A kind of imitation wood grain HDPE co-extruded foam board and preparation method thereof

By using co-extrusion coating technology to form a wood grain-like structure on the surface of the foamed core layer, the problems of uneven surface and monotonous color of polyethylene foamed materials are solved, improving the aesthetics and performance of foamed boards, making them suitable for the building materials industry.

CN114043696BActive Publication Date: 2024-11-05NINGBO HELONG NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111309744.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-02
Publication Date
2024-11-05
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

After polyethylene foam expands in the mold, it is easy to cause uneven 'orange peel' texture to form on the surface, which affects the appearance. In addition, the surface color is monotonous and it is difficult to form a natural wood grain effect.

Method used

By employing co-extrusion coating technology, functional particles of different colors in the surface co-extrusion layer are combined with the foamed core layer to form a wood grain structure. Materials such as HDPE, vinyl copolymer, polyethylene elastomer and surface filler are used to improve the adhesion and aesthetics of the surface co-extrusion layer.

Benefits of technology

It improves the wear resistance, impact resistance, and heat and sound insulation properties of foamed boards, reduces production costs, and gives the board surface a natural wood feel, making it suitable for the building materials industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114043696B_ABST
    Figure CN114043696B_ABST
Patent Text Reader

Abstract

The present application relates to a wood-grain HDPE co-extruded foam board and its preparation process, which belongs to the field of foamed board. It includes a foamed core layer and a surface co-extruded layer. The foamed core layer is made of the following raw materials: high-density polyethylene, melt enhancer, core layer filler, foaming agent, foaming activator, and cross-linking agent; the surface co-extruded layer is made of the following raw materials: HDPE, vinyl copolymer, polyethylene-based elastomer, surface filler, and two colors of surface masterbatch. The preparation method is as follows: prepare the materials; the core layer mixture is melted and foamed and cooled to be pre-shaped to obtain a foamed core layer; the molten two different colors of surface co-extruded materials are mixed and extruded to coat the surface of the foamed core layer matrix to form a wood-grain imitation surface co-extruded layer; cool and shape. The co-extruded foam board of the present application has good thermal insulation and sound insulation effects. Compared with traditional foamed boards, it has better wear resistance and surface hardness, is more economical in cost, and has a wider application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of foaming materials, in particular to an imitation wood grain HDPE co-extruded foaming board and a preparation method thereof. Background Art

[0002] Polyethylene foam material is a building material made of polypropylene resin as the main body, with foaming agent, cross-linking agent and other additives. Due to its advantages of low density, chemical corrosion resistance, good thermal insulation, low water absorption and low cost, it is widely used in filling materials, sound insulation materials, construction industry materials and lightweight materials.

[0003] However, since polyethylene foam materials are prone to uneven foaming, after the foam is foamed and expanded in the mold, the traction and stretching force is uneven during extrusion from the outlet die, resulting in the formation of "orange peel" on the surface of the polyethylene foam profile, which reduces the quality of the foamed board. In addition, the surface color of the foam material is single. If a variety of masterbatches are used to create a surface imitation wood grain process, the natural direction of the imitation wood grain on the surface of the final board is easily affected due to the formation of "orange peel", which is not conducive to the appearance of the foamed board. Summary of the invention

[0004] In order to improve the quality and aesthetics of a co-extruded foam board, the present application provides an imitation wood grain HDPE co-extruded foam board and a preparation process thereof.

[0005] In the first aspect, the present application discloses a method for preparing a wood-grain imitation HDPE co-extruded foamed board, which adopts the following technical scheme:

[0006] A method for preparing a wood-grain imitation HDPE co-extruded foamed board comprises the following preparation steps:

[0007] Step 1) Prepare the ingredients:

[0008] Core layer mixture: by weight, raw materials including 40-80 parts of high-density polyethylene, 5.15-10.5 parts of melt enhancer, 10-40 parts of core layer filler, and 0.5-1.5 parts of cross-linking agent are mixed evenly to obtain a core layer mixture for standby use; Surface layer mixture: by weight, raw materials including 65-90 parts of HDPE, 3-5 parts of vinyl copolymer, 5-10 parts of polyethylene elastomer, 3-10 parts of surface filler, and 1-5 parts of compatibilizer are mixed, plasticized and granulated to obtain surface co-extrusion layer functional particles, the surface co-extrusion layer functional particles are divided into two parts, and then 2-3 parts of surface masterbatches of different colors are respectively mixed to obtain two parts of surface layer mixtures for standby use;

