Polyvinyl alcohol film, stretched film, polarizing film, and method for producing polyvinyl alcohol film
By introducing a modified conjugated diene polymer into the PVA film to improve its stretching processability and formability, and removing attachments with water, the problems in stretching processing and productivity of the PVA film are solved, and high efficiency is achieved. Polarizing film forming.
Patent Information
- Application Number
- CN202080050406.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-07-10
AI Technical Summary
It is difficult for the existing PVA film to achieve high stretchability and low tensile stress at the same time during the stretching process, and the polarizing film is easily broken during the deformation process, and the rubber component is attached to the metal drum and is difficult to completely remove, affecting productivity.
Using a PVA film containing a modified conjugated diene polymer with hydrophilic groups, through reasonable polymerization degree and hydrophilic group content design, the stretchability and formability of the PVA film can be improved, and through Water removes rubber component attachments and improves productivity.
It achieves high stretchability and excellent productivity of the PVA film, and good formability of the polarizing film, avoiding the reduction in productivity caused by the adhesion of rubber components.
Smart Images

Figure DEST_PATH_IMAGE003 
Figure 429638DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The present invention relates to a polyvinyl alcohol film, a stretched film, a polarizing film and a method for producing the polyvinyl alcohol film. Background Art
[0002] Polyvinyl alcohol films (hereinafter, "polyvinyl alcohol" may be abbreviated as "PVA") are used in a wide range of application fields such as packaging films, water-soluble films, agricultural films, release films, and optical films.
[0003] Compared with other plastic films, PVA films without plasticizers are more rigid, and mechanical properties such as impact strength and process eligibility during secondary processing such as stretching sometimes become problems. In order to prevent these problems, products with improved flexibility by adding plasticizers to PVA films are usually used. In particular, when PVA films are used as raw materials for polarizing films, high stretchability is required during stretching, so products with improved stretching processability by adding plasticizers are used. However, PVA films containing such plasticizers have the problem that the plasticizer decreases over time and the stretching processability decreases.
[0004] To address this problem, as a method for imparting good stretchability by a method other than adding a plasticizer, in the case of PVA fibers, a method of adding an emulsified dispersion of ethylene-vinyl acetate copolymer to a spinning solution has been proposed (see Patent Document 1).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent document 1: Japanese Patent Publication No. 47-42050. Summary of the invention
[0008] Problems to be solved by the invention
[0009] On the other hand, as the use of PVA film, there is the use of PVA film implemented with various stretching treatments. In this use, high stretchability is required for the PVA film, and in order to reduce the residual stress that may cause problems such as deformation after processing, it is important to have low tensile stress.
[0010] However, in the method of adding the emulsified dispersion of the ethylene vinyl acetate copolymer, it is difficult to reduce the tensile stress of the PVA film while imparting high tensile properties, and the tensile processability of the PVA film is insufficient. In addition, there is a tendency that the greater the deformation speed of the PVA film, the greater the tensile stress of the PVA film. Therefore, a PVA film with a small tensile stress even at a high deformation speed is sought.
[0011] In addition, polarizing films obtained by stretching PVA films are used for optical purposes, mainly polarizing plates for liquid crystal displays and sunglasses. However, it is known that in recent years, when the polarizing films are further deformed, such as foldable displays and highly designed sunglasses, the polarizing films may break parallel to the stretching direction. The greater the deformation speed of the polarizing film, the more significant this problem becomes. Therefore, a polarizing film with excellent formability that does not break even when deformed at a high deformation speed is sought.
[0012] Here, the inventors of the present invention have found that by adding a rubber component to PVA, the stretching processability of the obtained PVA film, and the formability of the stretched film and the polarizing film can be improved. However, when the rubber component is added, when the film-making stock solution is cast onto the surface of a substrate such as a metal drum to manufacture the PVA film, a new problem arises in which the rubber component adheres to the substrate of the metal drum, etc. If the amount of the rubber component attached to the substrate of the metal drum, etc. increases, it sometimes becomes dirt and adheres to the PVA film. Therefore, it is necessary to remove the rubber component attached to the substrate of the metal drum, etc. by cleaning at any time. However, when using, for example, isoprene rubber, etc. as the rubber component, it is sometimes difficult to fully remove it by water-based cleaning, etc. In this way, the rubber component (attachment) attached to the substrate of the metal drum, etc. is sometimes difficult to remove even if cleaning, etc. is performed, and sometimes the productivity is reduced due to operations such as cleaning, so it is not preferred.
[0013] The present invention is based on the above-mentioned situation, and its purpose is to provide the following PVA film, stretched film and polarizing film manufactured from such PVA film, and a method for manufacturing such PVA film, wherein the PVA film has excellent stretching processability and productivity and can obtain a stretched film and polarizing film with excellent formability.
[0014] Solutions for solving problems
[0015] The above purpose is achieved by providing the following technical solutions:
[0016] [1] A polyvinyl alcohol film comprising polyvinyl alcohol (A) and a modified conjugated diene polymer having a hydrophilic group (B);
[0017] [2] The polyvinyl alcohol film according to [1], wherein the content of the modified conjugated diene polymer (B) is 10 parts by mass or more and 80 parts by mass or less based on 100 parts by mass of the polyvinyl alcohol (A);
[0018] [3] The polyvinyl alcohol film according to [1] or [2], wherein the degree of polymerization of the polyvinyl alcohol (A) is 1,000 or more and 10,000 or less, and the degree of saponification is 95 mol % or more;
[0019] [4] The polyvinyl alcohol film according to any one of [1] to [3], wherein the modified conjugated diene polymer (B) has a weight average molecular weight of 5,000 or more and 80,000 or less;
[0020] [5] The polyvinyl alcohol film according to any one of [1] to [4], wherein the hydrophilic group is a graft chain having a repeating structure containing a nonionic polar group;
[0021] [6] A stretched film obtained from the polyvinyl alcohol film according to any one of [1] to [5];
[0022] [7] A polarizing film obtained from the polyvinyl alcohol film according to any one of [1] to [5] or the stretched film of [6];
[0023] [8] A method for producing a polyvinyl alcohol film, which includes a step of forming a film using a film-forming stock solution obtained by mixing polyvinyl alcohol (A) with a dispersion containing a modified conjugated diene polymer (B) having a hydrophilic group;
[0024] [9] The method for producing a polyvinyl alcohol film according to [8], wherein the content of the modified conjugated diene polymer (B) in the film-forming stock solution is 10 parts by mass or more and 80 parts by mass or less with respect to 100 parts by mass of polyvinyl alcohol (A);
[0025]
[10] The method for producing a polyvinyl alcohol film according to [8] or [9], wherein the hydrophilic group is a graft chain having a repeating structure containing a nonionic polar group.
[0026] Advantages of the Invention
[0027] According to the present invention, there can be provided the following PVA film, a stretched film and a polarizing film produced from such a PVA film, and a method for producing such a PVA film. The PVA film has excellent stretchability and productivity, and a stretched film and a polarizing film with excellent formability can be obtained. Detailed Description of Embodiments
[0028] Hereinafter, embodiments of the PVA film, a method for producing the same, a stretched film, and a polarizing film of the present invention will be described in detail.
[0029] <PVA Film>
[0030] The PVA film according to one embodiment of the present invention contains PVA (A) and a modified conjugated diene polymer (B) having a hydrophilic group. This PVA film is usually an unstretched film (non-stretched film). As described in detail later, a stretched film is obtained by stretching this PVA film. Further, a polarizing film is obtained by subjecting this PVA film or this stretched film to dyeing processing or the like.
[0031] The PVA film has excellent stretching processability due to the inclusion of the modified conjugated diene polymer (B), and can also obtain a stretched film and a polarizing film with excellent formability. Furthermore, by providing the modified conjugated diene polymer (B) contained in the PVA film with a hydrophilic group, even when the modified conjugated diene polymer (B) is attached to a substrate such as a metal drum, the attached matter can be easily removed by water or the like. Therefore, the productivity of the PVA film is also excellent.
[0032] [PVA(A)]
[0033] PVA (polyvinyl alcohol) (A) is usually the main component of the PVA film. PVA (A) is a polymer having a vinyl alcohol unit (-CH2-CH (OH)-) as a main structural unit. It should be noted that the main structural unit refers to the structural unit that accounts for the largest proportion of all structural units, and the proportion of all structural units is preferably 50 mol% or more (hereinafter, the same applies to "main structural unit"). In addition to the vinyl alcohol unit, PVA (A) may also have a vinyl ester unit and other units.
[0034] As PVA (A), PVA obtained by saponifying polyvinyl ester obtained by polymerizing one or more vinyl esters can be used. As vinyl esters, vinyl acetate, vinyl formate, vinyl propionate, vinyl butyrate, vinyl pivalate, vinyl versatate, vinyl laurate, vinyl stearate, vinyl benzoate, isopropenyl acetate, etc. can be listed. Among the vinyl esters, from the viewpoints of ease of manufacture, ease of acquisition, cost, etc., preferably, a compound having a vinyloxycarbonyl group (H2C=CH-O-CO-) in the molecule is used, and more preferably vinyl acetate.
[0035] The polyvinyl ester is preferably a polyvinyl ester obtained by using only one or more vinyl esters as monomers, and more preferably a polyvinyl ester obtained by using only one vinyl ester as a monomer. As long as the effect of the present invention is not significantly impaired, it can be a copolymer resin formed by one or more vinyl esters and other monomers copolymerizable therewith.
[0036] The upper limit of the ratio of the structural unit derived from other copolymerizable monomers is preferably 15 mol%, more preferably 10 mol%, further preferably 5 mol%, and further preferably 1 mol%, depending on the molar number of all structural units constituting the copolymer resin. The lower limit of the ratio of the vinyl alcohol unit in the PVA (A) obtained by saponifying the polyvinyl ester to all structural units is preferably 85 mol%, more preferably 90 mol%, further preferably 95 mol%, and further preferably 99 mol%.
