A gallium doping method for producing single crystal silicon rods by Czochralski method

By using a specific ratio of gallium-silicon master alloy and silicon material, the problem of uneven concentration and dislocation during gallium element doping is solved, the full dissolution of gallium atoms and the improvement of crystal resistivity are achieved, improving the performance of single crystal silicon. Great quality.

CN114059152BActive Publication Date: 2024-10-15包头美科硅能源有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111373534.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-19
Publication Date
2024-10-15
Estimated Expiration
2041-11-19

AI Technical Summary

Technical Problem

In the production of single crystal silicon rods by Czochralski method, the low melting point and low segregation coefficient of gallium element during doping lead to uneven doping concentration and easy generation of dislocations during crystal growth, which affects product quality.

Method used

Gallium-silicon master alloy is used for doping. By mixing frozen pure gallium with silicon material and then rapidly cooling and crystallizing it, a high-concentration gallium-silicon master alloy is produced. During the melting process, it is mixed with silicon material in a specific ratio to dilute the gallium. The element concentration ensures that gallium atoms are fully dissolved in the silicon melt and reduces the generation of dislocations.

Benefits of technology

It effectively shortens the dissolution time of gallium element in silicon melt, reduces the probability of dislocation, improves the accuracy of crystal resistivity and finished product ratio, and reduces the resistivity deviation of the crystal head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114059152B_ABST
    Figure CN114059152B_ABST
Patent Text Reader

Abstract

The present invention discloses a gallium doping method for producing a single crystal silicon rod by a Czochralski method, which specifically comprises the following steps: (1) weighing frozen pure gallium and silicon material, mixing and placing them in a small crucible; (2) placing a plurality of small crucibles together in the same thermal field and melting them simultaneously; (3) after the melting is completed, rapidly cooling and crystallizing to produce a gallium-silicon master alloy; (4) placing the produced gallium-silicon master alloy and silicon material in a crucible and melting them simultaneously, and the melted silicon liquid dilutes the gallium concentration in the gallium-silicon master alloy; (5) performing Czochralski method single crystal growth after melting. The method is simple and easy to implement, and effectively solves the problem that the gallium-doped single crystal silicon rod is difficult to grow after the initial feeding and is prone to dislocation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a doping method for producing a Czochralski single crystal silicon rod, in particular to a gallium doping method for producing a Czochralski single crystal silicon rod, and belongs to the technical field of solar photovoltaics. Background Art

[0002] The P-type monocrystalline silicon rod materials used in the production of solar cells are mainly divided into two types: boron-doped and gallium-doped. For boron-doped Cz cells, when they are exposed to light, the cell performance will decay, which is the phenomenon of light-induced decay; while for gallium-doped cells, this light-induced decay is much smaller. Test data reported at home and abroad show that the decay efficiency of gallium-doped Cz cells is generally less than 1%, while the decay efficiency of boron-doped Cz cells is generally greater than 3%.

[0003] At present, the doping process of Czochralski single crystal silicon rod production when the doping element is gallium is as follows: Figure 1 The figure shows pure element doping, but gallium has a low melting point and will melt into liquid at room temperature. It is easy to adhere to the surface of the container during doping, causing loss, affecting the doping concentration and thus the resistivity characteristics of the crystal. The segregation coefficient of gallium in silicon crystal growth is low. During the crystal growth process, most of the gallium will be enriched in the melt. Pure gallium is doped into silicon melt. During the initialization of the material, the gallium is not fully dissolved in the silicon melt due to uneven mixing and stirring of the silicon melt and the gallium element. The formation of covalent bonds between gallium atoms and silicon atoms is prone to abnormal atomic arrangement, resulting in dislocations in the crystal, affecting product quality. However, after the secondary re-injection, the melt mixing time is longer, and the gallium element is fully dissolved in the silicon melt. Adding more silicon material is only equivalent to diluting the gallium concentration. The probability of dislocations during crystal growth is greatly reduced.

[0004] Based on the rules summarized from the growth of boron-doped single crystal silicon rods, the use of high-concentration alloy doping can effectively improve the problem of dislocation generation in the crystal after the initial feeding.