[0009] Step 2) Foam core layer extrusion:

[0010] The prepared core layer mixture is poured into the hopper of the core layer extruder for melting and plasticization, 0.4-5 parts of a foaming agent and 0.4-2 parts of a foaming activator are added to the homogenizing section at the rear end of the screw of the core layer extruder for foaming, and extruded into a core layer mold for foaming molding, and then the core layer is cooled and pre-shaped by the mold to obtain a foamed core layer;

[0011] Step 3) Surface co-extrusion coating:

[0012] The two prepared surface layer mixtures are respectively put into the hoppers of two surface layer extruders, and the two surface layer extruders melt and plasticize the poured surface layer mixtures to obtain surface co-extruded materials. The surface co-extruded materials of one surface layer extruder are merged into the other surface extruder through a confluence core. At the same time, the foaming core layer passes through the center of the co-extrusion die, and the melted surface co-extruded materials of two different colors are mixed and extruded to the co-extrusion die, and are coated on the surface of the foaming core layer substrate to form a surface co-extruded layer with imitation wood patterns;

[0013] Step 4) Cooling and shaping: After extrusion by the co-extrusion die, the co-extrusion cooling die is used for shaping to obtain a HDPE co-extruded foamed board with imitation wood grain.

[0014] By using high-density polyethylene, melt enhancer, core filler, cross-linking agent, foaming agent, and foaming activator for plasticizing, foaming, and cooling molding, a foaming core layer with good thermal insulation, energy saving, sound insulation, and lightweight properties is obtained. The foaming core layer is quickly cooled and pre-shaped by a cooling mold before the outlet mold, which reduces the formation of "orange peel" on the surface of the foaming core layer at the outlet mold, which is conducive to better co-extrusion coating of the subsequent surface co-extrusion layer; in addition, by using HDPE, vinyl copolymer, polyethylene-based elastomer, surface filler, and compatibilizer for plasticizing and granulating, the surface co-extrusion layer functional particles are obtained, and then the surface co-extrusion layer functional particles are mixed with masterbatches of different colors for plasticization. , making the colors of the two plasticized and molten surface co-extruded materials more controllable, and the masterbatch is not easily affected by the long plasticization time to affect its color development, so that the surface co-extruded layer is co-extruded and coated on the surface of the foamed core layer to form a more natural and beautiful imitation wood pattern; the present application adopts co-extrusion coating technology to coat the surface co-extruded layer on the surface of the foamed core layer, which can not only solve the problems of low surface hardness and wear resistance of the existing polyethylene foam board, but also compared with the previous simple non-foamed board, the co-extruded foam board reduces the cost, and greatly improves the sound insulation, heat insulation, light weight and impact resistance and other properties, and can also form a natural wood feel effect on the surface of the board, so that it can be more widely used in the field of building materials.

[0015] Preferably, the melt enhancer comprises: 0.15-0.5 parts of coated polytetrafluoroethylene particles and 5-10 parts of ultra-high molecular weight polyethylene.

[0016] Preferably, the coated polytetrafluoroethylene particles are shell-core structure particles with polytetrafluoroethylene as the core and one or more monomers of ethylene, propylene, butadiene, acrylic acid, and methacrylic acid as the shell, and the particle size is 0.05-1 mm. The molecular weight of the ultra-high molecular weight polyethylene is 2-5 million.

[0017] By using coated polytetrafluoroethylene particles and ultra-high molecular weight polyethylene as melt enhancers for the foaming core layer, the coated polytetrafluoroethylene particles have better dispersibility and resistance to high-temperature decomposition due to the shell coating on their surface, so that polytetrafluoroethylene has a better strength improvement effect on the foaming core layer, and combined with a certain amount of ultra-high molecular weight polyethylene, the foaming core layer can have good melt tension and fluidity during plasticization, which is beneficial to the uniform foaming of the foaming core layer, thereby improving the overall structural strength of the foaming core layer.