[0037] Examples of other monomers copolymerizable with vinyl esters include α-olefins having 2 to 30 carbon atoms, such as ethylene, propylene, 1-butene, and isobutylene; (meth)acrylic acid or its salts; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; (meth)acrylamide; N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, diacetone (meth)acrylamide, (meth)acrylamide propanesulfonic acid or its salts, (meth)acrylamide propanesulfonic acid or its salts, ) (meth)acrylamide derivatives such as acrylamidopropyldimethylamine or its salts, N-hydroxymethyl(meth)acrylamide or its derivatives; N-vinylamides such as N-vinylformamide, N-vinylacetamide, N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether; vinyl cyanide such as (meth)acrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters or anhydrides; itaconic acid or its salts, esters or anhydrides; vinyl silyl compounds such as vinyltrimethoxysilane; unsaturated sulfonic acids or their salts, etc.
[0038] The polyvinyl ester may have a structural unit derived from one or two or more of the above-mentioned monomers.
[0039] As PVA(A), PVA that has not been graft copolymerized can be preferably used. Among them, as long as the effect of the present invention is not significantly impaired, PVA(A) can be modified using one or more graft copolymerizable monomers. At least one of polyvinyl ester and PVA obtained by saponifying it can be graft copolymerized. Examples of graft copolymerizable monomers include unsaturated carboxylic acids or derivatives thereof; unsaturated sulfonic acids or derivatives thereof; α-olefins having 2 to 30 carbon atoms, etc. The proportion of structural units derived from graft copolymerizable monomers in polyvinyl ester or PVA(A) is preferably 5 mol% or less based on the molar number of all structural units constituting polyvinyl ester or PVA(A).
[0040] A part of the hydroxyl groups in PVA (A) may be cross-linked or not cross-linked. In addition, a part of the hydroxyl groups in PVA (A) may react with an aldehyde compound such as acetaldehyde or butyraldehyde to form an acetal structure.
[0041] The lower limit of the degree of polymerization of PVA (A) is preferably 1,000, more preferably 1,500, and further preferably 1,700. By making the degree of polymerization of PVA (A) greater than the above lower limit, the toughness of the PVA film, the resulting stretched film, and the polarizing film can be improved. On the other hand, the upper limit of the degree of polymerization is preferably 10,000, more preferably 8,000, and further preferably 5,000. By making the degree of polymerization of PVA (A) less than the above upper limit, the increase in the manufacturing cost of PVA (A) and the occurrence of defects during film making can be suppressed. It should be noted that the degree of polymerization of PVA (A) refers to the average degree of polymerization measured in accordance with the description of JIS K6726-1994.
[0042] As the lower limit of the saponification degree of PVA (A), for example, it can be 80 mol%, preferably 95 mol%, more preferably 98 mol%, and further preferably 99 mol%. By making the saponification degree more than the above lower limit, the effect of the present invention can be more fully exerted. In the case of the use of water-soluble film, PVA with a lower saponification degree can be used. On the other hand, the upper limit of the saponification degree can be 100 mol%. The saponification degree of PVA (A) refers to: the ratio (mol %) of the mole number of vinyl alcohol unit to the total mole number of vinyl alcohol unit relative to the structural unit (typically vinyl ester unit) that can be converted into vinyl alcohol unit by saponification. The saponification degree can be measured according to the record of JIS K6726-1994.
[0043] As the lower limit of the content of PVA (A) in the PVA film, it is sometimes preferably 60% by mass, more preferably 65% by mass, and further preferably 70% by mass, 75% by mass, 80% by mass or 85% by mass. By making the content of PVA (A) above the lower limit, the characteristics of PVA (A) can be fully utilized, and in addition, the transparency, smoothness, etc. of the obtained stretched film, polarizing film, etc. can be improved. On the other hand, as the upper limit of the content, it is sometimes preferably 99% by mass, more preferably 95% by mass, further preferably 90% by mass, and further preferably 85% by mass, 80% by mass, 75% by mass or 70% by mass. By making the content of PVA (A) below the upper limit, the formability of stretching processability, the obtained stretched film and polarizing film, etc. can be improved.
[0044] [Modified conjugated diene polymer (B)]
[0045] The modified conjugated diene polymer (B) is a conjugated diene polymer having a hydrophilic group. The modified conjugated diene polymer (B) may be a conjugated diene rubber having a hydrophilic group. For example, the modified conjugated diene polymer (B) is an unmodified conjugated diene polymer (B') (unmodified conjugated diene rubber) modified to introduce a hydrophilic group.
[0046] In the modified conjugated diene polymer (B), as a monomer unit constituting the polymer (usually the main chain of the polymer), a conjugated diene unit is included. That is, the modified conjugated diene polymer (B) is a polymer using a conjugated diene as a monomer. As a conjugated diene, for example, butadiene, isoprene, 2,3-dimethylbutadiene, 2-phenylbutadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,3-octadiene, 1,3-cyclohexadiene, 2-methyl-1,3-octadiene, 1,3,7-octatriene, myrcene, α-farnesene, β-farnesene, chloroprene, etc. can be listed. Among these, butadiene and isoprene are preferred, and isoprene is more preferred. In addition, the preferred structure (such as the configuration of monomer units) of the main chain of the modified conjugated diene polymer (B) may be the structure of the unmodified conjugated diene polymer (B′) described later.
[0047] The hydrophilic group possessed by the modified conjugated diene polymer (B) may be, for example, a group containing at least one of an oxygen atom and a nitrogen atom, and examples thereof include a hydroxyl group, a carboxyl group, an ester group (-COO-), an ether group (-O-), an amide group, a sulfonic group, an acid anhydride group, or a group containing one or more of these groups.
[0048] As the hydrophilic group, a graft chain having a repeating structure including a nonionic polar group is preferred. As the nonionic polar group, a hydroxyl group, an ester group, an ether group, an amide group, an acid anhydride group, etc. can be listed, preferably an ether group. The graft chain refers to a chain connected to the main chain directly or by means of other groups, but the synthesis method thereof is not specified.
[0049] Examples of the repeating structure containing a nonionic polar group include:
[0050] -(CR 2 R 3 -CR 4 R 5 -O)- represented by the polyalkylene glycol structure,
[0051] -(CH2-CR 7 COOR 8 )-shown poly (meth) acrylate structure, etc.,
[0052] A polyalkylene glycol structure is preferred.
[0053] The above R 2 , R 3 , R 4 and R 5 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 6 carbon atoms. 7 is a hydrogen atom or a methyl group. 8It is a monovalent hydrocarbon group having 1 to 6 carbon atoms. 8 A part or all of the hydrogen atoms of the hydrocarbon group shown may be substituted with a hydrophilic group.
[0054] As the above R 2 , R 3 , R 4 , R 5 and R 8 The monovalent hydrocarbon group having 1 to 6 carbon atoms shown in the formula (R) may include aliphatic hydrocarbon groups such as alkyl groups such as methyl, ethyl, and propyl groups, alkenyl groups such as vinyl groups, alicyclic groups such as cyclohexyl groups, and aromatic hydrocarbon groups such as phenyl groups. Among these, aliphatic hydrocarbon groups are preferred, and alkyl groups are more preferred. 2 , R 3 , R 4 and R 5 Each is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom.
[0055] The graft chain having a polyalkylene glycol structure is a hydrophilic group having a plurality of ether groups. The graft chain having a polyalkylene glycol structure can be represented by, for example, the following formula (A).
[0056] -(CR 2 R 3 -CR 4 R 5 -O) n -R 6 ・・・(A)
[0057] In formula (A), R 2 , R 3 , R 4 and R 5 Each R is independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 6 carbon atoms. 6 is a hydrogen atom, a monovalent hydrocarbon group having 1 to 6 carbon atoms, or an acyl group having 1 to 6 carbon atoms. n is an integer of 3 to 600.
[0058] The above R 2 , R 3 , R 4 and R 5 Each of R is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. 6 It is preferably a monovalent hydrocarbon group, more preferably an alkyl group, further preferably a methyl group and an ethyl group, and further preferably a methyl group. The lower limit of n is preferably 5, and more preferably 7. The upper limit of n is preferably 200, more preferably 100, and further preferably 40.
[0059] The graft chain having a poly(meth)acrylate structure can be represented by, for example, the following formula (B).
[0060] -(CH2-CR7 COOR 8 ) m -R 9 ・・・(B)
[0061] In formula (B), R 7 is a hydrogen atom or a methyl group. 8 It is a monovalent hydrocarbon group having 1 to 6 carbon atoms. 8 Some or all of the hydrogen atoms of the hydrocarbon group shown may be substituted with a hydrophilic group. 9 is a hydrogen atom or a monovalent organic group. m is an integer of 3 to 600. The organic group refers to a group containing carbon atoms, and examples thereof include a hydrocarbon group, an alkoxy group, an acyl group, a carboxyl group, or a group composed of a combination thereof.
[0062] Among the graft chains having a repeating structure including a nonionic polar group, a graft chain having a polyalkylene glycol structure is more preferred.
[0063] The average number of hydrophilic groups per molecule of the modified conjugated diene polymer (B) is preferably 1 to 30, more preferably 1 to 25, and even more preferably 1 to 20. Within the above range, the cleaning property of washing off deposits from the PVA film, that is, the productivity, is further improved.
[0064] The average number of hydrophilic groups per molecule of the modified conjugated diene polymer (B) can be determined from the equivalent weight (g / hydrophilic group-mol) of the hydrophilic group of the modified conjugated diene polymer (B) and the polystyrene-equivalent number average molecular weight Mn using the following formula.
[0065] (Average number of hydrophilic groups per molecule) = [(number average molecular weight Mn) / (molecular weight of styrene unit) × (average molecular weight of conjugated diene and other monomer units contained as required except conjugated diene)] / (equivalent weight of hydrophilic group)
[0066] It should be noted that the equivalent weight of the hydrophilic group of the modified conjugated diene polymer (B) refers to the mass of isoprene, butadiene and other monomers contained as required per 1 mol of the hydrophilic group. 1 H-NMR or 13 C-NMR was calculated based on the area ratio of the peak derived from the hydrophilic group to the peak derived from the polymer main chain.
