A method for preparing rutin hydrogel with optical activity
Through the hydrogen bond interaction between acrylic hydrogels and rutin, a stable and optically active rutin hydrogel is prepared, which solves the leakage problem of rutin gel materials in transportation and storage and gives them optical activity. , suitable for the preparation of smart materials.
Patent Information
- Application Number
- CN202111394820.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-23
AI Technical Summary
Existing rutin gel materials are prone to rutin leakage during processing, transportation and storage, and are easily oxidized, limiting their stability and application range.
Acrylic hydrogel is used to initiate copolymerization with N,N'-methylenebisacrylamide through initiator to form hydrogen bond interaction with phenolic hydroxyl groups in rutin solution, and prepare rutin hydrocoagulation with hydrogen bonding force Glue, isolates rutin from air, enhances its stability and imparts optical activity.
Through hydrogen bonding, the rutin molecules are fixed, the non-radiative energy loss is reduced, the fluorescence emission intensity is enhanced, the structural stability and optical performance of rutin hydrogel are improved, and it is suitable for the preparation of intelligent optical materials and expanding its application prospects.
Smart Images

Figure CN114045167B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of luminescent material preparation, and in particular relates to a method for preparing rutin hydrogel with optical activity. Background Art
[0002] Hydrogel is a new type of material that has emerged in recent years. It is a functional polymer material with a three-dimensional network structure formed by hydrophilic polymers. The highly cross-linked polymer network gives hydrogel excellent water retention and good mechanical, chemical and biological properties. Due to its excellent structural properties, hydrogel can be processed into various required shapes and endowed with new functions, so it is widely used in the fields of medicine, materials, and chemical industry.
[0003] Rutin is a common flavonoid compound, a natural product, widely present in the roots, stems, leaves, flowers and fruits of plants, with multiple biological activities such as anti-oxidation, anti-tumor, anti-inflammatory, and protection of cardiovascular and cerebrovascular vessels, and can be used in food, cosmetics, medical and health industries. Rutin is a 3-O-rutinoside of quercetin, which is easily destroyed in the gastrointestinal tract, limiting the clinical application of rutin. In order to improve its stability in the body and prevent rutin from being exposed to air and oxidized, researchers have reformed the dosage form of rutin using gel materials as carriers. For example, Wei Yachao et al. (In vitro drug release behavior of PLGA-PEG-PLGA thermosensitive hydrogel [J]. Journal of Qingdao University of Science and Technology (Natural Science Edition), 2014, 35 (02): 170-173.]) wrapped troxerutin tablets in PLGA-PEG-PLGA hydrogel to achieve the purpose of sustained release of troxerutin tablets. Jiang Yachao et al. (Study on the Preparation Technology of Rutin Hydrogel Gastric Floating Tablets [J]. Guangzhou Chemical Industry, 2021, 49(15): 49-51.) wrapped rutin with HPMC gel material to prepare rutin gastric floating tablets, thereby achieving the purpose of sustained release of rutin.
[0004] At present, the method for preparing rutin gel material is mainly physical embedding method, the interaction between rutin and gel is weak, and rutin may leak during processing, transportation and storage, thus making it lose its function. Therefore, it is necessary to develop a new type of rutin gel material. Summary of the invention
[0005] In view of the above problems existing in the prior art, in order to strengthen the interaction between rutin and gel material, the purpose of the present invention is to provide a method for preparing rutin hydrogel.
[0006] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing an optically active rutin hydrogel comprises the steps of drying an acrylic hydrogel and immersing the dried acrylic hydrogel in a rutin solution to fully swell and adsorb rutin to obtain the rutin hydrogel.
[0008] Furthermore, the acrylic hydrogel is obtained by copolymerizing acrylic acid and N,N'-methylenebisacrylamide initiated by an initiator.
[0009] Furthermore, the initiator is a persulfate compound.
[0010] Furthermore, the initiator is ammonium persulfate.
[0011] Furthermore, the mass ratio of acrylic acid to N,N'-methylenebisacrylamide is (100-600):1.
[0012] Furthermore, the mass ratio of acrylic acid to persulfate compound is (100-300):1.
[0013] Furthermore, acrylic acid and N,N'-methylenebisacrylamide are both in the form of ethanol or methanol solution with a volume fraction of 20% to 60%.
[0014] Furthermore, the copolymerization reaction conditions are as follows: the temperature is controlled at 40-60° C. and the reaction time is 30-60 min.
[0015] Furthermore, the drying method is freeze drying.
[0016] Furthermore, the rutin solution is an alcohol solution containing rutin, and the rutin concentration is 0.5 to 1.5 mg·mL -1 .
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The present invention prepares a novel rutin gel material, so that rutin and hydrogel form rutin hydrogel through hydrogen bonding, thereby isolating rutin from air and solving the problem that rutin is easily oxidized.