[0005] The process of gallium dissolving into silicon melt is the process of gallium atoms and silicon atoms forming covalent bonds. Because the radius of the gallium atom (1.40) and the radius of the silicon atom (1.34) are relatively close, the binding force of the atomic nucleus on the outermost electrons is similar; and the valence radius of the gallium atom (+3) is 0.47, and the valence radius of the silicon atom (+4) is 0.24, which further proves that the two atoms are slow in the process of forming covalent bonds, resulting in the slow dissolution of gallium in the silicon melt, which causes the incompletely dissolved gallium to enter the silicon crystal, causing dislocations in the crystal. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a gallium doping method for producing single crystal silicon rods by the Czochralski method. The method is simple and easy to implement and effectively solves the problem that crystal growth is difficult and dislocations are easily generated after the initial feeding of gallium-doped single crystal silicon rods.

[0007] In order to solve the above technical problems, the present invention provides a gallium doping method for producing single crystal silicon rods by Czochralski method, which specifically comprises the following steps:

[0008] (1) Weigh frozen pure gallium and silicon material, mix them and place them in a small crucible;

[0009] (2) Multiple small crucibles are placed together in the same heat field and melted simultaneously;

[0010] (3) After the melting is completed, the alloy is rapidly cooled and crystallized to produce a gallium-silicon master alloy;

[0011] (4) placing the produced gallium-silicon master alloy and silicon material into a crucible and melting them simultaneously, and the molten silicon liquid dilutes the gallium element concentration in the gallium-silicon master alloy;

[0012] (5) After melting, single crystal growth is carried out by the Czochralski method.

[0013] The technical solution further defined in the present invention is:

[0014] Furthermore, in the gallium doping method for producing single crystal silicon rods by the Czochralski method, the weight ratio of pure gallium to silicon material in step (1) is 1:1000 to 1:20.

[0015] In the gallium doping method for producing single crystal silicon rods by the Czochralski method, argon gas is continuously introduced during the melting process in step (2), and the argon gas flow rate is 30-200 slpm.

[0016] In the gallium doping method for producing single crystal silicon rods by the Czochralski method, in step (4), the weight ratio of gallium-silicon master alloy to silicon material is 1:50 to 1:500.

[0017] In the gallium doping method for producing single crystal silicon rods by the Czochralski method, the melting temperature in step (4) is 1500-1800° C. and the melting time is 3-20 hours.

[0018] In the gallium doping method for producing single crystal silicon rods by the Czochralski method, the gallium concentration before melting and dilution in step (4) is between 1×1018 and 9×1018 particles / cm³, and the gallium concentration after melting and dilution is between 1×1016 and 8×1016 particles / cm³.

[0019] The beneficial effects of the present invention are:

[0020] When impurity elements are directly mixed into silicon melt, the dissolution process is relatively slow and lasts for a long time. When silicon single crystal rods are grown before they are completely dissolved, dislocations are likely to occur. The present invention uses a high-concentration gallium-silicon alloy that has already been dissolved, and then increases the dilution concentration of the silicon material. The dissolution process time will be greatly shortened, reducing the probability of dislocations.

[0021] Since the segregation coefficient of gallium in silicon crystal is very low, it is impossible to produce alloy by crystal growth. In the present invention, gallium and silicon are mixed in a small quartz crucible in a quantitative ratio (gallium: silicon material = 1:1000-1:20), the silicon material is melted, fully mixed with gallium, and then quickly cooled and crystallized to produce gallium-silicon master alloy. Then, according to the element ratio requirements (the element ratio requirements are mainly based on the resistivity requirements of the output crystal), a fixed amount (weight ratio alloy: silicon material = 1:50-1 :500) gallium-silicon master alloy is added to the silicon material. The molten silicon liquid dilutes the gallium concentration in the gallium-silicon master alloy (the gallium concentration before melting and dilution is 1×1018-9×1018 / cm³, and the gallium concentration after melting and dilution is 1×1016-8×1016 / cm³). The gallium element is fully dissolved in the silicon melt, and the Czochralski single crystal grows. The gallium element is fully dissolved, and the gallium atoms have formed covalent bonds with the silicon atoms, which will not destroy the lattice structure and reduce the probability of dislocation, so as to meet the electrical performance requirements of the gallium-doped silicon single crystal rod.

[0022] The alloy used in the present invention can effectively accelerate the formation of covalent bonds between gallium and silicon atoms, reduce the probability of dislocation and disconnection of crystals caused by nucleation of gallium atoms, and reduce the number of times the first crystal is released from 3 times to less than 1.5 times.