[0067] In the modified conjugated diene polymer (B), about the position to be introduced into the hydrophilic group, it can be the polymerization end, it can also be the side chain of the polymer chain, from the viewpoint that a plurality of hydrophilic groups can be easily introduced, it is preferably the side chain of the polymer chain. In addition, the hydrophilic group can include 1 kind alone, it can also include more than 2 kinds. That is, the modified conjugated diene polymer (B) can utilize 1 kind of modified compound to be modified, in addition, it is also possible to utilize more than 2 kinds of modified compounds to be modified.
[0068] The melt viscosity of the modified conjugated diene polymer (B) measured at 38°C is preferably 0.1 to 4,000 Pa·s, more preferably 1 to 3,500 Pa·s, and further preferably 1 to 3,000 Pa·s. By making the melt viscosity of the modified conjugated diene polymer (B) within the above range, the stretching processability of the resulting PVA film, the formability of the stretched film and the polarizing film, etc. are improved. It should be noted that the melt viscosity of the modified conjugated diene polymer (B) is a value measured at 38°C using a Brookfield viscometer.
[0069] The weight average molecular weight (Mw) of the modified conjugated diene polymer (B) is preferably 5,000 or more and 80,000 or less, more preferably 6,000 or more and 50,000 or less, and further preferably 7,000 or more and 30,000 or less. The Mw of the modified conjugated diene polymer (B) is the weight average molecular weight calculated by gel permeation chromatography (GPC). By making the Mw of the modified conjugated diene polymer (B) within the above range, the process qualification during manufacturing is excellent and the economy becomes good. In addition, the stretching processability of the PVA film, the formability of the stretched film and the polarizing film, etc. are improved. It should be noted that two or more modified conjugated diene polymers (B) with different Mw can be used in combination.
[0070] The molecular weight distribution (Mw / Mn) of the modified conjugated diene polymer (B) is preferably 1.0 to 20.0, more preferably 1.0 to 15.0, and further preferably 1.0 to 10.0. By making Mw / Mn within the above range, the viscosity deviation of the modified conjugated diene polymer (B) becomes smaller, so it is preferred. It should be noted that the molecular weight distribution (Mw / Mn) refers to the ratio of the weight average molecular weight (Mw) / number average molecular weight (Mn) converted by standard polystyrene obtained by GPC measurement.
[0071] The vinyl content of the modified conjugated diene polymer (B) is 0 mol% or more and less than 100 mol%, preferably 1 mol% or more and less than 70 mol%, and more preferably 3 mol% or more and less than 50 mol%. "Vinyl content" refers to the total molar percentage of conjugated diene units bonded by 1,2-bonds or 3,4-bonds (conjugated diene units bonded by other than 1,4-bonds) in the total 100 mol% of conjugated diene units contained in the modified liquid diene polymer (B). The vinyl content can be expressed as 1 H-NMR and calculated based on the area ratio of the peak derived from the conjugated diene unit bonded by 1,2-bond or 3,4-bond to the peak derived from the conjugated diene unit bonded by 1,4-bond. The vinyl content of the modified conjugated diene polymer (B) can be set to a desired value by, for example, controlling the type of solvent used when producing the unmodified conjugated diene polymer (B'), the polar compound used as needed, the polymerization temperature, etc.
[0072] The glass transition temperature (Tg) of the modified conjugated diene polymer (B) is preferably -150 to 50° C., more preferably -130 to 50° C., and even more preferably -130 to 30° C. When Tg is within the above range, the stretching processability of the PVA film, the formability of the stretched film, and the like are further improved.
[0073] The modified conjugated diene polymer (B) may be used alone or in combination of two or more.
[0074] The lower limit of the content of the modified conjugated diene polymer (B) in the PVA film can be, for example, 5 parts by mass, preferably 10 parts by mass, more preferably 15 parts by mass, and further preferably 20 parts by mass, 25 parts by mass, 30 parts by mass or 35 parts by mass relative to 100 parts by mass of PVA (A). By making the content of the modified conjugated diene polymer (B) above the lower limit, the stretching processability of the PVA film and the formability of the stretched film and the polarizing film are further improved.
[0075] The upper limit of the content of the modified conjugated diene polymer (B) in the PVA film is relative to PVA100 mass parts, for example, can be 100 mass parts, is preferably 80 mass parts sometimes, is more preferably 60 mass parts, is further preferably 40 mass parts, 30 mass parts or 20 mass parts.By making the content of modified conjugated diene polymer (B) be below the above-mentioned upper limit, thus the stretching processability of the PVA film etc. is more suitable for.In addition, by making the content of modified conjugated diene polymer (B) be below the above-mentioned upper limit, thus transparency, other optical properties, surface properties etc. can be improved.
[0076] (Method for synthesizing modified conjugated diene polymer (B))
[0077] The synthesis method of the modified conjugated diene polymer (B) is not particularly limited, and the modified conjugated diene polymer (B) can be obtained, for example, by acid-modifying an unmodified conjugated diene polymer (B') and, if necessary, grafting the modified conjugated diene polymer (B) with a compound (X) described below.
[0078] In the unmodified conjugated diene polymer (B') used as the raw material, 50% or more of the total monomer units constituting the polymer are monomer units of butadiene and / or isoprene, which is a preferred embodiment. The total content of butadiene units and isoprene units is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, relative to the total monomer units of the unmodified conjugated diene polymer (B').
[0079] Examples of other monomer units other than the butadiene unit and the isoprene unit that may be contained in the unmodified conjugated diene polymer (B′) include conjugated diene units other than the above-mentioned butadiene and isoprene, and aromatic vinyl compound units.
[0080] Examples of the aromatic vinyl compound providing the aromatic vinyl compound unit include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-tert-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 2,4,6-trimethylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, vinylanthracene, N,N-diethyl-4-aminoethylstyrene, vinylpyridine, 4-methoxystyrene, monochlorostyrene, dichlorostyrene, and divinylbenzene. Among these, styrene, α-methylstyrene, and 4-methylstyrene are preferred.
[0081] The content of other monomer units except butadiene units and isoprene units in the unmodified conjugated diene polymer (B') is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. For example, if the vinyl aromatic compound unit is below the above range, there is a tendency to improve the stretching processability of the PVA film and the formability of the stretched film and the polarizing film.
[0082] The unmodified conjugated diene polymer (B′) is preferably a polymer obtained by polymerizing a conjugated diene and, if necessary, other monomers other than the conjugated diene by, for example, emulsion polymerization or solution polymerization.
[0083] As the emulsion polymerization method, a known method or a method based on a known method can be applied. For example, a predetermined amount of monomers containing a conjugated diene is emulsified and dispersed in the presence of an emulsifier, and emulsion polymerization is carried out using a radical polymerization initiator.
[0084] Examples of the emulsifier include long-chain fatty acid salts and rosin acid salts having at least 10 carbon atoms. Examples of the long-chain fatty acid salts include potassium or sodium salts of fatty acids such as capric acid, lauric acid, myristic acid, palmitic acid, oleic acid, and stearic acid.
[0085] As the dispersion medium, water is usually used, and a water-soluble organic solvent such as methanol or ethanol may be contained within a range that does not impair the stability during polymerization.
[0086] Examples of the radical polymerization initiator include persulfates such as ammonium persulfate and potassium persulfate; organic peroxides; and hydrogen peroxide.
[0087] In order to adjust the molecular weight of the obtained unmodified conjugated diene polymer (B'), a chain transfer agent may be used. Examples of the chain transfer agent include mercaptans such as tert-dodecyl mercaptan and n-dodecyl mercaptan; carbon tetrachloride, thioglycolic acid, diterpene, terpinolene, γ-terpinene, α-methylstyrene dimer, and the like.
[0088] The temperature of the emulsion polymerization can be appropriately set depending on the type of radical polymerization initiator used, and is usually in the range of 0 to 100° C., preferably in the range of 0 to 60° C. The polymerization method may be either continuous polymerization or batch polymerization.
[0089] The polymerization reaction can be stopped by adding a polymerization inhibitor. Examples of the polymerization inhibitor include amine compounds such as isopropylhydroxylamine, diethylhydroxylamine, and hydroxylamine; quinone compounds such as hydroquinone and benzoquinone; and sodium nitrite.
[0090] After stopping the polymerization reaction, an antioxidant can be added as needed. After stopping the polymerization reaction, unreacted monomers are removed from the obtained latex as needed. Then, using salts such as sodium chloride, calcium chloride, potassium chloride as coagulants, acids such as nitric acid and sulfuric acid are added as needed to adjust the pH of the coagulation system to a specified value, and the unmodified conjugated diene polymer (B') is coagulated. Thereafter, the polymer is recovered by separating the dispersion medium. Then, after washing and dehydration, the unmodified conjugated diene polymer (B') is obtained by drying. It should be noted that during coagulation, the latex can be mixed with a stretching oil made into an emulsified dispersion liquid in advance as needed, and recovered in the form of an unmodified conjugated diene polymer (B') extended by oil.
[0091] As the solution polymerization method, a known method or a method based on a known method can be applied. For example, a monomer containing a conjugated diene is polymerized in a solvent using a Ziegler catalyst, a metallocene catalyst, an anion polymerizable active metal or an active metal compound, if necessary, in the presence of a polar compound.
[0092] Examples of the solvent include aliphatic hydrocarbons such as n-butane, n-pentane, isopentane, n-hexane, n-heptane, and isooctane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.
[0093] Examples of anionically polymerizable active metals include alkali metals such as lithium, sodium, and potassium; alkaline earth metals such as beryllium, magnesium, calcium, strontium, and barium; and lanthanide rare earth metals such as lanthanum and neodymium. Among anionically polymerizable active metals, alkali metals and alkaline earth metals are preferred, and alkali metals are more preferred.
[0094] As the active metal compound capable of anionic polymerization, an organic alkali metal compound is preferred. Examples of the organic alkali metal compound include organic monolithium compounds such as methyl lithium, ethyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexyl lithium, phenyl lithium, stilbene lithium, etc.; polyfunctional organic lithium compounds such as dilithium methane, dilithium naphthalene, 1,4-dilithium butane, 1,4-dilithium-2-ethylcyclohexane, 1,3,5-trilithium benzene; sodium naphthalene, potassium naphthalene, etc. Among the organic alkali metal compounds, organic lithium compounds are preferred, and organic monolithium compounds are more preferred.