[0018] Preferably, the core layer filler is a combination of one or more of talc and light calcium carbonate.

[0019] By adopting the above core layer fillers, the foamed core layer has a certain hardness, so that the co-extruded foamed board has better overall structural stability.

[0020] Preferably, the core layer mixture further comprises 1-2 parts of a dispersant, and the dispersant is a combination of one or more of stearic acid, zinc stearate, and calcium stearate.

[0021] By plasticizing and melting the dispersant together with high-density polyethylene, melt enhancer and core layer filler evenly, the subsequent foaming agent and foaming activator can be better dispersed, and the foaming core layer can be foamed more evenly, thereby further improving the overall strength of the foaming core layer, reducing the formation of "orange peel", and facilitating the surface co-extrusion layer to better cover and bond to the surface of the foaming core layer.

[0022] Preferably, the cross-linking agent is a combination of one or more of a TAC cross-linking agent, a TAIC cross-linking agent, and a DCP cross-linking agent.

[0023] By adopting the above cross-linking agent, the core layer mixture is further cross-linked and copolymerized in the system after being melted and plasticized, so that the foam structure formed in the foaming process is stabilized, which is beneficial to improving the mechanical properties and thermal insulation properties of the foamed core layer.

[0024] Preferably, the foaming agent is a combination of one or more of sodium bicarbonate and azodicarbonamide, and the foaming activator is zinc oxide.

[0025] By using the above foaming agent and foaming activator to melt the core layer mixture containing high-density polyethylene, melt enhancer, core layer filler, etc. and then foaming it, the foamed core layer has better bubble nucleation activity, the density of the board is reduced, and the board has good heat insulation and sound insulation.

[0026] Preferably, the polyethylene-based elastomer is a combination of one or more of POE, TPO and EVA.

[0027] By using the above polyethylene-based elastomer as the raw material of the surface co-extrusion layer, the functional particles of the surface co-extrusion layer can be better coated on the surface of the foamed core layer during melt plasticization and extrusion, thereby reducing the surface layer detachment phenomenon caused by the difference in expansion rate between the foamed core layer and the surface co-extrusion layer, thereby making the adhesion between the foamed core layer and the surface co-extrusion layer better and the durability better. In addition, the polyethylene-based elastomer can improve the toughness of the board, thereby having a better impact resistance when the board is subjected to external force.

[0028] Preferably, the vinyl copolymer is a combination of one or more of EAA, EEA, and EMAA.

[0029] By using the above vinyl copolymer as the raw material of the surface co-extrusion layer, the surface co-extrusion layer can have good adhesion to the foam core layer, and has better structural integrity after co-extrusion coating and molding, so that the surface of the co-extruded foam board is smoother and more beautiful, and has better mechanical properties.

[0030] Preferably, the compatibilizer is maleic anhydride grafted polyethylene.

[0031] By adding maleic anhydride grafted polyethylene compatibilizer, maleic anhydride functional groups are grafted onto vinyl copolymers and polyethylene-based elastomers, thereby enhancing the compatibility of the surface filler in the surface co-extruded material, allowing the surface filler to be better dispersed in the molten surface co-extruded material, which is beneficial to better improve the surface strength and wear resistance of the co-extruded foam board.

[0032] Preferably, the surface filler is a combination of one or more of hollow glass microspheres, fumed silica, and talcum powder.

[0033] By adopting the above surface fillers, the roughness of the surface co-extruded layer is improved to a certain extent, the diffuse reflection of the surface of the co-extruded foam board is increased, and the glossiness is reduced, so that the surface of the co-extruded foam board is matte and has a more natural wood grain texture.

[0034] Preferably, the head of one of the surface layer extruders is connected to the barrel of the other surface layer extruder at one third of the side close to the hopper through a confluence core.

[0035] By connecting the front surface extruder to the appropriate position of the barrel of the rear surface extruder, it is beneficial to make the surface co-extrusion materials of two different colors mixed and then extruded and coated on the surface of the foaming core layer to form a texture closer to natural wood.