[0019] (2) The inventor unexpectedly discovered that the prepared rutin hydrogel also has optical activity. The structure of rutin is shown below:
[0020]
[0021] It has a larger conjugated system and a certain aggregation-induced emission effect (AIE), but the luminescence is weak. The inventor believes that when the rutin hydrogel material is formed, the hydroxyl group of rutin and the hydrogel interact through hydrogen bonds. The formation of hydrogen bonds makes rutin "fixed", greatly limiting the vibration and rotation of rutin molecules, hindering non-radiative transitions, reducing energy loss between systems, releasing more energy in the form of radiation, and significantly enhancing the fluorescence emission intensity.
[0022] (3) Rutin imparts optical activity to hydrogel materials, and hydrogel materials are easy to process. Therefore, rutin hydrogel materials can be used in the preparation of intelligent optical materials such as sensors, target recognition, and photothermal switches, and have broad application prospects.
[0023] (4) The acrylic hydrogel of the present invention contains carboxyl groups, which can form hydrogen bonds with the phenolic hydroxyl groups in rutin. The interaction force is strong, and the formed rutin hydrogel has a stable structure and rutin is not easy to dissociate. The preparation of acrylic hydrogel is simple, the reaction conditions are mild, and the formed hydrogel has a strong structure and is not easy to break.
[0024] (5) The preparation method of the present invention is simple, fast, low-cost, and suitable for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the infrared spectrum of rutin;
[0026] Figure 2 is the infrared spectrum of the hydrogel;
[0027] Figure 3 is the infrared spectrum of rutin hydrogel;
[0028] Figure 4 This is the fluorescence spectrum of rutin;
[0029] Figure 5 is the fluorescence spectrum of the hydrogel;
[0030] Figure 6 is the fluorescence spectrum of rutin hydrogel;
[0031] Figure 7 The concentration of rutin is 0.05 mg mL -1 Fluorescence spectrum of rutin hydrogel material prepared at ;
[0032] Figure 8 The concentration of rutin is 0.1 mg mL -1 Fluorescence spectrum of rutin hydrogel material prepared at ;
[0033] Fig. 9 The concentration of rutin is 0.3 mg mL-1 Fluorescence spectrum of rutin hydrogel material prepared. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with specific embodiments.
[0035] The swelling ratio was calculated according to the following formula:
[0036]
[0037] Where: SR——equilibrium swelling rate of hydrogel
[0038] W S ——Dry hydrogel mass (g)
[0039] W T ——Mass of hydrogel at swelling equilibrium (g)
[0040] Example 1
[0041] Accurately weigh 15g of acrylic acid and 0.075g of N,N'-methylenebisacrylamide, dissolve them in 20mL of 30% ethanol solution respectively, add them into a beaker to mix, react at 60°C, stir thoroughly, and after 10 minutes, weigh 0.04g of ammonium persulfate, dissolve it in 5mL of distilled water, and add it dropwise to the mixed solution of acrylic acid and N,N'-methylenebisacrylamide. Continue to react for 60 minutes. After the solution becomes viscous, stop heating and cool it naturally to room temperature to obtain a clear, transparent and regularly shaped polyacrylic acid hydrogel.
[0042] Weigh a certain amount of rutin and dissolve it in 50% ethanol solution to prepare a concentration of 0.5 mg mL -1 The hydrogel was cut into pieces, freeze-dried and weighed, and the dried hydrogel was immersed in a rutin solution for 48 hours to fully swell and adsorb rutin, thereby obtaining a rutin hydrogel with a swelling rate of 2735%.
[0043] Example 2
[0044] Accurately weigh 7.5g of acrylic acid and 0.03g of N,N'-methylenebisacrylamide, dissolve them in 15mL of 40% ethanol solution respectively, add them into a beaker to mix, react at 50°C, stir thoroughly, after 10min, weigh 0.03g of ammonium persulfate, dissolve it in 5mL of distilled water, add it dropwise to the mixed solution of acrylic acid and N,N'-methylenebisacrylamide, continue to react for 30min, stop heating after the solution becomes viscous, and naturally cool to room temperature to obtain a clear, transparent and regularly shaped polyacrylic acid hydrogel.
[0045] Weigh a certain amount of rutin and dissolve it in 50% ethanol solution to prepare a concentration of 1.5 mg mL -1The hydrogel was cut into pieces, freeze-dried and weighed, and the dried hydrogel was immersed in a rutin solution for 48 hours to fully swell and adsorb rutin, thereby obtaining a rutin hydrogel with a swelling rate of 2227%.