[0095] The amount of the organic alkali metal compound used can be appropriately set depending on the melt viscosity, molecular weight, etc. of the target unmodified conjugated diene polymer (B') and modified conjugated diene polymer (B), and is usually used in an amount of 0.01 to 3 parts by mass based on 100 parts by mass of all monomers including conjugated dienes.
[0096] The organic alkali metal compound can also be used in the form of an organic alkali metal amide by reacting with a secondary amine such as dibutylamine, dihexylamine, or dibenzylamine.
[0097] Polar compounds generally do not deactivate the reaction in anionic polymerization and are used to adjust the microstructure of the conjugated diene site. Examples of polar compounds include ether compounds such as dibutyl ether, tetrahydrofuran, and ethylene glycol diethyl ether; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, phosphine compounds, and the like. Polar compounds are generally used in an amount of 0.01 to 1000 moles relative to the organic alkali metal compound.
[0098] The temperature of solution polymerization is usually in the range of -80 to 150° C., preferably in the range of 0 to 100° C., and more preferably in the range of 10 to 90° C. The polymerization method may be either a batch method or a continuous method.
[0099] The polymerization reaction can be stopped by adding a polymerization inhibitor. Examples of the polymerization inhibitor include alcohols such as methanol and isopropanol. The unmodified conjugated diene polymer (B') can be separated by injecting the obtained polymerization reaction solution into a poor solvent such as methanol, or by washing the polymerization reaction solution with water, separating it, and then drying it.
[0100] As a method for producing the unmodified conjugated diene polymer (B'), among the above methods, a solution polymerization method is preferred.
[0101] The acid modification of the unmodified conjugated diene polymer (B') can be carried out by a conventionally known method, and preferably a method of adding an unsaturated carboxylic acid or an unsaturated carboxylic acid derivative to the unmodified conjugated diene polymer (B').
[0102] Examples of the unsaturated carboxylic acid include maleic acid, fumaric acid, itaconic acid, (meth)acrylic acid, etc. Examples of the unsaturated carboxylic acid derivative include anhydrides, esters, amides, imides, etc. of the unsaturated carboxylic acid.
[0103] Among the unsaturated carboxylic acids and unsaturated carboxylic acid derivatives, maleic acid and its derivatives are preferred, and maleic anhydride is more preferred. That is, as the acid-modified conjugated diene polymer, maleic anhydride-modified conjugated diene polymer is preferred. It should be noted that the acid-modified conjugated diene polymer itself is also a modified conjugated diene polymer (B) having hydrophilic groups such as carboxyl groups and acid anhydride groups.
[0104] The method of adding unsaturated carboxylic acid or unsaturated carboxylic acid derivative to the unmodified conjugated diene polymer (B') is not particularly limited, and can be, for example, a method of adding unsaturated carboxylic acid or unsaturated carboxylic acid derivative and a free radical catalyst as required to the unmodified conjugated diene polymer (B'), and heating in the presence or absence of an organic solvent. It should be noted that the acid-modified conjugated diene polymer can be directly modified using the compound (X) described later, or can be modified after hydrogenation.
[0105] As the compound (X) reacting with the acid-modified conjugated diene polymer, a compound (alcohol or amine) having at least one hydroxyl or amino group can be cited. By reacting the acid-modified conjugated diene polymer with this compound (X), an ester group or an amide group as a hydrophilic group is formed in the conjugated diene polymer. As compound (X), it is preferably a compound having a hydrophilic group on the basis of having one hydroxyl or amino group. Such suitable compounds also include compounds having more than two hydroxyls or amino groups. By reacting the acid-modified conjugated diene polymer with this compound (X), on the basis of forming an ester group or an amide group as a hydrophilic group in the conjugated diene polymer, a hydrophilic group further possessed by compound (X) is also introduced into the conjugated diene polymer.
[0106] As compound (X), a compound having at least one hydroxyl group or amino group and having a repeating structure containing a nonionic polar group is more preferred. As a more suitable compound (X), a compound represented by the following formula (1) can be cited. By using a compound represented by the following formula (1), a graft chain having a repeating structure containing a nonionic polar group as a hydrophilic group, i.e., a graft chain having a polyalkylene glycol structure, can be introduced into the conjugated diene polymer.
[0107] [Chemistry 1]
[0108]
[0109] In formula (1), R 1 R is hydroxyl or amino. 2 , R 3 , R 4 and R 5 Each independently represents hydrogen or a hydrocarbon group having 1 to 6 carbon atoms. 6 is a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or an acyl group having 1 to 6 carbon atoms. n is an integer of 3 to 600.
[0110] As R 1 , preferably hydroxyl. 2 ~R 6 The suitable form of n can be the same as R in the above formula (A) 2 ~R 6 Same as the appropriate form of n.
[0111] Examples of the compound represented by formula (1) include triethylene glycol, triethylene glycol monomethyl ether, polyethylene glycol, polyethylene glycol monoalkyl ether, polyethylene glycol monoalkylene alkyl ether, polyethylene glycol monoalkylene alkenyl ether, polyethylene glycol monoalkyl ester, propylene glycol, propylene glycol monoalkyl ether, polypropylene glycol, polypropylene glycol monoalkyl ether, methoxypolyethylene glycol amine, and monoalkyl ethers of copolymers of propylene oxide and ethylene oxide.
[0112] The lower limit of the weight average molecular weight of the compound represented by formula (1) is, for example, 100, preferably 200, and more preferably 300. On the other hand, the upper limit of the weight average molecular weight is, for example, 10,000, and more preferably 8,000, 6,000, 4,000, 2,000, or 1,000. The compound represented by formula (1) may be used alone or in combination of two or more.
[0113] The method for adding the compound (X) to the acid-modified conjugated diene polymer is not particularly limited. The following method can be adopted: adding the compound (X) to the acid-modified conjugated diene polymer, further adding an amine catalyst as required, and heating in the presence or absence of an organic solvent.
[0114] Examples of the amine catalyst include tertiary amines such as tetramethylethylenediamine, trimethylamine, and dimethylbenzylamine.
[0115] Examples of the organic solvent used in the above method generally include hydrocarbon solvents, halogenated hydrocarbon solvents, etc. Among these organic solvents, hydrocarbon solvents such as n-butane, n-hexane, n-heptane, cyclohexane, benzene, toluene, and xylene are preferred.
[0116] When the addition compound (X) is reacted by the above method, an antioxidant may be added from the viewpoint of suppressing side reactions.
[0117] Examples of antioxidants include 2,6-di-tert-butyl-4-methylphenol (BHT), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol) (AO-40), 3,9-bis[1,1-dimethyl-2-[3-(3-tert-butyl-4-hydroxy-5-methylphenol)] [(1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl]-1,4-bis[(octylthio)methyl]-6-methylphenol (Irganox1520L), 2,4-bis[(dodecylthio)methyl]-6-methylphenol (Irganox1726), 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl]-1,4-bis[(octylthio)methyl]-6-methylphenol (Irganox1726), phenyl acrylate (Sumilizer GS), 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate (Sumilizer GM), 6-tert-butyl-4-[3-(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphinane-6-yloxy)propyl]-2-methylphenol (Sumilizer GP), tris(2,4-di-tert-butylphenyl)phosphite (Irgafos168), 3,3'-dioctadecyl dithiodipropionate, hydroquinone, p-methoxyphenol, N-phenyl-N'-(1,3-dimethylbutyl) p-phenylenediamine (Nokluck 6C), bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (LA-77Y), N,N-dioctadecylhydroxylamine (Irgastab FS042), bis(4-tert-octylphenyl)amine (Irganox5057), etc. The antioxidant may be used alone or in combination of two or more.
[0118] The amount of the antioxidant added is preferably 0 to 10 parts by mass, more preferably 0 to 5 parts by mass, based on 100 parts by mass of the unmodified conjugated diene polymer (B').
[0119] The reaction conditions of the acid-modified conjugated diene polymer and the compound (X) are not particularly limited, but the reaction temperature is preferably 10 to 200° C., more preferably 30 to 180° C. The reaction time is preferably 1 to 200 hours, more preferably 1 to 100 hours, and even more preferably 1 to 50 hours.
[0120] The total amount of the unsaturated carboxylic acid, the unsaturated carboxylic acid derivative and the compound (X) added to the modified conjugated diene polymer (B) is preferably 1 to 400 parts by mass, more preferably 20 to 300 parts by mass, and even more preferably 50 to 250 parts by mass, relative to 100 parts by mass of the unmodified conjugated diene polymer (B'). It should be noted that the amount of addition can be determined using various analytical equipment such as nuclear magnetic resonance spectroscopy.
[0121] The modified conjugated diene polymer (B) can be synthesized according to the method described in, for example, International Publication No. 2010 / 038835, Japanese Patent Application Laid-Open No. 2015-086283, or the like, in addition to the above-mentioned synthesis method.
[0122] [Plasticizer]
[0123] The PVA film may further contain a plasticizer. By making the PVA film contain a plasticizer, it is possible to achieve improvements in stretching processability, handling properties, roll quality, etc. As preferred plasticizers, polyols can be listed, and as specific examples, ethylene glycol, glycerol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol, trimethylolpropane, etc. can be listed. These plasticizers can be used in one or more than two kinds. Among these, glycerol is preferably used from the viewpoint of improving the effect of stretching processability and roll quality.
[0124] As the lower limit of the content of the plasticizer in the PVA film, relative to 100 parts by mass of PVA (A), preferably 1 part by mass, more preferably 5 parts by mass. By making the content of the plasticizer above the lower limit, the processing stretchability and the like are further improved. On the other hand, as the upper limit of the content, preferably 20 parts by mass, more preferably 15 parts by mass. By making the content of the plasticizer below the upper limit, it is possible to suppress the PVA film from being too soft or the plasticizer from seeping out to the surface and causing the reduction in handling properties.
[0125] [Other additives, etc.]
