A method for preparing potassium ion exchange membrane

Through the synergistic effect of graphene and valinomycin, a potassium ion exchange membrane with high potassium ion selectivity is prepared, which solves the problems of low potassium salt separation efficiency and poor stability in the existing technology, and realizes efficient and low-energy potassium ion exchange membrane. Salt purification effect.

CN114053879BActive Publication Date: 2024-10-11ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111536562.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-16
Publication Date
2024-10-11
Estimated Expiration
2041-12-16

AI Technical Summary

Technical Problem

The existing technology has problems such as insufficient selectivity, high energy consumption, and large salt consumption when separating potassium salts from concentrated brine, and it is difficult to effectively improve the separation efficiency of potassium ions.

Method used

Using graphene and a graft polymer of a liquid base polymer containing an amide structure in the side chain and valinomycin, through the synergistic effect of graphene's 2D nanochannels and valinomycin, high potassium ion selectivity and stability are prepared Potassium ion exchange membrane.

Benefits of technology

It significantly improves the selectivity and service life of potassium ions, reduces energy consumption, improves the dielectric properties and stability of the membrane, and achieves efficient purification of potassium salts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114053879B_ABST
    Figure CN114053879B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a potassium ion exchange membrane, comprising the following steps: adding graphene and a dispersant to a solvent to obtain a graphene dispersion; mixing a liquid base polymer containing an amide structure in a side chain with valinomycin, and reacting at 25 to 50° C. to obtain a grafted polymer; adding the obtained grafted polymer to a graphene dispersion to obtain a mixed dispersion of graphene-grafted polymers; casting the mixed dispersion into a film to obtain a potassium ion exchange membrane. In the ion exchange membrane prepared by the present invention, valinomycin and the base polymer form a grafted polymer by reaction, so that valinomycin in the obtained ion exchange membrane is not easy to fall off, the stability of the ion exchange membrane during use is ensured, and the service life can be improved; the present invention also composites graphene midway in the ion exchange membrane, utilizes the 2D nanochannel of graphene for ion transport, and improves the dielectric properties and stability of the membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange membranes, and in particular to a method for preparing a potassium ion exchange membrane. Background Art

[0002] With the increasing shortage of fresh water resources, obtaining fresh water from seawater has become an important means for people to solve the problem of fresh water shortage. After the seawater is desalinated, it will form two parts: desalinated fresh water and concentrated brine. Concentrated brine contains a large amount of metal salt components such as sodium, potassium, calcium, and magnesium. These salt components are often required in some other industrial production. Therefore, extracting salt components from concentrated brine can obtain higher economic benefits.

[0003] We can extract these resources from concentrated brine, which has higher economic benefits and environmental advantages than seawater. For example, potassium salts in seawater can be used to produce potassium fertilizers. For the production of potassium fertilizers, obtaining high-purity and high-concentration potassium salts from concentrated brine is an indispensable process. However, in concentrated brine, potassium salts usually exist together with a large amount of sodium salts and other ionic salts, which makes separation difficult. For example, the product yield of the recrystallization method is relatively low, the energy consumption of the electrostatic adsorption method is too high, and the salt consumption of the ion exchange method is very large. Compared with traditional separation technologies, membrane technology has the advantages of modularity, strong scalability, and low energy consumption. It is a method of separating potassium salts with industrial prospects. However, this method is more dependent on the performance of the exchange membrane. In order to achieve the separation efficiency of potassium ions, it is necessary to obtain an exchange membrane with high potassium ion selectivity and high permeability.

[0004] The patent document with patent application number CN201110422887.X discloses a sensing membrane for potassium ion selective electrode, a production method and its application. In the patent, the sensing membrane is made of a casting solution, and the components of the casting solution are: 20-40% polymer, 50-80% plasticizer, 2-10% ion selective carrier and 0.1-2% fat soluble salt, all calculated as weight percentage of the total weight of the solute, and the total content of the solute is 150-400 mg / mL; the polymer is one or more of carboxyl polyvinyl chloride, high molecular weight polyvinyl chloride, or polyurethane; the plasticizer is diisooctyl sebacate; the ion selective carrier is valinomycin; the fat soluble salt is potassium tetra(4-chlorophenyl) boric acid; the solvent is tetrahydrofuran or a mixture of tetrahydrofuran and acetone. The patent uses a polymer to load valinomycin with high potassium ion selectivity to prepare a sensing membrane with high potassium ion selectivity, which improves the selectivity for potassium ions, but there is still a need to further improve the selectivity. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing a potassium ion exchange membrane to obtain an exchange membrane with high potassium ion selectivity, long service life and low pollution.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a potassium ion exchange membrane comprises the following steps:

[0008] S1, adding graphene and a dispersant into a solvent to obtain a graphene dispersion;

[0009] S2, mixing a liquid base polymer having an amide structure in the side chain with valinomycin, and reacting at 25-50° C. to obtain a grafted polymer;

[0010] S3, adding the grafted polymer obtained in step S2 to the graphene dispersion obtained in step S1 to obtain a mixed dispersion of graphene-grafted polymer;

[0011] S4, casting the mixed dispersion into a film to obtain a potassium ion exchange membrane.