[0023] The alloy doping of the present invention can effectively control the doping weight and improve the hit rate of crystal resistivity. The head resistivity deviation of the crystal doped with direct elements is within ±0.2Ω·cm, and the head resistivity deviation of the alloy doped crystal can be controlled within ±0.05Ω·cm, which effectively increases the proportion of qualified finished crystals by 3%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A flow chart of a gallium doping method for producing single crystal silicon rods by the Czochralski method in the prior art;

[0025] Figure 2 The present invention is a flow chart of the gallium doping method for producing single crystal silicon rods by the Czochralski method. DETAILED DESCRIPTION

[0026] Example 1

[0027] This embodiment provides a gallium doping method for producing single crystal silicon rods by Czochralski method, the process is as follows Figure 2 As shown, the specific steps include:

[0028] (1) Weigh frozen pure gallium and silicon material, mix them and place them in a small crucible;

[0029] The weight ratio of pure gallium to silicon is 1:1000~1:20. The amount of silicon placed in each crucible is 100~2000 grams, and the amount of pure gallium is 5~20 grams.

[0030] (2) Multiple small crucibles are placed together in the same heat field and melted simultaneously;

[0031] To maximize production, multiple crucibles can be placed in the same heat field to melt simultaneously;

[0032] Starting from the material processing, a certain flow of argon is continuously introduced, and the specific argon flow rate is 30~200SLPM;

[0033] (3) After the melting is completed, the alloy is rapidly cooled and crystallized to produce a gallium-silicon master alloy;

[0034] (4) placing the produced gallium-silicon master alloy and silicon material into a crucible and melting them simultaneously, and the molten silicon liquid dilutes the gallium element concentration in the gallium-silicon master alloy;

[0035] The weight ratio of gallium-silicon master alloy to silicon material is 1:50~1:500.

[0036] According to the existing normal single crystal production process conditions, the melting temperature is 1500~1800℃ and the melting time is 3~20 hours;

[0037] The gallium concentration before melting and dilution is 1×1018~9×1018 / cm³, and the gallium concentration after melting and dilution is 1×1016~8×1016 / cm³;

[0038] (5) After melting, single crystal growth is carried out by the Czochralski method.

[0039] When impurity elements are directly mixed into silicon melt, the dissolution process is relatively slow and lasts for a long time. When silicon single crystal rods are grown before they are completely dissolved, dislocations are likely to occur. The present invention uses a high-concentration gallium-silicon alloy that has already been dissolved, and then increases the dilution concentration of the silicon material. The dissolution process time will be greatly shortened, reducing the probability of dislocations.

[0040] The alloy doping of the present invention can effectively control the doping weight and improve the hit rate of crystal resistivity. The head resistivity deviation of the crystal doped with direct elements is within ±0.2Ω·cm, and the head resistivity deviation of the alloy doped crystal can be controlled within ±0.05Ω·cm, which effectively increases the proportion of qualified finished crystals by 3%.

[0041] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.

Claims

1. A gallium doping method for producing single crystal silicon rods by Czochralski method, characterized in that: The specific steps include: (1) Weigh frozen pure gallium and silicon material, mix them and place them in a small crucible; In step (1), the weight ratio of pure gallium to silicon material is 1:1000 to 1:

20. (2) Multiple small crucibles are placed together in the same heat field and melted simultaneously; In step (2), argon gas is continuously introduced during melting, with the argon gas flow rate being 30-200 slpm; (3) After the melting is completed, the alloy is rapidly cooled and crystallized to produce a gallium-silicon master alloy; (4) placing the produced gallium-silicon master alloy and silicon material into a crucible and melting them simultaneously, and the molten silicon liquid dilutes the gallium element concentration in the gallium-silicon master alloy; The weight ratio of gallium-silicon master alloy to silicon material is 1:50-1:

500. The melting temperature is 1500-1800°C and the melting time is 3-20 hours. (5) After melting, single crystal growth is carried out by the Czochralski method.

2. The gallium doping method in the production of single crystal silicon rods by the Czochralski method according to claim 1, characterized in that: In step (4), the gallium concentration before melting and dilution is between 1×1018 and 9×1018 pieces / cm³, and the gallium concentration after melting and dilution is between 1×1016 and 8×1016 pieces / cm³.