[0126] If necessary, the PVA film may further contain appropriate fillers, processing stabilizers such as copper compounds, weathering stabilizers, colorants, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, flame retardants, other thermoplastic resins, lubricants, fragrances, defoamers, deodorants, extenders, peeling agents, mold release agents, reinforcing agents, crosslinking agents, mildewproof agents, preservatives, crystallization rate retarders, surfactants and other additives.
[0127] Among other additives, it is preferred to include a surfactant from the viewpoint of film forming properties. By including a surfactant, uneven thickness of the PVA film can be suppressed, or the film can be easily peeled off from a substrate such as a metal roller or belt used for self-made film. The type of surfactant is not particularly limited, but from the viewpoint of peeling properties from a metal roller or belt, an anionic surfactant and a nonionic surfactant are preferred.
[0128] Preferred anionic surfactants include, for example, carboxylic acid type surfactants such as potassium laurate; sulfate ester type surfactants such as polyoxyethylene lauryl ether sulfate and octyl sulfate; and sulfonic acid type surfactants such as dodecylbenzenesulfonate.
[0129] As the nonionic surfactant, preferred are, for example, alkyl ether types such as polyoxyethylene oleyl ether; alkyl phenyl ether types such as polyoxyethylene octylphenyl ether; alkyl ester types such as polyoxyethylene laurate; alkyl amine types such as polyoxyethylene lauryl amino ether; alkyl amide types such as polyoxyethylene lauric acid amide; polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether; alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide; allyl phenyl ether types such as polyoxyalkylene allyl phenyl ether, etc.
[0130] These surfactants may be used alone or in combination of two or more.
[0131] When the PVA film includes a surfactant, the lower limit of its content is preferably 0.01 mass parts, more preferably 0.03 mass parts relative to 100 mass parts of PVA (A). By making the content of the surfactant more than the above lower limit, the peeling property, the film forming property, etc. are further improved. On the other hand, as the upper limit of the content, it is preferably 0.5 mass parts, more preferably 0.3 mass parts. By making the content of the surfactant below the above upper limit, the surfactant can be suppressed from oozing out of the surface of the PVA film, the films are closely attached to each other, and the handling property is reduced.
[0132] The upper limit of the content of other additives in the PVA film other than PVA (A), modified conjugated diene polymer (B), plasticizer and surfactant is preferably 10% by mass, more preferably 5% by mass, more preferably 1% by mass, and even more preferably 0.2% by mass. When the content of other additives exceeds the above upper limit, the processing stretchability of the PVA film, the formability and transparency of the obtained stretched film and polarizing film, etc. are sometimes affected.
[0133] [Shape, etc.]
[0134] The shape of the PVA film is not particularly limited, and from the perspective of being able to be continuously manufactured with good productivity, a long film is preferably used. The length of the long PVA film is not particularly limited, and can be appropriately set according to the purpose, etc. For example, the length can be set in the range of more than 5m and less than 20,000m. The width of the PVA film is not particularly limited, and for example, in the case of a water-soluble film, the lower limit can be set to 1cm. In addition, in various uses, since wide-width PVA films have been sought in recent years, the lower limit is preferably 1m, more preferably 2m, and further preferably 4m. The upper limit of the width of the PVA film is not particularly limited, and for example, it can be set to 7m. If the width is too wide, when the PVA film is manufactured using a practical device, there is a tendency to be difficult to produce uniformly.
[0135] The PVA film may be a single-layer film or a multi-layer film (laminate).
[0136] The upper limit of the thickness (average thickness) of the PVA film is not particularly limited, for example, 100 μm, preferably 60 μm, and more preferably 40 μm. On the other hand, as the lower limit of the thickness, it is preferably 1 μm, more preferably 5 μm, and further preferably 10 μm. By making the thickness of the PVA film within the above range, it is possible to improve handling properties, stretching properties, etc. It should be noted that the thickness (average thickness) is set to the average value of the measured values at any 5 locations.
[0137] [use]
[0138] The PVA film can be used for various purposes similar to the previous PVA film, such as packaging film, water-soluble film, agricultural film, release film, optical film, etc. In addition, the PVA film is suitable as a raw material film for stretch film and polarizing film. In particular, the PVA film has excellent stretching processability, and can obtain a stretch film and a polarizing film with excellent formability, so it is suitable as a raw material film for optical film material. That is, an optical film can be suitably obtained by stretching the PVA film. It should be noted that the PVA film described in one embodiment of the present invention can be a packaging film, a water-soluble film, an agricultural film, a release film, a stretch film, an optical film or a polarizing film.
[0139] An optical film refers to a film with light transmittance used in an optical device. As an optical device, a display device such as a liquid crystal display device and an organic EL display can be listed as a representative example. As an optical film, a polarizing film, a polarizer protective film, a color compensation film, a brightness enhancement film, a viewing angle expansion film, a phase difference film, etc. can be listed. In addition, the PVA film can also be used as a gas barrier film of an organic EL display, etc., by utilizing its good transparency and gas barrier properties, as another example of an optical film.
[0140] It should be noted that the PVA film can be suitably used as a raw material film for a stretched film and a polarizing film as described above, and can also be used for various purposes without stretching.
[0141] <Method for manufacturing PVA film>
[0142] The method for manufacturing the PVA film is not particularly limited, and a manufacturing method in which the thickness and width of the PVA film after film formation are more uniform can be preferably adopted. For example, it can be obtained by forming a film using a film-forming stock solution obtained by dissolving PVA (A) and a modified conjugated diene polymer (B) constituting the PVA film, and other components such as a plasticizer as required in a liquid medium. In addition, if necessary, a film-forming stock solution in which PVA (A) or the like is melted can also be used for manufacturing.
[0143] The method for manufacturing the PVA film according to one embodiment of the present invention includes a step of forming a film using a film-forming stock solution obtained by mixing a dispersion liquid of PVA (A) and a modified conjugated diene polymer (B) containing a hydrophilic group. According to this manufacturing method, a PVA film excellent in stretchability and productivity can be manufactured, and a stretched film and a polarizing film excellent in formability can be obtained from the PVA film.
[0144] The specific forms and suitable forms of PVA (A) and the modified conjugated diene polymer (B) used in this manufacturing method are the same as those of PVA (A) and the modified conjugated diene polymer (B) as the components of the PVA film according to one embodiment of the present invention described above.
[0145] The lower limit of the content of the modified conjugated diene polymer (B) in the film-forming stock solution is, for example, sometimes 5 parts by mass, preferably 10 parts by mass, more preferably 15 parts by mass, further preferably 20 parts by mass, 25 parts by mass, 30 parts by mass, or 35 parts by mass with respect to 100 parts by mass of PVA (A). On the other hand, the upper limit of this content is, for example, 100 parts by mass, sometimes preferably 80 parts by mass, more preferably 60 parts by mass, further preferably 40 parts by mass, 30 parts by mass, or 20 parts by mass.
[0146] In the film-forming stock solution, the modified conjugated diene polymer (B) is preferably uniformly mixed. It should be noted that by mixing the dispersion liquid of the modified conjugated diene polymer (B) with a liquid medium, PVA (A), and other additives, etc., a film-forming stock solution in which the modified conjugated diene polymer (B) is uniformly mixed can be effectively obtained. In addition, when the film-forming stock solution contains a plasticizer, other additives, etc., it is preferable that these components are uniformly mixed.
[0147] The method for producing the dispersion of the modified conjugated diene polymer (B) is not particularly limited, and the dispersion can be obtained, for example, by adding water after synthesizing the modified conjugated diene polymer (B) and stirring with an emulsifier or a stirrer, etc. In this case, the average particle size of the modified conjugated diene polymer (B) can be adjusted by adjusting the stirring intensity, stirring time, etc., adjusting the pH with an acid or a base, selecting an emulsifier, etc.
[0148] The acid or base used in the preparation of the dispersion of the modified conjugated diene polymer (B) is not particularly limited. Examples of the acid include hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, citric acid, carbonic acid, and acetic acid. Examples of the base include sodium hydroxide, potassium hydroxide, and ammonia.
[0149] When an emulsifier is used in the manufacture of the dispersion of the modified conjugated diene polymer (B), there is no particular limitation on the emulsifier, and common emulsifiers such as anionic, nonionic, and nonionic-anionic can be used. Specific examples of emulsifiers include sodium salts, potassium salts, or ammonium salts of aliphatic carboxylic acids such as laurate, myristate, palmitate, stearate, and alkenyl succinate as anionic emulsifiers; sodium salts, potassium salts, or ammonium salts of disproportionated or hydrogenated products of natural rosin; sodium salts, potassium salts, or ammonium salts of aliphatic sulfuric acid compounds such as lauryl sulfate, etc. In addition, as nonionic-anionic emulsifiers, polyoxyethylene octylphenyl ether sulfonates, polyoxyethylene octylphenyl ether sulfate ester salts, polyoxyethylene alkyl ether sulfates, etc. can be listed. As counter cations of these salts, sodium, potassium, or ammonium can be listed.
[0150] Examples of the liquid medium used in the membrane-forming stock solution include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, glycerol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, trimethylolpropane, ethylenediamine, and diethylenetriamine. One or more of these liquid media can be used. Among these, water is preferred from the viewpoint of small environmental burden and recyclability.
[0151] The volatility of the film-making stock solution (the proportion of volatile components such as liquid medium removed by volatilization and evaporation in the film-making stock solution) also varies depending on the film-making method, film-making conditions, etc., and generally speaking, as a lower limit, it is preferably 50% by mass, more preferably 55% by mass, and further preferably 60% by mass. By making the volatility of the film-making stock solution above the above lower limit, the viscosity of the film-making stock solution will not be too high, and the filtration and degassing during the preparation of the film-making stock solution can be smoothly carried out, and it is easy to manufacture foreign matter and PVA films with few shortcomings. On the other hand, as the upper limit of the volatility, it is preferably 95% by mass, more preferably 90% by mass. By making the volatility of the film-making stock solution below the above upper limit, the concentration of the film-making stock solution will not be too low, and it is easy to industrially manufacture PVA films.