[0046] Example 3
[0047] Accurately weigh 30g of acrylic acid and 0.05g of N,N'-methylenebisacrylamide, dissolve them in 25mL of 50% methanol solution respectively, add them into a beaker to mix, react at 40°C, stir thoroughly, after 10min, weigh 0.1g of ammonium persulfate, dissolve it in 5mL of distilled water, add it dropwise to the mixed solution of acrylic acid and N,N'-methylenebisacrylamide, continue to react for 40min, stop heating after the solution becomes viscous, and naturally cool to room temperature to obtain a clear, transparent and regularly shaped polyacrylic acid hydrogel.
[0048] Weigh a certain amount of rutin and dissolve it in 50% ethanol solution to prepare a concentration of 1 mg mL -1 The hydrogel was cut into pieces, freeze-dried and weighed, and the dried hydrogel was immersed in a rutin solution for 48 hours to fully swell and adsorb rutin, thereby obtaining a rutin hydrogel with a swelling rate of 2458%.
[0049] Example 4
[0050] 7.5 g of acrylic acid and 0.03 g of N,N'-methylenebisacrylamide were accurately weighed, dissolved in 25 mL of 30% ethanol solution respectively, added to a beaker for mixing, reacted at 40°C, and stirred thoroughly for 10 minutes. 0.03 g of potassium persulfate was weighed, dissolved in 5 mL of distilled water, and added dropwise to the mixed solution of acrylic acid and N,N'-methylenebisacrylamide. The solution became viscous and began to react violently for about 10 minutes, generating a large number of bubbles and splashing liquid, posing potential safety issues. The resulting hydrogel had poor uniformity and contained many bubbles, so rutin hydrogel was not further prepared.
[0051] Example 5
[0052] Polyvinyl alcohol hydrogel is used to replace acrylic hydrogel for the preparation of rutin hydrogel. The specific reaction process is: weigh 10g of polyvinyl alcohol, dissolve it in 70g of water, heat and stir at 90°C, and after the polyethylene is completely dissolved, place the sample at -20°C and freeze it for 24h. After taking it out, place it at room temperature for 2h, freeze it again at -20°C, and freeze it repeatedly 3-5 times to obtain polyvinyl alcohol hydrogel. The preparation process is complicated and the reaction conditions are harsh. Moreover, since polyvinyl alcohol hydrogel is formed by hydrogen bonding, it has poor mechanical strength and is easy to dissociate at room temperature, which not only affects the test, but also dissolves during the preparation of rutin hydrogel, and rutin hydrogel cannot be obtained.
[0053] Example 6
[0054] Weigh a certain amount of rutin and dissolve it in 50% ethanol solution to prepare concentrations of 0.05, 0.1 and 0.3 mg mL -1 The hydrogel obtained in Example 1 was cut into pieces, freeze-dried and weighed, and the dried hydrogel was immersed in a rutin solution for 48 hours to fully swell and absorb rutin, thereby obtaining a rutin hydrogel.
[0055] The luminescence performance of the rutin hydrogel was tested using a fluorescence spectrometer under the following test conditions: excitation slit 7.5nm, emission slit 2.5nm, excitation wavelength 380nm. Figures 7 to 9 As shown, the rutin concentrations are 0.05, 0.1, and 0.3 mg mL -1 The luminescence properties of the rutin hydrogel material prepared by the adsorption of 0.5 mg·mL -1 The rutin solution is low.
[0056] The theoretical basis for rutin hydrogel to isolate rutin from air: rutin contains phenolic hydroxyl groups, which have strong antioxidant activity and are easily oxidized into quinone compounds, consuming reactive oxygen species, thus achieving an antioxidant effect. In rutin hydrogel, the hydroxyl groups in rutin interact with the carboxyl groups in the hydrogel (taking acrylic hydrogel as an example) through hydrogen bonds, and the phenolic hydroxyl groups are not easily oxidized into quinone compounds; at the same time, the rutin adsorbed inside the hydrogel is isolated from the air, is not easily exposed to reactive oxygen species, and is even less likely to be oxidized.