[0012] The present invention firstly utilizes a liquid base polymer containing an amide structure in the side chain to mix with valinomycin to obtain a grafted polymer composed of a base polymer and valinomycin. Specifically, the amide structure of the base polymer in the present invention is formed by condensation of a carboxyl group directly or indirectly connected to the polymer main chain and an amine-containing compound. During the reaction process between the base polymer and valinomycin, the amine-containing compound will be removed and replaced by valinomycin. The "liquid" here refers to a base polymer whose physical state is liquid at room temperature, and the most common ones are: poly (N-isopropylacrylamide), poly (N-tert-butylacrylamide), etc. In the present invention, the main structure of the membrane is formed by the base polymer. Since valinomycin reacts with the side chain of the base polymer, valinomycin and the base polymer form an integrated structure, so that valinomycin in the prepared potassium ion exchange membrane is not easy to fall off. The present invention also uses graphene to modify the potassium ion exchange membrane. Specifically, during the formation of the membrane, the base polymer-valinomycin grafted polymer forms a layer of intermediate substrate, and the graphene is deposited and compounded on the intermediate substrate to obtain a three-layer structure similar to graphene-intermediate substrate-graphene. The graphene is a regular mesh structure with uniformly distributed 2D nanochannels. The ions in the 2D nanochannel solution contact the intermediate substrate. Since the valinomycin in the intermediate substrate has an ion channel with high potassium ion selectivity, potassium ions in the ions passing through the 2D nanochannel will be preferentially selected, thereby obtaining high potassium ion selectivity. At the same time, the graphene layered structure can also play a surface protection role on the intermediate substrate, avoiding the falling off of valinomycin and the loss of the selective effect on potassium ions caused by the contamination of valinomycin by impurities in the solution.

[0013] Furthermore, step S2 also includes a step of removing the unreacted base polymer in the grafted polymer, the steps are as follows: dissolving the grafted polymer obtained by the reaction in excess anhydrous ether, then adding tetrahydrofuran thereto to precipitate and separate the grafted polymer; extracting the separated precipitate with tetrahydrofuran; drying the precipitate to obtain a grafted polymer free of base polymer. The unreacted base polymer will dissolve in tetrahydrofuran, while the base polymer-valinemycin grafted polymer will form a precipitate. The above method can be used to separate the base polymer from the grafted polymer, thereby improving the purity of the grafted polymer. In order to further enhance the purification effect, the obtained precipitate can be repeatedly dissolved, precipitated, and extracted before drying.

[0014] Furthermore, step S4 also includes the following steps: first, the mixed dispersion obtained in step S3 is filtered through a microporous filter membrane to obtain a graphene-polymer solid, and then the graphene-polymer solid is redispersed in a third solvent to obtain a newly prepared mixed dispersion, and finally the newly prepared mixed dispersion is cast into a film. After removing the unreacted base polymer, valinomycin may still remain in the mixed dispersion, so the mixed dispersion obtained in step S3 can be filtered. The microporous filter membrane (such as a polyamide microporous filter membrane) used in the filtration process should have a pore size larger than valinomycin and smaller than the grafted polymer, so that the grafted polymer is intercepted to form a precipitate, and the valinomycin is removed with the solvent. The obtained grafted polymer precipitate is dissolved again in an organic solvent to obtain a further purified newly prepared mixed dispersion.

[0015] Furthermore, the dispersant is selected from one or more of sodium dodecylbenzene sulfonate (SDBS), sodium cholate (SC), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), and 1-pyrenecarboxylic acid (PCA).

[0016] Furthermore, the first solvent is selected from one or more of chloroform, dichloromethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), and N, N-dimethylformamide (DMF).

[0017] Furthermore, the mass ratio of the graphene to the dispersant is (0.5~2):1.

[0018] Furthermore, in the mixed dispersion, the mass ratio of the grafted polymer to the graphene is (0.05-0.3):1; preferably, in the mixed dispersion, the mass ratio of the grafted polymer to the graphene is (0.15-0.2):1.