[0036] In the second aspect, the present application discloses a wood-grain imitation HDPE co-extruded foam board, which adopts the following technical solution:

[0037] A wood-grain imitation HDPE co-extruded foamed board is prepared by the above-mentioned method for preparing the wood-grain imitation HDPE co-extruded foamed board.

[0038] The co-extruded foam board formed by co-extrusion coating the surface of the foam core layer with a surface co-extrusion layer can not only improve the wear resistance and impact resistance of the single foam board, but also form a surface co-extrusion layer with natural wood grain on the surface of the foam core layer, so that the co-extruded foam board has the heat insulation, sound insulation and light weight characteristics of the foam board, and also has the good mechanical properties of the non-porous board, so that the co-extruded foam board has a wider application value.

[0039] In a third aspect, the present application discloses a HDPE surface co-extruded layer functional particle, which adopts the following technical solution: a HDPE surface co-extruded layer functional particle, wherein the surface co-extruded layer functional particle is prepared by the above-mentioned preparation method of the imitation wood grain HDPE co-extruded foam board.

[0040] The surface co-extrusion layer functional particles are prepared by granulating HDPE, vinyl copolymer, polyethylene elastomer, surface filler and compatibilizer. They have better coating and bonding effect on polyethylene foam materials in the co-extrusion process, and have excellent surface hardness and wear resistance. After plasticizing and granulating into functional particles, subsequent production is convenient and the equipment requirements for co-extrusion processing are reduced.

[0041] In summary, the present application includes at least one of the following beneficial technical effects:

[0042] 1. By adopting the co-extrusion coating process, the surface co-extrusion layer is co-extruded and coated on the surface of the foam core layer. The co-extruded foam board formed has the advantages of energy saving and heat preservation, sound insulation and heat insulation, light weight, high wear resistance, strong impact resistance, low cost, etc., and has good economic value;

[0043] 2. By dividing the surface co-extruded layer functional particles into two parts, and mixing the surface masterbatches of different colors and melting and plasticizing them respectively, the two parts of surface co-extruded materials of different colors are mixed and co-extruded and coated on the surface of the foaming core layer, forming a co-extruded foam board with natural wood texture, which has better aesthetics, and makes the co-extruded foam board more widely used in the field of building materials;

[0044] 3. The surface co-extrusion layer functional particles are prepared by granulating HDPE, vinyl copolymer, polyethylene-based elastomer, surface filler and compatibilizer, so that the surface co-extrusion layer functional particles can have a better coating and bonding effect on the polyethylene foam material in the co-extrusion process, so that the co-extruded foam board is not easy to be separated from the surface due to the different expansion rates of the foaming core layer and the surface co-extrusion layer, thereby having better durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a schematic diagram of a co-extrusion foam board production line according to an embodiment of the present invention.

[0046] Explanation of reference numerals: 100, core layer extruder; 101, core layer cooling die; 200, surface layer extruder; 201, confluence core; 300, co-extrusion die; 301, co-extrusion cooling die. DETAILED DESCRIPTION

[0047] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0048] Example

[0049] Example 1

[0050] A wood-grained HDPE co-extruded foam board, the raw materials and dosage of which are shown in Table 1, Figure 1 , and its preparation method comprises the following steps:

[0051] Step 1) Prepare the ingredients:

[0052] Core layer mixture: according to the proportions in Table 1, the high-density polyethylene, melt enhancer, core layer filler, cross-linking agent and core layer colorant in the foaming layer raw material are mixed evenly to obtain a core layer mixture for standby use;

[0053] Surface layer mixture: HDPE, vinyl copolymer, surface filler, compatibilizer and polyethylene elastomer are uniformly mixed according to the ratio in Table 1, melt-plasticized and granulated at 200°C by a granulator to obtain surface co-extruded layer functional particles with a diameter of 2-3 mm, and the surface co-extruded layer functional particles are weighed according to the ratio and divided into two equal parts, and then the surface masterbatches of different colors are mixed in equal amounts to obtain two parts of surface layer mixtures for standby use;

[0054] Step 2) Foam core layer extrusion:

