] Example 7
[0079] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0080] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0081] Step 2: Break the photovoltaic laminate into small pieces of 2cm*2cm, weigh 60g of the small pieces and add them into 1L of 0.5mol / l sodium bicarbonate ethylene glycol solution for reaction. The heating temperature is 150℃. After 6h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0082] Finally, a total of 0.26 g of fluorine film and 58.56 g of bottom precipitate were recovered.
[0083] Example 8
[0084] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0085] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0086] Step 2: Break the photovoltaic laminate into small pieces of 1cm*1cm, weigh 200g of the small pieces and add them into 1L of 0.7mol / l sodium carbonate ethylene glycol solution for reaction. The heating temperature is 150℃. After 5h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0087] Finally, a total of 0.24 g of fluorine film and 58.57 g of bottom precipitate were recovered.
[0088] Example 9
[0089] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0090] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a laminate;
[0091] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.8mol / l potassium hydroxide ethanol solution for reaction. The heating temperature is 120℃. After 1h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0092] Finally, a total of 0.25 g of fluorine film and 58.51 g of bottom precipitate were recovered.
[0093] Example 10
[0094] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0095] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a laminate;
[0096] Step 2: Crush the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.3mol / l potassium hydroxide ethanol solution for reaction. The heating temperature is 100℃. After 4h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0097] Finally, a total of 0.21 g of fluorine film and 58.60 g of bottom precipitate were recovered.
[0098] Embodiment 11
[0099] This embodiment provides a method for separating a photovoltaic module back sheet, and the photovoltaic modules are separated and their components are recycled according to the following steps:
[0100] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a laminate;
[0101] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.3mol / l potassium hydroxide ethylene glycol solution for reaction. The heating temperature is 120℃. After 2h of reaction, the back panel is completely separated, with the fluorine film floating on the upper layer of the reaction solution, the PET layer dissolving into the reaction solution, and the other parts of the photovoltaic laminate sinking to the bottom of the reaction solution.
[0102] Finally, a total of 0.22 g of fluorine film and 58.54 g of bottom precipitate were recovered.
[0103] Comparative Example 1
[0104] This comparative example provides a method for separating the back sheet of a photovoltaic module, and the photovoltaic modules are separated according to the following steps to recycle the components thereof:
[0105] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0106] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of ethanol solution for reaction. The heating temperature is 150℃. After 24h of reaction, the back panel is still not dissolved in the solution, resulting in inability to separate.
[0107] Comparative Example 2
[0108] This comparative example provides a method for separating the back sheet of a photovoltaic module, and the photovoltaic modules are separated according to the following steps to recycle the components thereof:
[0109] Step 1: Take a photovoltaic module, mechanically remove the aluminum frame and junction box to obtain a photovoltaic laminate;
[0110] Step 2: Break the photovoltaic laminate into small pieces of 1.5cm*1.5cm, weigh 60g of the small pieces and add them into 1L of 0.3mol / l potassium hydroxide aqueous solution for reaction. The heating temperature is 150℃. After 24h of reaction, the back panel is still not dissolved in the solution, resulting in inability to separate.
[0111] The present invention has many specific application paths, and the above is only a preferred embodiment of the present invention. It should be pointed out that the above embodiments are only used to illustrate the present invention, and are not used to limit the protection scope of the present invention. For those of ordinary skill in the art, several improvements can be made without departing from the principle of the present invention, and these improvements should also be regarded as the protection scope of the present invention.
Claims
1. A method for separating a back sheet of a photovoltaic module, wherein the photovoltaic module comprises glass, a cell layer, a fluorine-containing back sheet and an aluminum frame junction box accessory device, It is characterized in that The method comprises: Step 1, removing the aluminum frame and junction box of the photovoltaic module to obtain a photovoltaic laminate including glass, a battery layer and a fluorine-containing backsheet; Step 2, adding the photovoltaic laminate into an alkaline alcohol solution for reaction, after the reaction is completed, the fluorine film in the fluorine-containing backsheet floats on the upper layer of the reaction solution, the PET layer in the fluorine-containing backsheet dissolves in the reaction solution, and the other parts of the photovoltaic laminate sink to the bottom of the solution, thereby separating the backsheet from other parts in the photovoltaic laminate; Among them, the reaction conditions of step 2 are: reaction temperature is 60-150°C, and reaction time is 0.15-24h; in step 2, the base in the alkaline alcohol solution includes at least one of NaOH, KOH, sodium carbonate, and sodium bicarbonate, the alcohol in the alkaline alcohol solution includes at least one of ethanol and ethylene glycol, and the concentration of the base in the alkaline alcohol solution is greater than or equal to 0.05mol / L.
2. The method for separating a photovoltaic module back sheet according to claim 1, It is characterized in that In step 2, the reaction conditions also include: accelerating the reaction rate by a combination of one or more of physical stirring, ultrasonic stirring, and crushing the photovoltaic laminate before the reaction.
3. The method for separating the back sheet of a photovoltaic module according to claim 1, It is characterized in that In step 2, after the photovoltaic laminate is added to the alkaline alcohol solution, the mass volume ratio of the photovoltaic laminate to the alkaline alcohol solution is 50 to 850 g:1 L.
4. The method for separating a photovoltaic module back sheet according to claim 1, It is characterized in that The alkaline alcohol solution is potassium hydroxide ethanol solution.
5. The method for separating a photovoltaic module back sheet according to claim 1, It is characterized in that In the alkaline alcohol solution, the concentration of the alkali is 0.2-0.8 mol / L.
6. The method for separating a photovoltaic module back sheet according to claim 1, It is characterized in that The reaction conditions of step 2 are: reaction temperature is 90-120° C., and reaction time is 0.5 to 8 h.
7. The method for separating a photovoltaic module back sheet according to claim 1, It is characterized in that In the reaction, the alcohol solution can be reused through a condensation reflux device.