[0019] Furthermore, in step S2, the mass ratio of valinomycin to the base polymer is (0.002-0.01):1.

[0020] Furthermore, the reaction in S2 is carried out under a nitrogen protective atmosphere.

[0021] Furthermore, the base polymer is poly(N-isopropylacrylamide).

[0022] In summary, the application of the technical solution of the present invention can achieve the following beneficial effects:

[0023] (1) The potassium ion exchange membrane prepared by the present invention contains valinomycin, which is a highly potassium ion selective material that can significantly increase the diffusion rate of potassium ions while substantially not changing the diffusion rate of sodium ions, thereby purifying potassium salts from sodium salts that are more difficult to separate.

[0024] (2) In the potassium ion exchange membrane prepared by the present invention, valinomycin reacts with the base polymer to form a grafted polymer, so that the valinomycin in the obtained ion exchange membrane is not easy to fall off, thereby ensuring the stability of the ion exchange membrane during use and increasing the service life.

[0025] (3) The present invention also composites graphene in the potassium ion exchange membrane and utilizes the 2D nanochannels of graphene for ion transport. The addition of graphene material can effectively improve the dielectric properties and stability of the membrane.

[0026] (4) The preparation conditions of the present invention are mild and the process is relatively simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a SEM image of the potassium ion exchange membrane prepared in Example 2;

[0028] Figure 2 This is a SEM image of the potassium ion exchange membrane prepared in Example 5. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to specific embodiments. The operation methods involved in the present invention are all conventional methods in the art unless otherwise specified; the reagents and materials used in this experiment are all commercially available unless otherwise specified.

[0030] Example 1

[0031] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0032] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0033] ③ Take 1 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0034] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0035] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0036] Example 2

[0037] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0038] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0039] ③ Take 2 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0040] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0041] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0042] Example 3

[0043] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0044] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0045] ③ Take 3 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0046] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0047] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0048] Example 4

[0049] ① Weigh 20 mg of graphene and 20 mg of sodium cholate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0050] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0051] ③ Take 4 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0052] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0053] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0054] Example 5

[0055] ① Weigh 20 mg of graphene and 20 mg of sodium cholate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0056] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0057] ③ Take 6 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0058] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0059] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0060] Example 6

[0061] ① Weigh 20 mg of graphene and 20 mg of sodium cholate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0062] ② 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0063] ③ Take 7 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0064] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0065] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0066] Example 7

[0067] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0068] ② 5 g of poly (N-isopropylacrylamide) and 40 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0069] ③ Take 4 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0070] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0071] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0072] Example 8

[0073] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0074] ② 5 g of poly (N-isopropylacrylamide) and 20 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0075] ③ Take 4 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0076] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0077] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0078] Example 9

[0079] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0080] ② 5g of poly (N-isopropylacrylamide) and 10mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0081] ③ Take 4 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0082] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0083] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0084] Example 10

[0085] ① Weigh 20 mg of graphene and 20 mg of sodium dodecylbenzene sulfonate and add them to 200 mL of chloroform. Perform ultrasonic-assisted extraction at 25 °C to obtain a graphene dispersion for 48 h.

[0086] ② 5g of poly (N-isopropylacrylamide) and 60mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0087] ③ Take 4 mg of the grafted polymer obtained in step ② and mix it with the graphene dispersion prepared in step ①, and then perform ultrasonic treatment for 1 hour to obtain a mixed dispersion;

[0088] ④ Using a polyamide microporous filter membrane to vacuum filter the mixed dispersion obtained in ③, and then putting the filtered solid into chloroform again to obtain a new mixed dispersion;

[0089] ⑤ Cast the newly prepared mixed dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then peel it off to obtain a potassium ion exchange membrane.

[0090] Comparative Example 1

[0091] A sensing membrane for a potassium ion selective electrode, and a production method thereof, comprising the following specific steps:

[0092] (1) Add the solvent to the solute mixture under a fume hood at room temperature, add a clean magnetic particle, seal the bottle mouth with a sealing film, and place it on a magnetic stirrer to stir the solution at a stirring rate of 500-800r / min for 12 hours to ensure that the solutes and solvents are fully mixed;

[0093] (2) Use a glass pipette to transfer the evenly stirred solution to a flat and clean stainless steel membrane container, and cover the container with a glass cover so that the membrane solution can evaporate slowly and remain clean;

[0094] (3) The membrane produced after the solvent in the solution evaporates for 72 hours is the potassium ion sensing membrane.