[0152] As the film-making method when using film-making stock solution to manufacture PVA film, a previously known method can be used. As the film-making method, it can be a method of applying the film-making stock solution to the substrate of a metal drum etc. and manufacturing the PVA film on the substrate, or it can be a method of directly manufacturing a monolayer PVA film. As the film-making method, for example, a cast film-making method, an extrusion film-making method, a wet film-making method, a gel film-making method etc. can be listed, and these film-making methods can only adopt 1 kind, or two or more kinds can be combined. Among these film-making methods, from the aspect of being able to obtain a PVA film with uniform thickness and width and good physical properties, it is preferably a cast film-making method and an extrusion film-making method.
[0153] Here, according to the method for producing a PVA film described in one embodiment of the present invention, the modified conjugated diene polymer (B) added to the film-making stock solution has a hydrophilic group, so the modified conjugated diene polymer (B) is difficult to adhere to a substrate such as a metal drum. In addition, if it has already adhered, it can also be easily washed off with water or the like. Therefore, according to this production method, a PVA film with high productivity and excellent stretching processability can be produced.
[0154] The manufactured PVA film can be heat-treated as needed. The heat treatment temperature is not particularly limited, as long as it is appropriately adjusted. If the heat treatment temperature is too high, discoloration and degradation of the PVA film can be observed. Therefore, as the upper limit of the heat treatment temperature, it is preferably 210°C, more preferably 180°C, and further preferably 150°C. On the other hand, as the lower limit of the heat treatment temperature, for example, it is 60°C, preferably 90°C.
[0155] The heat treatment time is not particularly limited and can be appropriately adjusted. From the viewpoint of efficiently manufacturing the PVA film, the upper limit is preferably 30 minutes, more preferably 15 minutes. On the other hand, the lower limit is, for example, preferably 10 seconds, more preferably 1 minute.
[0156] <Stretch Film>
[0157] The stretched film described in one embodiment of the present invention is a stretched film obtained by stretching the PVA film described in one embodiment of the present invention. In the stretched film, the PVA is usually oriented along a specified direction (stretching direction). The stretched film can be uniaxially stretched or biaxially stretched, preferably uniaxially stretched. The uniaxially stretched stretched film can be suitably used as an optical film such as a polarizing film. The stretched film can be a monolayer film or a multilayer film, preferably a monolayer film. The stretched film is difficult to produce problems such as fragmentation caused by deformation by containing a modified conjugated diene polymer (B), and is therefore suitable for foldable displays, sunglasses with high design, etc.
[0158] The upper limit of the thickness (average thickness) of the stretched film is, for example, 30 μm, preferably 16 μm. By making the thickness of the stretched film below the upper limit, sufficient thinning can be achieved. On the other hand, as the lower limit of the thickness, it is preferably 5 μm, more preferably 8 μm. By making the thickness of the stretched film above the lower limit, it is difficult to break, and the handling properties can be improved.
[0159] The stretched film can be used as a packaging film, a water-soluble film, an agricultural film, a release film, an optical film, etc., and is preferably used as an optical film.
[0160] Examples of the optical film include a polarizing film, a polarizing plate protective film, a color compensation film, and a brightness enhancement film. Among these, a polarizing film is preferred.
[0161] <Method for producing stretched film>
[0162] The stretched film can be obtained by the manufacturing method having the step of stretching the PVA film. That is, the manufacturing process of the stretched film is arbitrary except for the stretching process, and can be manufactured by the same method as before except for using the above-mentioned PVA film. Therefore, the manufacturing process of the stretched film does not need to include the treatment (dyeing treatment, fixing treatment, etc.) other than the stretching treatment in the manufacturing process of the polarizing film described later. That is, according to this manufacturing method, the stretched film can be obtained relatively easily without going through special processes.
[0163] By dyeing the PVA film or the stretched film, etc., a polarizing film having excellent formability can be provided.
[0164] <Polarizing Film>
[0165] The polarizing film according to one embodiment of the present invention is obtained by dyeing the PVA film or the stretched film according to one embodiment of the present invention. In the polarizing film, a dichroic pigment and boric acid are adsorbed on the PVA film or the stretched film. The polarizing film contains the modified conjugated diene polymer (B) and is less likely to cause problems such as breakage due to deformation, and is therefore suitable for foldable displays, sunglasses with high design, and the like.
[0166] The polarizing film can also be laminated to both sides or one side thereof with an optically transparent protective film having mechanical strength to be used as a polarizing plate. As the protective film, a triacetyl cellulose (TAC) film, a cellulose acetate-butyrate (CAB) film, an acrylic film, a polyester film, etc. can be used. In addition, as the adhesive for lamination, PVA adhesives, ultraviolet curing adhesives, etc. can be listed, preferably PVA adhesives.
[0167] The polarizing plate obtained by the above operation may be further bonded with an optical film such as a phase difference film, a viewing angle enhancement film, and a brightness enhancement film. It should be noted that as the viewing angle enhancement film, etc., a stretched film described in one embodiment of the present invention may also be used. The polarizing plate may be bonded to a glass substrate after being coated with an adhesive such as an acrylic acid and used as a component of a liquid crystal display device.
[0168] <Method for Manufacturing Polarizing Film>
[0169] As a specific method for manufacturing the polarizing film, there can be cited a method of subjecting the PVA film to swelling treatment, dyeing treatment, uniaxial stretching treatment, and further subjecting the PVA film to crosslinking treatment, fixing treatment, washing treatment, drying treatment, heat treatment, etc. as required. In this case, the order of the swelling treatment, dyeing treatment, crosslinking treatment, uniaxial stretching treatment, fixing treatment, etc. is not particularly limited, and two or more treatments may be performed simultaneously. In addition, one or more of the treatments may be performed two or more times.
[0170] In addition, as other methods for manufacturing the polarizing film, there can be cited a method of subjecting the stretched film to various treatments other than the swelling treatment. That is, the stretched film can be subjected to dyeing treatment and uniaxial stretching treatment, and further subjected to crosslinking treatment, fixing treatment, cleaning treatment, drying treatment, heat treatment, etc. as required, thereby obtaining the polarizing film. In this case, the order of the dyeing treatment, crosslinking treatment, uniaxial stretching treatment, fixing treatment, etc. is not particularly limited, and two or more treatments may be performed simultaneously. In addition, one or more of the treatments may be performed two or more times.
[0171] Among these methods for manufacturing the polarizing film, a method having the following steps is particularly preferred: subjecting the PVA film to swelling treatment, dyeing treatment, and uniaxial stretching treatment, and further subjecting the PVA film to cross-linking treatment, fixing treatment, cleaning treatment, drying treatment, heat treatment, etc. as needed, and then subjecting the film to uniaxial stretching using a dry stretching method.
[0172] Hereinafter, a case where the polarizing film is produced using the PVA film will be described in detail, but the conditions of each treatment such as dyeing treatment described later are the same also when the polarizing film is produced using the stretched film.
[0173] The swelling treatment can be carried out by immersing the PVA film in water. As the lower limit of the water temperature when immersed in water, it is preferably 20°C, more preferably 22°C, and further preferably 25°C. On the other hand, as the upper limit of the temperature, it is preferably 55°C, more preferably 40°C, and further preferably 35°C. In addition, as the lower limit of the time of immersion in water, it is preferably 0.1 minute, and more preferably 0.5 minute. On the other hand, as the upper limit of the time, it is preferably 5 minutes, and more preferably 3 minutes. It should be noted that the water when immersed in water is not limited to pure water, and can be an aqueous solution in which various components are dissolved, or a mixture of water and an aqueous medium.
[0174] The dyeing treatment can be performed by bringing a dichroic dye into contact with the PVA film. As the dichroic dye, an iodine-based dye or a dichroic dye is generally used.
[0175] In the case of iodine-based pigments, as the period of dyeing treatment, it can be any stage before uniaxial stretching treatment, during uniaxial stretching treatment and after uniaxial stretching treatment. The dyeing treatment is generally carried out by immersing the PVA film in a solution (especially an aqueous solution) containing iodine-potassium iodide as a dyeing bath. The iodine concentration in the dyeing bath is preferably 0.01 mass % or more and 0.5 mass % or less, and the concentration of potassium iodide is preferably 0.01 mass % or more and 10 mass % or less. In addition, the lower limit of the temperature of the dyeing bath is preferably 20 ° C, more preferably 25 ° C. On the other hand, the upper limit of the temperature is preferably 50 ° C, more preferably 40 ° C.
[0176] In the case of a dichroic dye, the dyeing treatment may be performed at any stage of the preparation of the PVA film, before the uniaxial stretching treatment, during the uniaxial stretching treatment, or after the uniaxial stretching treatment. In the dyeing treatment, a dichroic dye, such as an azo compound, is adsorbed and impregnated into the product obtained by subjecting the PVA film to a swelling treatment. When the swelling treatment is omitted, the swelling treatment may be performed simultaneously with the dyeing treatment.
[0177] The azo compound may be used in the form of a free acid or a salt thereof, such as an alkali metal salt such as a lithium salt, a sodium salt or a potassium salt, or an organic salt such as an ammonium salt or an alkylamine salt, preferably a sodium salt.
[0178] The dyeing treatment is generally performed by immersing the PVA film in a solution (especially an aqueous solution) containing an azo compound as a dyeing bath. The concentration of each azo compound in the dyeing bath is preferably 0.00001% by mass or more and 10% by mass or less. In addition, the temperature of the dyeing bath is preferably 5 to 60°C, more preferably 20 to 50°C, and particularly preferably 35 to 50°C. The time of immersion in the solution can be appropriately adjusted, preferably adjusted to 30 seconds to 20 minutes, more preferably 1 to 10 minutes.
[0179] As the dyeing solution, it is possible to further contain a dyeing auxiliary as required on the basis of containing an azo compound. As dyeing auxiliary, sodium carbonate, sodium bicarbonate, sodium chloride, sodium sulfate, anhydrous sodium sulfate and sodium tripolyphosphate etc. can be listed. The content of the dyeing auxiliary can be adjusted with any concentration according to the time and temperature based on the dyeing property of the dye, and as each content, it is preferably 0.01 to 5% by mass in the dyeing solution, and more preferably 0.1 to 2% by mass.