[0055] The prepared core layer mixture is poured into the hopper of the core layer extruder 100 to be melted and plasticized at 160°C, and a foaming agent and a foaming activator are added to the homogenizing section at the rear end of the screw of the core layer extruder 100 according to the ratio in Table 1, and the temperature is maintained at 200°C for foaming, and extruded into the core layer mold for foaming molding, and then cooled to 50°C for pre-molding through the core layer cooling mold 101 to obtain a foamed core layer;

[0056] Step 3) Surface co-extrusion coating:

[0057] The two prepared surface layer mixtures are respectively put into the hoppers of two surface layer extruders 200, and the head of one surface layer extruder 200 is connected to the barrel of the other surface layer extruder 200 at one third of the side close to the hopper through a confluence core 201. The two surface layer extruders 200 melt and plasticize the poured surface layer mixtures at 210°C to obtain surface co-extruded materials. The surface co-extruded materials of one surface layer extruder 200 are merged into the other surface extruder 200 through the confluence core 201. At the same time, the foaming core layer passes through the center of the co-extrusion die 300, and the melted surface co-extruded materials of two different colors are mixed and extruded to the co-extrusion die 300, and coated on the surface of the foaming core layer substrate to form a surface co-extruded layer with imitation wood pattern;

[0058] Step 4) Cooling and shaping:

[0059] After being extruded by the co-extrusion die, the co-extrusion cooling die 301 is cooled to 40° C. to set the shape, thereby obtaining a HDPE co-extruded foamed board with imitation wood grain.

[0060] Example 2

[0061] A wood-grained HDPE co-extruded foam board, the raw materials and dosage of which are shown in Table 1, Figure 1 , and its preparation method comprises the following steps:

[0062] Step 1) Prepare the ingredients:

[0063] Core layer mixture: according to the proportions in Table 1, the high-density polyethylene, melt enhancer, core layer filler, crosslinking agent, dispersant and core layer colorant in the foaming layer raw material are mixed evenly to obtain a core layer mixture for standby use;

[0064] Surface layer mixture: HDPE, vinyl copolymer, surface filler, compatibilizer and polyethylene elastomer are uniformly mixed according to the ratio in Table 1, melt-plasticized and granulated at 160°C by a granulator to obtain surface co-extruded layer functional particles with a diameter of 2-3 mm, and the surface co-extruded layer functional particles are weighed according to the ratio and divided into two equal parts, and then the surface masterbatches of different colors are mixed in equal amounts to obtain two parts of surface layer mixtures for standby use;

[0065] Step 2) Foam core layer extrusion:

[0066] The prepared core layer mixture is poured into the hopper of the core layer extruder 100 to be melted and plasticized at 140°C, and a foaming agent and a foaming activator are added to the homogenizing section at the rear end of the screw of the core layer extruder 100 according to the ratio in Table 1, and the temperature is maintained at 180°C for foaming, and extruded into the core layer mold for foaming molding, and then cooled to 50°C through the core layer cooling mold 101 for pre-molding to obtain a foamed core layer;

[0067] Step 3) Surface co-extrusion coating:

[0068] The two prepared surface layer mixtures are respectively put into the hoppers of two surface layer extruders 200, and the head of one surface layer extruder 200 is connected to the barrel of the other surface layer extruder 200 at one third of the side close to the hopper through a confluence core 201. The two surface layer extruders 200 melt and plasticize the poured surface layer mixtures at 190°C to obtain surface co-extruded materials. The surface co-extruded materials of one surface layer extruder 200 are merged into the other surface extruder 200 through the confluence core 201. At the same time, the foaming core layer passes through the center of the co-extrusion die 300, and the melted surface co-extruded materials of two different colors are mixed and extruded to the co-extrusion die 300, and coated on the surface of the foaming core layer substrate to form a surface co-extruded layer with imitation wood pattern;

[0069] Step 4) Cooling and shaping:

[0070] After being extruded by the co-extrusion die, the co-extrusion cooling die 301 is cooled to 40° C. to set the shape, thereby obtaining a HDPE co-extruded foamed board with imitation wood grain.