[0095] The solute is composed of 30% high molecular weight polyvinyl chloride, 65% diisooctyl sebacate, 4% valinomycin and 1% potassium tetra(4-chlorophenyl)borate, and the solvent is tetrahydrofuran.

[0096] Comparative Example 2

[0097] Example 4

[0098] ① 5 g of poly (N-isopropylacrylamide) and 50 mg of valinomycin were stirred in a constant temperature bath at 40°C and subjected to nitrogen pressure vibration polymerization for 18 h to obtain a grafted polymer, and then the grafted polymer was dissolved in anhydrous ether, and tetrahydrofuran was added to the anhydrous ether to obtain a precipitate of the grafted polymer. After the grafted polymer precipitate was separated, the above dissolution and precipitation process was repeated twice, and the precipitate was extracted with tetrahydrofuran. Finally, the precipitate was dried under vacuum for 18 h to obtain a purified grafted polymer, and the grafted polymer was set aside;

[0099] ② dispersing the grafted polymer in chloroform to form a grafted polymer dispersion, vacuum filtering the grafted polymer dispersion using a polyamide microporous filter membrane, and then re-adding the filtered solid to chloroform to obtain a newly prepared grafted polymer dispersion;

[0100] ⑤ Cast the newly prepared graft polymer dispersion on a glass substrate to form a film, dry it at room temperature and pressure, and then obtain a potassium ion exchange membrane after peeling.

[0101] The properties of the films obtained in Examples 1 to 10 and the comparative examples are tested below.

[0102] The ion exchange experiment was conducted using a homemade electrodialysis device, which consists of two electrode chambers, a concentrated water chamber and a concentrated water chamber, with a channel diameter of 4 cm. First, the grafted polymer-graphene membrane was cut into a circle with a diameter of 4.5 cm, and then the grafted polymer-graphene membrane was installed inside. The effective area of ​​the membrane in the permeation experiment was 16 cm 2 . The fresh water side was filled with salt solutions (i.e., KNO3, NaNO3, LiNO3, Pb(NO3)2, Ca(NO3)2, Mg(NO3)2, Cr(NO3)3, 0.1mol / L, 200mL), while the concentrate side was filled with deionized water to the same level (200mL). The fresh water side and the concentrate side were always stirred, and the polar water chamber was circulated. The permeation experiment lasted for 24 hours. Then, the concentration of different ions was tested by using inductively coupled plasma emission spectrometry (ICP). The ion permeation experiment of each salt solution was repeated at least three times using the same membrane to minimize the experimental error.

[0103] (1) During the electrodialysis operation, the volume of the solution in each chamber does not change, K + / Na + Selectivity (S) is calculated as follows:

[0104]

[0105] Where: S is K + To Na + The selectivity coefficient of K +is the fresh water chamber K before and after electrodialysis + Concentration difference (mol / L); ΔC Na + is the Na in the fresh water chamber before and after electrodialysis + Concentration difference (mol / L); C K + It is K in the fresh water chamber of the electrodialysis device + Initial concentration (mol / L); C Na + It is the Na in the fresh water compartment of the electrodialysis device. + The selectivity data are recorded in Table 1.

[0106] (2) For the grafted polymer-graphene membranes prepared in Examples 1 to 6, the grafted polymer-graphene membranes were taken out after the permeation experiment was carried out for 24 hours, and were touched and pressed with a glass rod to observe whether they were easily damaged. The results are recorded in Table 2.

[0107] Table 1

[0108]

[0109] Table 2

[0110]