[0180] By cross-linking the PVA film, it is possible to effectively prevent PVA from dissolving into water during wet stretching at high temperature. From this point of view, it is preferred to perform cross-linking before uniaxial stretching. The cross-linking treatment can be performed by immersing the PVA film in an aqueous solution containing a cross-linking agent. As the cross-linking agent, one or more of boron inorganic compounds such as borate such as boric acid and borax can be used. The lower limit of the concentration of the cross-linking agent in the aqueous solution containing the cross-linking agent is preferably 1% by mass, more preferably 2% by mass, and further preferably 3% by mass. On the other hand, the upper limit of the concentration is preferably 15% by mass, more preferably 7% by mass, and further preferably 6% by mass. By making the concentration of the cross-linking agent within the above range, sufficient stretchability can be maintained. When using iodine-based pigments, the aqueous solution containing the cross-linking agent may contain auxiliary agents such as potassium iodide. The lower limit of the temperature of the aqueous solution containing the cross-linking agent is preferably 20°C, more preferably 25°C. On the other hand, the upper limit of the temperature is preferably 50°C, more preferably 40°C. By setting the temperature within the above range, cross-linking can be performed efficiently.
[0181] The uniaxial stretching process can be carried out using any one of the wet stretching method and the dry stretching method. In the case of the wet stretching method, it can be carried out in a boric acid aqueous solution, or in the above-mentioned dyeing bath or in the fixing treatment bath described later. In addition, in the case of the dry stretching method, the uniaxial stretching process can be directly carried out at room temperature, or the uniaxial stretching process can be carried out while heating, or the PVA film after absorbing water can be used and uniaxially stretched in the air. Among these, the wet stretching method is preferably used, and the uniaxial stretching process is more preferably carried out in a boric acid aqueous solution. The lower limit of the boric acid concentration of the boric acid aqueous solution is preferably 0.5 mass %, more preferably 1.0 mass %, and further preferably 1.5 mass %. On the other hand, the upper limit of the boric acid concentration is preferably 6 mass %, and more preferably 5 mass %. In addition, when the boric acid aqueous solution is an iodine-based pigment, potassium iodide can be contained, and its concentration is preferably set to more than 0.01 mass % and less than 10 mass %.
[0182] From the viewpoint of polarization performance of the obtained polarizing film, the lower limit of the stretch ratio in the uniaxial stretching treatment is preferably 3 times, and more preferably 5 times. The upper limit of the stretch ratio is not particularly limited, and for example, it may be preferably 10 times, and more preferably 8 times.
[0183] When manufacturing a polarizing film, in order to make the dichroic pigment (iodine-based pigment, etc.) firmly adsorbed on the PVA film, it is preferably fixed after the uniaxial stretching treatment. As a fixed treatment bath used in the fixed treatment, an aqueous solution containing one or more boron inorganic compounds such as boric acid and borax can be used. In addition, iodine compounds and metal compounds can be added to the fixed treatment bath as needed. The lower limit of the concentration of the boron inorganic compound in the fixed treatment bath is preferably 0.5% by mass, more preferably 1% by mass. On the other hand, the upper limit of the concentration is preferably 15% by mass, more preferably 10% by mass. By making the concentration within the above range, the dichroic pigment can be more firmly adsorbed. The lower limit of the temperature of the fixed treatment bath is preferably 15°C. On the other hand, the upper limit of the temperature is preferably 60°C, more preferably 40°C.
[0184] The cleaning process is generally carried out by immersing the PVA film in water or the like. In the case of iodine-based pigments, from the viewpoint of improving polarization performance, the water or the like used in the cleaning process preferably contains an auxiliary agent such as potassium iodide. At this time, the concentration of iodides such as potassium iodide is preferably set to be greater than 0.5% by mass and less than 10% by mass. In addition, the lower limit of the temperature of the water or the like used in the cleaning process is generally 5°C, preferably 10°C, and more preferably 15°C. On the other hand, the upper limit of the temperature is generally 50°C, preferably 45°C, and more preferably 40°C. From an economic point of view, it is not preferred that the temperature of the water or the like is too low. On the other hand, if the temperature of the water or the like is too high, the polarization performance is sometimes reduced.
[0185] The drying conditions are not particularly limited, but the lower limit of the drying temperature is preferably 30° C., more preferably 50° C. On the other hand, the upper limit of the drying temperature is preferably 150° C., more preferably 130° C. By drying at a temperature within the above range, a polarizing film having excellent dimensional stability can be easily obtained.
[0186] By performing a heat treatment after a drying treatment, a polarizing film having excellent dimensional stability can be obtained. Here, the heat treatment refers to a treatment in which the polarizing film having a moisture content of 5% or less after the drying treatment is further heated to improve the dimensional stability of the polarizing film. The heat treatment conditions are not particularly limited, and the heat treatment is preferably performed in the range of 60°C to 150°C. By performing a heat treatment at a temperature above 60°C, the dimensional stabilization effect based on the heat treatment can be improved. On the other hand, by performing a heat treatment at a temperature below 150°C, yellowing of the polarizing film can be suppressed.
[0187] The polarizing film is not limited to a two-dimensional shape (planar), but also includes a polarizing film processed into a three-dimensional shape. That is, the polarizing film can be formed by stretching after dyeing. As a method for stretching the dyed film, there are various methods such as wet stretching, vacuum forming, and thermoforming, but it is not limited to this. As a stretching ratio, from the viewpoint of maintaining performance, it is preferably 1.2 to 2 times stretching, and more preferably 1.3 to 1.5 times. As a stretching speed, from the viewpoint of productivity, it is preferably 100 to 10000% / minute, and more preferably 500 to 5000% / minute. As a stretching temperature, it is preferably below 100°C when using iodine-based dyes, and it is preferably below 160°C when using dichroic dyes. In the case of iodine-based dyes, by forming below 100°C, it is possible to suppress decolorization and breakage during stretching. Example
[0188] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples at all. It should be noted that the evaluation methods used in the following examples and comparative examples are as follows.
[0189] [Method for measuring weight average molecular weight of modified conjugated diene polymer]
[0190] The weight average molecular weight of the modified conjugated diene polymer is determined by GPC (gel permeation chromatography) using a molecular weight converted to standard polystyrene.
[0191] The measurement apparatus and conditions are as follows.
[0192] Equipment: GPC equipment "GPC8020" manufactured by Tosoh Corporation
[0193] Separation column: "TSKgelG4000HXL" manufactured by Tosoh Corporation
[0194] Detector: "RI-8020" manufactured by Tosoh Corporation
[0195] Eluent: Tetrahydrofuran
[0196] Eluent flow rate: 1.0ml / min
[0197] Sample concentration: 5mg / 10ml
[0198] Column temperature: 40°C.
[0199] [Stretching processability of PVA film (tensile stress)]
[0200] The PVA film was humidified at 23°C and 50% RH for 24 hours, and a film sheet with a length of 30 mm and a width of 10 mm was cut from the PVA film. Afterwards, the PVA film sheet was installed in a tensile test device ("single-column table-type tester: 5952") manufactured by Instron Corporation with an initial clamp interval of 10 mm, and a tensile test was performed at a speed of 100 [mm / min]. The test force [N] when the clamp interval at this time reaches 30 mm was divided by the cross-sectional area [mm 2 ] and the value obtained is taken as the tensile stress [N / mm 2 ]. At this time, the same measurement is repeated 10 times for one sample, and the average value is used as the data. Tensile stress is less than 50N / mm 2 It is judged that it is easy to stretch and has good stretching processability.
[0201] [Washability (Productivity) of Conjugated Diene Polymer Adhering to Metal Drum during Production of PVA Film]
[0202] When the PVA film is produced, the conjugated diene polymer present on the surface of the PVA film will adhere to the metal drum, so this cleaning test is performed. Specifically, after the PVA film is produced, the metal drum is wiped with a cotton cloth soaked in water. Thereafter, it is visually confirmed whether the conjugated diene polymer remains on the surface of the metal drum. If it remains, it is recorded as B, and if it does not remain, it is recorded as A.
[0203] [Formability of polarizing film (TD breaking deformation)]
[0204] The polarizing film was humidified at 23°C and 50% RH for more than 24 hours, and a film piece with a length direction (MD) of 10 mm and a width direction (TD) of 30 mm was cut out from the polarizing film. Afterwards, the polarizing film piece was installed in a tensile test device ("AGS-H") manufactured by Shimadzu Corporation in such a way that the initial clamp spacing was 10 mm and the stretching direction was consistent with the TD of the polarizing film, and a tensile test was carried out at a speed of 100 [mm / min] (1000% / minute) in a heating environment of 140°C. At this time, the same measurement was repeated 10 times for one sample, and the value with the largest TD fracture deformation was used as the data. When the TD fracture deformation is 40% or more, it is judged to be easy to form and has good formability. Here, the TD fracture deformation refers to the value of (X / 10)×100(%) when the polarizing film is stretched Xmm from the initial distance between the clamps (10 mm) and breaks in the above-mentioned tensile test.
[0205] [Production Example 1]
[0206] (1) Synthesis of conjugated diene polymer (B'-1)
[0207] The fully dried 5L autoclave was purged with nitrogen, and 1200 g of hexane and 112 g of sec-butyl lithium (10.5% by mass hexane solution) were added, and the temperature was raised to 50°C. Thereafter, under stirring conditions, 1200 g of isoprene was gradually added while controlling the polymerization temperature to 50°C, and the polymerization was carried out for 1 hour. Thereafter, methanol was added to stop the polymerization reaction to obtain a polymer solution. Water was added to the obtained polymer solution, stirred, and the polymer solution was washed with water. After the stirring was terminated and the water was discharged after confirming that the polymer solution phase and the aqueous phase had been separated. The conjugated diene polymer (B'-1) was obtained by vacuum drying the polymer solution after the washing at 70°C for 24 hours.
[0208] (2) Synthesis of Aqueous Dispersion of Conjugated Diene Polymer (B'-1)
[0209] 15 g of an emulsifier ("Fusion Fluor RS-710" manufactured by Toho Chemical Industry Co., Ltd.) was added to 250 g of the conjugated diene polymer (B'-1) and stirred for 20 minutes. Then, 177 g of water was added little by little while stirring. After adding a predetermined amount of water, the mixture was stirred for 20 minutes to obtain an aqueous dispersion of the conjugated diene polymer (B'-1).