[0071] Example 3

[0072] A wood-grained HDPE co-extruded foam board, the raw materials and dosage of which are shown in Table 1, Figure 1 The preparation method comprises the following steps:

[0073] Step 1) Prepare the ingredients:

[0074] Core layer mixture: according to the proportions in Table 1, the high-density polyethylene, melt enhancer, core layer filler, crosslinking agent, dispersant and core layer colorant in the foaming layer raw material are mixed evenly to obtain a core layer mixture for standby use;

[0075] Surface layer mixture: HDPE, vinyl copolymer, surface filler, compatibilizer and polyethylene elastomer are uniformly mixed according to the ratio in Table 1, melt-plasticized and granulated at 180°C by a granulator to obtain surface co-extruded layer functional particles with a diameter of 2-3 mm, and the surface co-extruded layer functional particles and anti-ultraviolet masterbatch are weighed according to the ratio and divided into two equal parts, and then the same amount of surface masterbatches of different colors are mixed respectively to obtain two parts of surface layer mixtures for standby use;

[0076] Step 2) Foam core layer extrusion:

[0077] The prepared core layer mixture is poured into the hopper of the core layer extruder 100 to be melted and plasticized at 150°C, and a foaming agent and a foaming activator are added to the homogenizing section at the rear end of the screw of the core layer extruder 100 according to the ratio in Table 1, and the temperature is maintained at 190°C for foaming, and extruded into the core layer mold for foaming molding, and then cooled to 50°C through the core layer cooling mold 101 for pre-molding to obtain a foamed core layer;

[0078] Step 3) Surface co-extrusion coating:

[0079] The two prepared surface layer mixtures are respectively put into the hoppers of two surface layer extruders 200, the head of one surface layer extruder 200 is connected to the barrel of the other surface layer extruder 200 at one third of the side close to the hopper through a confluence core 201, and the two surface layer extruders 200 melt and plasticize the poured surface layer mixtures at 200°C to obtain surface co-extruded materials, and the surface co-extruded materials of one surface layer extruder 200 are merged into the other surface extruder 200 through the confluence core 201. At the same time, the foaming core layer passes through the center of the co-extrusion die 300, and the melted surface co-extruded materials of two different colors are mixed and extruded to the co-extrusion die 300, and coated on the surface of the foaming core layer substrate to form a surface co-extruded layer with imitation wood pattern;

[0080] Step 4) Cooling and shaping:

[0081] After being extruded by the co-extrusion die, the co-extrusion cooling die 301 is cooled to 40° C. to set the shape, thereby obtaining a HDPE co-extruded foamed board with imitation wood grain.

[0082] Embodiment 4-6

[0083] The difference from Example 3 is that the raw material dosages of Examples 4-6 are different, see Table 1 for details.

[0084] Table 1. Raw materials and dosage of Examples 1-6 (unit: kg)

[0085]

[0086]

[0087] The raw materials used in this application are commercially available products except for the following special instructions:

[0088] High-density polyethylene and HDPE use YEM-4902T high-density polyethylene from Yangzi Petrochemical;

[0089] The coated polytetrafluoroethylene particles use the DL-155 anti-dripping agent produced by Dongguan Xinrui New Materials Co., Ltd., with a PTFE content of 55%;

[0090] The ultra-high molecular weight polyethylene uses American Ticona GUR 4150 ultra-high molecular weight polyethylene;

[0091] The cross-linking agent used was TAIC cross-linking agent from Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0092] The compatibilizer is HDPE-g-MAH compatibilizer with the brand number 40E529 from DuPont Company of the United States;

[0093] The anti-UV masterbatch is 2207 anti-UV masterbatch from Covestro of Germany.

[0094] Comparative Example

[0095] Comparative Example 1: A co-extruded foamed board, which is different from Example 1 in that, in step 1) of Comparative Example 1, no melt enhancer is added when preparing the core layer concrete.

[0096] Comparative Example 2: A co-extruded foamed board, which is different from Example 1 in that, in step 1) of Comparative Example 2, an equal mass of HDPE is used to replace the vinyl copolymer when granulating the high-energy particles of the surface co-extruded layer.