[0057] The hydrogel and the rutin hydrogel (Example 1) were freeze-dried, and the structures of the rutin, the hydrogel and the rutin hydrogel were characterized by infrared spectrometer. Figure 1 The infrared spectrum of rutin is 3348~3423cm -1 is the stretching vibration absorption peak of OH, 2905~2935cm -1 The CH2 stretching vibration absorption peak of rutinose is 1652 cm -1 is the stretching vibration absorption peak of C=O, 1598cm -1 and 1504cm -1 is the stretching vibration absorption peak of the benzene ring, 1458cm -1 is the shear vibration absorption peak of CH2, 1361 is the bending vibration absorption peak of CH3, and 1012-1296 is the stretching vibration of CO. Figure 2 This is the infrared spectrum of the hydrogel, 2000~3600cm -1 It is a peak-like absorption peak formed by the superposition of the characteristic peaks of the associated OH in the carboxyl group of polyacrylic acid and the characteristic peaks of the alkyl group, 1696cm -1The C=O stretching vibration absorption peak of the carboxyl group of polyacrylic acid is 1446 cm -1 and 1407cm -1 Bending vibration of the alkane of polyacrylic acid, 1232 cm -1 and 1162cm -1 These are the antisymmetric and symmetric stretching vibration absorption peaks of the CO bond of the polypropylene part. Figure 3 This is the infrared spectrum of rutin hydrogel, 2000~3600cm -1 is the stretching vibration absorption peak of OH, among which 3347cm -1 and 3422cm -1 The absorption peak at 2858 cm-1 is consistent with the hydroxyl stretching vibration absorption peak of rutin. -1 and 2935cm -1 The stretching vibration absorption peak of CH2 at 1700cm is similar to that of rutinose. -1 The C=O stretching vibration absorption peak of the carboxyl group of polyacrylic acid is 1650cm -1 The peak of C=O stretching vibration of rutin is 1596cm -1 and 1500cm -1 It is the stretching vibration absorption peak of the benzene ring of rutin, 1449cm -1 and 1404cm -1 Bending vibration of the alkane of polyacrylic acid, 1358 cm -1 It is the bending vibration absorption peak of methyl group, 1010~1290cm -1 is the stretching vibration of CO, among which 1232cm -1 and 1161cm -1 The absorption peaks are the antisymmetric and symmetric stretching vibration absorption peaks of the CO bond of the polypropylene part. Infrared data show that rutin hydrogel has the characteristic absorption peaks of both rutin and polyacrylic acid hydrogel, and some absorption peak shifts change, especially the shape of the OH absorption peak in rutin hydrogel also changes, indicating that rutin and hydrogel form rutin hydrogel through hydrogen bonding.
[0058] The luminescence properties of rutin, hydrogel and rutin hydrogel (Example 1) were tested using a fluorescence spectrometer under the following test conditions: excitation slit 7.5nm, emission slit 2.5nm, excitation wavelength 380nm. Figures 4 to 6 shown. Figure 4 This is the fluorescence emission spectrum of rutin. When rutin is excited at 380nm, it produces a fluorescence emission peak at 400nm-600nm, and the maximum emission peaks are at 465nm, 486nm and 530nm respectively. Figure 5This is the fluorescence emission spectrum of the hydrogel. The fluorescence emission peak is weak in the range of 400nm-600nm, and there are several small bulges at 401nm, 422nm and 484nm. Figure 6 This is the fluorescence emission spectrum of rutin hydrogel, which produces a strong fluorescence emission peak at 400nm-600nm, and the maximum emission peaks are at 427nm, 443nm, 486nm and 530nm, respectively, which are consistent with the fluorescence emission peaks of rutin and hydrogel, and the fluorescence intensity is significantly enhanced, and the peak shape is also changed, further indicating that rutin and hydrogel in rutin hydrogel interact through hydrogen bonds, and the synergistic effect makes rutin hydrogel have excellent optical properties.
Claims
1. A method for preparing an optically active rutin hydrogel, characterized in that: After drying, the acrylic hydrogel is immersed in a rutin solution to fully swell and adsorb rutin to obtain the rutin hydrogel; The acrylic hydrogel is obtained by copolymerizing acrylic acid and N,N'-methylenebisacrylamide initiated by an initiator; The mass ratio of acrylic acid to N,N'-methylenebisacrylamide is (100~600):
1.
2. The preparation method according to claim 1, characterized in that: The initiator is a persulfate compound.
3. The preparation method according to claim 2, characterized in that: The initiator is ammonium persulfate.
4. The preparation method according to claim 1, characterized in that: The mass ratio of acrylic acid to initiator is (100~300):
1.
5. The preparation method according to claim 1, characterized in that: The conditions for the copolymerization reaction are that the temperature is controlled at 40~60°C and the reaction time is 30~60min.
6. The preparation method according to claim 1, characterized in that: Acrylic acid and N,N'-methylenebisacrylamide are both prepared in ethanol or methanol solutions with a volume fraction of 20% to 60%.
7. The preparation method according to claim 6, characterized in that: The specific copolymerization method is: mixing acrylic acid solution and N,N'-methylenebisacrylamide solution, reacting at 40-60°C, adding ammonium persulfate after 5-15 minutes, and continuing the reaction for 30-60 minutes. After the solution becomes viscous, stop heating and cool naturally to room temperature to obtain the rutin hydrogel.
8. The method for preparing the optically active rutin hydrogel according to claim 1, characterized in that: The drying method is freeze drying.
9. The method for preparing the optically active rutin hydrogel according to claim 1, characterized in that: Rutin solution is an alcohol solution containing rutin, with a rutin concentration of 0.5~1.5 mg•mL -1 .