[0210] [Production Example 2]
[0211] (1) Synthesis of modified conjugated diene polymer (B-1) having a hydrophilic group
[0212] 200 g of the conjugated diene polymer (B'-1) obtained in Preparation Example 1 and 40 g of maleic anhydride were added to a reaction container and reacted at 170°C for 24 hours. Furthermore, 408 g of polyethylene glycol monomethyl ether (polyethylene glycol monomethyl ether 1000 manufactured by Tokyo Chemical Industry Co., Ltd., average molecular weight: 1,000, average number of polyoxyethylene units: 22) and 0.7 g of N,N-dimethylbenzylamine were added and reacted for 6 hours to obtain a modified conjugated diene polymer (B-1) having a hydrophilic group. The weight average molecular weight of the obtained modified conjugated diene polymer (B-1) was 27,000.
[0213] (2) Synthesis of aqueous dispersion of modified conjugated diene polymer (B-1)
[0214] 13 g of an aqueous sodium hydroxide solution (sodium hydroxide concentration: 50% by mass) was added to 250 g of the modified conjugated diene polymer (B-1), and the mixture was stirred at 50° C. for 60 minutes. Subsequently, 451 g of water was added little by little while stirring to obtain an aqueous dispersion of the modified conjugated diene polymer (B-1).
[0215] [Production Example 3]
[0216] (1) Synthesis of modified conjugated diene polymer (B-2) having a hydrophilic group
[0217] 250 g of the conjugated diene polymer (B'-1) obtained in Preparation Example 1 and 50 g of maleic anhydride were added to a reaction container and reacted at 170°C for 24 hours. Furthermore, 204 g of polyethylene glycol monomethyl ether (polyethylene glycol monomethyl ether 400 manufactured by Tokyo Chemical Industry Co., Ltd., average molecular weight: 400, average number of polyoxyethylene units: 8) and 0.9 g of N,N-dimethylbenzylamine were added and reacted for 6 hours to obtain a modified liquid diene polymer (B-2) having a hydrophilic group. The weight average molecular weight of the obtained modified conjugated diene polymer (B-2) was 18,000.
[0218] (2) Preparation of aqueous dispersion of modified conjugated diene polymer (B-2)
[0219] To 250 g of the modified conjugated diene polymer (B-2) was added 20 g of an aqueous sodium hydroxide solution (sodium hydroxide concentration: 50% by mass), and the mixture was stirred at 50° C. for 60 minutes. Subsequently, 443 g of water was added little by little while stirring to obtain an aqueous dispersion of the modified conjugated diene polymer (B-2).
[0220] [Example 1]
[0221] (Production of PVA film)
[0222] 100 parts by mass of PVA (saponified product of homopolymer of vinyl acetate, degree of polymerization of 2,400, degree of saponification of 99.5 mol%), 15 parts by mass of modified conjugated diene polymer (B-1), 10 parts by mass of glycerol as a plasticizer, 0.1 parts by mass of sodium polyoxyethylene lauryl ether sulfate as a surfactant and water are mixed to prepare a film-making stock solution having a volatility of 85% by mass. Here, the modified conjugated diene polymer (B-1) is obtained by mixing the substance in the state of aqueous dispersion obtained in the above-mentioned Production Example 2 with other components. The above-mentioned film-making stock solution is cast onto a metal drum with a surface temperature of 80°C and dried until the volatility (water content) reaches 5% by mass to obtain a long PVA film (PVA film before heat treatment) having a thickness of 30 μm, a length of 1.5 m and a width of 30 cm. The PVA film is heat-treated at a temperature of 110°C for 10 minutes to obtain the PVA film of Example 1.
[0223] (Production of polarizing film)
[0224] A sample of 5 cm in width and 10 cm in length was cut from the central part of the width direction of the obtained PVA film in such a way that a uniaxial stretching of 5 cm in width and 5 cm in length could be performed. The sample was immersed in pure water at 40°C for 120 seconds, and uniaxially stretched to 1.3 times in the length direction to perform swelling treatment (uniaxial stretching in the first stage). Next, it was immersed in a dyeing treatment bath (temperature 48°C) containing an aqueous solution of 0.00002% by mass of Direct blue 15 dye, 0.1% by mass of sodium tripolyphosphate and 0.1% by mass of sodium sulfate for 300 seconds, and uniaxially stretched to 2.4 times in the length direction as a whole to adsorb the dye (uniaxial stretching in the second stage). Furthermore, it was immersed in a cross-linking treatment bath (temperature 40°C) containing an aqueous solution of 2% by mass of boric acid for 60 seconds, and uniaxially stretched to 2.7 times in the length direction as a whole to adsorb boric acid (uniaxial stretching in the third stage). Then, the film was immersed in a stretching treatment bath (temperature 58° C.) containing an aqueous solution containing 3.9% by mass of boric acid, and uniaxially stretched along the length direction to 4.0 times the initial film length to orient it (uniaxial stretching in the fourth stage). Immediately after stretching, the film was immersed in a water tank (temperature 25° C.) as a washing tank for 5 seconds. Finally, the film was dried at 70° C. for 3 minutes to obtain the polarizing film of Example 1.
[0225] [Example 2]
[0226] In the preparation of the PVA film of Example 1, a PVA film and a polarizing film were obtained in the same manner except that 30 parts by mass of the modified conjugated diene polymer (B-1) was added.
[0227] [Example 3]
[0228] In the preparation of the PVA film of Example 1, a PVA film and a polarizing film were obtained by the same method except that 45 parts by mass of the modified conjugated diene polymer (B-1) was added.
[0229] [Example 4]
[0230] In the preparation of the PVA film of Example 3, a PVA film and a polarizing film were obtained by the same method except that the modified conjugated diene polymer (B-1) was changed to the modified conjugated diene polymer (B-2).
[0231] [Comparative Example 1]
[0232] In the preparation of the PVA film of Example 1, a PVA film and a polarizing film were obtained by the same method except that the modified conjugated diene polymer (B-1) was not added.
[0233] [Comparative Example 2]
[0234] In the preparation of the PVA film of Example 1, a PVA film and a polarizing film were obtained by the same method except that the modified conjugated diene polymer (B-1) was changed to an unmodified conjugated diene polymer (B′-1).
[0235] The above method was used to evaluate the stretching processability of each PVA film obtained in each embodiment and comparative example, the cleanability (productivity) of the metal drum in close contact when making the PVA film, and the formability of the polarizing film. The evaluation results are shown in Table 1. It should be noted that, with respect to Comparative Example 1, since the conjugated diene polymer was not added to the film-making stock solution of the PVA film, the evaluation of the cleanability (productivity) was not implemented. In addition, with respect to Comparative Example 2, since the conjugated diene polymer remained on the metal drum during the evaluation of the cleanability (productivity), the evaluation of the stretching processability and formability was not implemented.
[0236]
[0237] As shown in Table 1, the PVA films obtained in Examples 1 to 4 have low tensile stress and excellent tensile processability. In addition, in Examples 1 to 4, the conjugated diene polymer attached to the metal drum during the production of the PVA film can be easily removed by washing, and the washability is excellent. That is, it can be said that the PVA films of Examples 1 to 4 can shorten the cleaning time of the metal drum and have excellent productivity. Furthermore, the TD fracture deformation of the polarizing films obtained in Examples 1 to 4 is large, and it is not easy to break during molding. That is, the polarizing films obtained in Examples 1 to 4 have excellent moldability.
[0238] On the other hand, in Comparative Example 1 in which no conjugated diene polymer was added, the obtained PVA film had low stretching processability and poor formability of the obtained polarizing film. In addition, in Comparative Example 2 in which an unmodified conjugated diene polymer was added, the conjugated diene polymer attached to the metal drum during the production of the PVA film could not be easily removed by washing, and the washing property was poor. In other words, it can be said that the PVA film of Comparative Example 2 took time to wash the metal drum, and thus had low productivity.
[0239] Industrial Applicability
[0240] The PVA film of the present invention is used for packaging films, water-soluble films, agricultural films, release films, optical films, and the like, and is particularly suitable for use as a polarizing film as an optical film.
Claims
1. A polyvinyl alcohol film comprising polyvinyl alcohol (A) and a modified conjugated diene polymer (B) having a hydrophilic group, wherein the hydrophilic group is a graft chain having a repeating structure containing an ether group, The weight average molecular weight of the modified conjugated diene polymer (B) is 5,000 or more and 80,000 or less.
2. The polyvinyl alcohol film according to claim 1, wherein The content of the modified conjugated diene polymer (B) is 10 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the polyvinyl alcohol (A).
3. The polyvinyl alcohol film according to claim 1 or 2, wherein The degree of polymerization of the polyvinyl alcohol (A) is 1,000 or more and 10,000 or less, and the degree of saponification is 95 mol% or more. 4 . A stretched film obtained from the polyvinyl alcohol film according to claim 1 . 5 . A polarizing film obtained from the polyvinyl alcohol film according to claim 1 or the stretched film according to claim 4 .
6. A method for producing a polyvinyl alcohol film, comprising the step of using a film-forming stock solution to form a film, wherein the film-forming stock solution is obtained by mixing polyvinyl alcohol (A) with a dispersion containing a modified conjugated diene polymer (B) having a hydrophilic group, wherein the hydrophilic group is a graft chain having a repeating structure containing an ether group, and the weight average molecular weight of the modified conjugated diene polymer (B) is greater than 5,000 and less than 80,000.
7. The method for producing a polyvinyl alcohol film according to claim 6, wherein: The content of the modified conjugated diene polymer (B) in the film-forming stock solution is 10 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the polyvinyl alcohol (A).
Citation Information
Patent Citations
Curable resin composition
JP2015086283A
Method for producing graft copolymer, graft copolymer obtained by the method, rubber composition containing the graft copolymer, and tire
WO2010038835A1
Melt-processed blend containing polyvinyl alcohol
JP1996225703A
Oxygen-scavenging polymer composition containing ethylene-vinyl alcohol copolymer
JP2004526835A
Photosensitive resin structure for letterpress printing
JP2010188693A