[0097] Comparative Example 3: A co-extruded foam board, which is different from Example 1 in that, in step 1) of Comparative Example 3, the high-energy particles of the surface co-extruded layer are granulated with an equal mass of HDPE polyethylene-based elastomer.

[0098] Comparative Example 4: A co-extruded foamed board, which is different from Example 1 in that, in step 1) of Comparative Example 4, no surface filler and compatibilizer are added when the surface co-extruded layer high-energy particles are granulated.

[0099] Performance testing

[0100] Test sample objects: The imitation wood grain HDPE co-extruded foamed boards prepared in the above Examples 1-6 are used as experimental samples 1-6, and the co-extruded foamed boards prepared in Comparative Examples 1-4 are used as control samples 1-4.

[0101] Test reference standards: According to the test method of ASTM D4060-14, the wear resistance of the sample objects is tested using a Taber abrasion tester; according to the test method of BS EN 15534-1:2014, the impact resistance of the sample objects is tested using an impact ball; according to GB 2411-1980 (1989) Plastic Shore Hardness Test Method, the surface hardness of the sample objects is tested using a D-type hardness tester; according to the sample method of GB / T 16422.3-2014 Plastic Laboratory Light Source Exposure Test Method Part 3: Fluorescent Ultraviolet Lamp and GB / T 9341 Plastic Bending Performance Test Method, UVA-340 fluorescent ultraviolet lamp is used for irradiation and irradiation for 200 hours using method A in the standard to test the aging resistance of the sample objects.

[0102] Test results: Each sample object is set as five parallel groups for performance testing, among which the average wear mass of the five groups of sample objects is used as the evaluation of wear resistance; the number of "pass" or "failure" after the impact ball is recorded, and the cumulative number of "failures" is used as the evaluation of impact resistance; the average Shore hardness of the five groups of sample objects is used as the evaluation of surface hardness; the average bending strength of the five groups of sample objects after accelerated aging by ultraviolet irradiation is used as the evaluation of aging resistance. The test results of each test sample object are detailed in Table 2.

[0103] Table 2. Performance test results

[0104] project Wear quality Impact failure times Surface hardness Bending strength Experimental sample 1 39.8mg 0 75D 17.6Mpa Experimental sample 2 38.5mg 0 80D 18.4Mpa Experimental sample 3 38.0mg 0 77D 20.8Mpa Experimental sample 4 38.2mg 0 78D 21.2Mpa Experimental sample 5 37.3mg 0 82D 22.7Mpa Experimental sample 6 37.7mg 0 81D 23.0Mpa Control sample 1 41.0mg 4 74D 15.2Mpa Control sample 2 47.6mg 4 68D 13.4Mpa Control sample 3 46.9mg 5 72D 12.0Mpa Control sample 4 49.2mg 2 54D 15.9Mpa

[0105] According to the test results in Table 2, the wear masses of experimental samples 1-6 are all below 40 mg, there is no impact failure in the impact resistance test, and the surface hardness is above 75D. It can be seen that the foamed co-extruded layer formed by coating the foamed core layer with the surface co-extruded layer has mechanical properties similar to those of the non-porous sheet, and has better wear resistance and impact resistance than the traditional polyethylene foamed sheet.

[0106] In addition, the experimental samples 1-6 have better wear resistance and impact resistance than the control sample 1, indicating that the addition of the melt enhancer is beneficial to improving the overall mechanical properties of the co-extruded foam board; and the experimental samples 1-6 have not only higher wear resistance and impact resistance than the control samples 2-4, but also higher surface hardness, indicating that the vinyl copolymer, polyethylene elastomer and surface filler can make the quality of the co-extruded foam board more excellent. In addition, after light aging treatment, the bending strength of the experimental samples 1-6 still maintains a higher level than that of the control samples 2-3, indicating that the addition of vinyl copolymers and polyethylene elastomers is beneficial to improve the bonding strength between the surface co-extruded layer and the foamed core layer, making it less likely for the co-extruded foam board to have a surface layer detachment, thereby having better durability.