[0111] In summary, according to Table 1, except for Example 6, the potassium ion exchange membranes prepared by the method of the present invention in Examples 1 to 10 have the ability to separate Na + and K + The effect of K + / Na + The selectivity reached more than 2, which is better than the membrane made by the prior art in the comparative example. Obviously, the amount of valinomycin used in the comparative example is significantly higher than that in the embodiment of the present invention, but the selectivity of Examples 2 to 9 of the present invention for potassium ions is higher than that in the comparative example. This is because the 2D channel formed by graphene can improve the selectivity for potassium ions, thereby forming a synergistic effect with valinomycin. According to the data of Examples 1 to 6, when the content of the grafted polymer in the potassium ion exchange membrane is gradually increased, the K + / Na + The selectivity is also gradually improved, which is mainly because the content of valinomycin carried by the grafted polymer is gradually increasing. However, according to Table 2, when the content of the grafted polymer in the potassium ion exchange membrane is increased to a certain extent, that is, the grafted polymer: graphene = 0.3:1, the durability and physical strength of the membrane decrease. When the ratio of grafted polymer to graphene is further increased to 0.35:1, the membrane has been seriously damaged after being disturbed by the glass rod. According to the data of Example 6 in Table 1, the membrane prepared in Example 6 has lost K+ / Na + Selectivity, this is also because the strength of the membrane is insufficient. During use, the structure gradually collapses, thus losing the function of separating the two polar chambers. The inventor analyzed that the above phenomenon is because the increase in the proportion of grafted polymer will cause the mechanical properties of the membrane to deteriorate, the tensile strength will decrease, and it will affect the π-π attraction between the graphene nanosheets, so the stability in water deteriorates, resulting in long-term use and a short life. Therefore, the mass ratio of grafted polymer to graphene in the present invention is preferably (0.15~0.2):1. Combined with Comparative Example 2, the membrane prepared in Comparative Example 2 was severely damaged in structure after 24h of experiment, and lost its selectivity for potassium ions. Therefore, it can be judged that the addition of graphene can enhance the physical strength of the membrane during use. According to the data of Examples 4 and 7~10, it can be seen that when preparing potassium ion exchange membranes, the increase in the amount of valinomycin added can make K + / Na + The selectivity is improved, but from Examples 4 and 10, a higher selectivity can be obtained when the amount of valinomycin added is 1%, and further increasing the amount of valinomycin added has little effect on the selectivity. Therefore, the optimal range of the amount of valinomycin added should be 0.2%~1%.

[0112] From the attached figure, Figure 1 This is the microstructure diagram of the potassium ion exchange membrane when the ratio of grafted polymer to graphene is 0.1:1. Figure 2 This is the microstructure of the potassium ion exchange membrane when the ratio of grafted polymer to graphene is 0.3:1. It can be seen that Figure 1 The surface structure of the middle film is relatively flat, and the graphene is stacked in an orderly manner. Figure 2 The surface structure of the middle membrane is disordered and gully-shaped. The above changes are caused by grafting. Due to the van der Waals force between graphene nanosheets and grafted polymers, the grafted polymers can be regarded as a "net-like" structure evenly distributed in the two-dimensional nanochannels between graphene nanosheets. As the proportion of grafted polymers relative to graphene gradually increases, the number of grafted polymers between graphene nanosheets gradually increases, and the microstructure of grafted polymers is irregular, so the graphene nanosheets are affected and become irregularly arranged. In the case of irregular arrangement, the structural stability of the membrane is greatly reduced.

[0113] In summary, in the potassium ion exchange membrane prepared by the present invention, graphene can enhance the grafted polymer membrane, improve its physical strength and service life, and graphene and valinomycin can form a synergistic effect to further enhance the selectivity of valinomycin for potassium ions.

[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may also be combined, the steps may be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they may still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a potassium ion exchange membrane, comprising the following steps: S1, adding graphene and a dispersant into a solvent to obtain a graphene dispersion; S2, mixing a liquid base polymer having an amide structure in the side chain with valinomycin, and reacting at 25-50° C. to obtain a grafted polymer; S3, adding the grafted polymer obtained in step S2 to the graphene dispersion obtained in step S1 to obtain a mixed dispersion of graphene-grafted polymer; in the mixed dispersion, the mass ratio of the grafted polymer to the graphene is (0.15-0.2):1; S4, casting the mixed dispersion into a film to obtain a potassium ion exchange membrane.

2. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: Step S2 also includes removing the unreacted base polymer in the grafted polymer, and the steps are as follows: dissolving the grafted polymer obtained by the reaction in excess anhydrous ether, then adding tetrahydrofuran thereto to precipitate the grafted polymer and separate it; extracting the separated precipitate with tetrahydrofuran; and drying the precipitate to obtain a grafted polymer free of the base polymer.

3. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: Step S4 also includes the following steps: first filtering the mixed dispersion prepared in step S3 through a microporous filter membrane to obtain a graphene-polymer solid, then re-dispersing the graphene-polymer solid in a solvent to obtain a new mixed dispersion, and finally casting the new mixed dispersion into a film.

4. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: The dispersant is selected from one or more of sodium dodecylbenzene sulfonate, sodium cholate, polyvinyl chloride, polyvinyl pyrrolidone, and 1-pyrenecarboxylic acid.

5. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: In step S1, the mass ratio of graphene to dispersant is (0.5~2):

1.

6. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: In step S2, the mass ratio of valinomycin to the base polymer is (0.002-0.01):

1.

7. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: In step S2, the reaction is carried out under an inert gas protective atmosphere.

8. A method for preparing a potassium ion exchange membrane according to claim 1, characterized in that: The base polymer is poly(N-isopropylacrylamide).