[0107] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing a wood-grain imitation HDPE co-extruded foamed board, characterized in that: The method comprises the following preparation steps: Step 1) Prepare the ingredients: Core layer mixture: by weight, 40-80 parts of high-density polyethylene, 5.15-10.5 parts of melt enhancer, 10-40 parts of core layer filler, and 0.5-1.5 parts of cross-linking agent are mixed evenly to obtain a core layer mixture for later use; The melt enhancer comprises: 0.15-0.5 parts of coated polytetrafluoroethylene particles and 5-10 parts of ultra-high molecular weight polyethylene; Surface layer mixture: by weight, 65-90 parts of HDPE, 3-5 parts of vinyl copolymer, 5-10 parts of polyethylene elastomer, 3-10 parts of surface filler, and 1-5 parts of compatibilizer are mixed and plasticized to obtain surface co-extrusion layer functional particles, the surface co-extrusion layer functional particles are divided into two parts, and then 2-3 parts of surface masterbatches of different colors are respectively mixed to obtain two parts of surface layer mixtures for standby use; the vinyl copolymer is a combination of EAA, EEA, and EMAA; The polyethylene-based elastomer is a combination of one or more of POE, TPO and EVA; Step 2) extruding a foamed core layer: pouring the prepared core layer mixture into the hopper of a core layer extruder (100) for melting and plasticizing, adding 0.4-5 parts of a foaming agent and 0.4-2 parts of a foaming activator to the homogenizing section at the rear end of the screw of the core layer extruder (100) for foaming, and extruding into a core layer mold for foaming molding, and then passing through a core layer cooling mold (101) for pre-molding to obtain a foamed core layer; Step 3) surface co-extrusion coating: two prepared surface mixtures are respectively put into the hoppers of two surface extruders (200), and the two surface extruders (200) melt and plasticize the poured surface mixtures to obtain surface co-extrusion materials. The surface co-extrusion materials of one surface extruder (200) are merged into the other surface extruder (200) through the confluence core (201). At the same time, the foaming core layer passes through the center of the co-extrusion die (300), and the melted surface co-extrusion materials of two different colors are mixed and extruded into the co-extrusion die (300), and coated on the surface of the foaming core layer substrate to form a surface co-extrusion layer with imitation wood pattern; Step 4) Cooling and shaping: After extrusion by the co-extrusion die, the co-extrusion cooling die (301) is used for shaping to obtain a HDPE co-extruded foamed board with imitation wood grain.

2. The method for preparing a wood-grain imitation HDPE co-extruded foam board according to claim 1 is characterized in that, by weight, the core layer mixture also includes 1-2 parts of a dispersant, and the dispersant is a combination of one or more of stearic acid, zinc stearate, and calcium stearate.

3. The method for preparing a wood-grain imitation HDPE co-extruded foamed board according to claim 1, characterized in that the foaming agent is a combination of one or more of sodium bicarbonate and azodicarbonamide, and the foaming activator is zinc oxide.

4. The method for preparing a wood-grain imitation HDPE co-extruded foamed board according to claim 1, characterized in that the surface filler is a combination of one or more of hollow glass microspheres, fumed silica, and talcum powder.

5. The method for preparing a wood-grain imitation HDPE co-extruded foamed board according to any one of claims 1 to 4, characterized in that: When preparing the functional particles of the surface co-extrusion layer, the plasticizing and granulating temperature is 160-200°C; when preparing the foaming core layer, the plasticizing temperature of the feeding section of the core layer extruder (100) is 140-160°C, and the foaming temperature of the homogenizing section is 180-200°C; when preparing the surface co-extrusion layer, the working temperature of the surface layer extruder (200) is 190-210°C.

6. A wood-grain imitation HDPE co-extruded foam board, characterized in that: The imitation wood grain HDPE co-extruded foamed board is prepared by the preparation method of the imitation wood grain HDPE co-extruded foamed board according to any one of claims 1 to 5.

7. A HDPE surface co-extruded layer functional particle, characterized in that: The surface co-extruded layer functional particles are the surface co-extruded layer functional particles obtained by granulation in step 1) of the preparation method of the imitation wood grain HDPE co-extruded foam board according to any one of claims 1 to 6.