A method for reverse aging of aluminum electrolytic capacitors
By performing reverse aging after forward aging of aluminum electrolytic capacitors, the problems of cathode foil and cathode lead foil defects were solved, resulting in longer capacitor life and improved safety.
Patent Information
- Application Number
- CN202010817382.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-08-14
AI Technical Summary
The existing forward aging process for aluminum electrolytic capacitors cannot effectively repair defects in the cathode foil and cathode lead foil, resulting in severe hydration, increased gas production and heat generation, and the regeneration voltage can easily damage the circuit board, posing a safety hazard.
After forward aging, reverse aging is performed by reversing the positive and negative terminals of the capacitor and applying a low voltage to repair defects in the cathode foil and cathode lead foil.
It effectively reduces the risk of hydration of the cathode foil, reduces capacitor polarization effect, extends capacitor life, and reduces the harm caused by regeneration voltage.
Smart Images

Figure QLYQS_2 
Figure QLYQS_4 
Figure QLYQS_6
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum electrolytic capacitors, and in particular to a reverse aging method for aluminum electrolytic capacitors. Background Art
[0002] Aluminum electrolytic capacitors include core packs, electrolytes, and encapsulated aluminum shells and covers; the core packs are mainly composed of lead foils, anode foils, cathode foils, and electrolytic paper, all of which need to be cut into corresponding sizes according to the specifications of aluminum electrolytic capacitors. The manufacturing process of aluminum electrolytic capacitors includes: cutting, winding, impregnation, assembly, aging, and packaging.
[0003] In the prior art, aluminum electrolytic capacitors are usually only subjected to forward aging when undergoing an aging process, that is, the anode and cathode of the aging power supply are connected to the positive and negative electrodes of the capacitor respectively, and the boost aging is performed according to the aging process required by the capacitor specifications. According to the principle of electrochemical reaction, the forward aging process only repairs the defects of the anode foil and the anode lead foil with an oxide film, and the defects are mainly the cutting edge of the anode foil, the oxide film defects on the surface of the anode foil, and the cutting edge of the anode lead foil. However, the cutting and oxide film defects of the cathode foil and the cathode lead foil cannot be effectively repaired, which will cause the cathode foil to be easily hydrated during use, causing serious gas production, increased losses, and increased heat generation, thereby increasing the risk of premature valve opening failure. In addition, when the aluminum electrolytic capacitor is only subjected to forward aging, the capacitor is prone to regeneration voltage after being placed in the warehouse for a period of time. If the high regeneration voltage is not discharged during the use of the capacitor, it is easy to damage the circuit board, and even cause physical danger to the installer. Sparking when the positive and negative electrodes are short-circuited also brings great inconvenience to the installation. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes a new aluminum electrolytic capacitor aging process, which performs reverse aging after the forward aging of the capacitor product, that is, the positive and negative electrodes of the capacitor are reversely connected to the aging power supply, and low voltage (U≤50V) is loaded for aging. After reverse aging, the defects of the cathode foil and cathode lead foil of the product are effectively repaired, which can greatly reduce the hydration risk of the cathode foil, and can effectively reduce the charge of the positive and negative electrode areas, reduce the polarization effect of the capacitor, and effectively weaken the regenerative voltage of the capacitor, thereby extending the life of the capacitor and reducing the harm caused by the regenerative voltage.
[0005] To achieve the above object, the present invention adopts the following technical solutions.
[0006] The present invention provides a reverse aging method for an aluminum electrolytic capacitor, comprising:
[0007] Forward aging of aluminum electrolytic capacitors;
[0008] After the forward aging is completed, the positive and negative poles of the capacitor are reversely connected to the aging power supply for reverse aging.
[0009] The forward aging process can be performed according to methods known in the art.
[0010] The forward aging includes a positive 1 aging stage, a positive 2 aging stage and a positive 3 aging stage. The positive 1 aging stage is a boost stage, the positive 2 aging stage is a high temperature aging stage, and the positive 3 aging stage is a normal temperature aging stage.
[0011] Specifically, in the first aging stage of forward aging, the voltage is first increased to a value higher than the rated voltage, and then the voltage is maintained constant for a period of time. After the first aging stage, the voltage is discharged to 0V; in the second aging stage, the voltage is increased to the rated voltage again, and then the voltage is maintained constant at high temperature for a period of time. After the first aging stage, the voltage is discharged to 0V; in the third aging stage, the voltage is increased to the rated voltage again, and the voltage is maintained constant at room temperature for a period of time. After the third aging stage, the voltage is discharged to 0V, and the forward aging is completed.
[0012] According to the embodiment provided by the present invention, the parameters related to the positive first aging stage include: the boost current is mA / capacitor, the boosted voltage value is U+20~U+40V, and the voltage is kept constant for 30~120min, and the temperature is 25~55℃; where C is the rated capacity of the capacitor and U is the rated voltage of the capacitor.
[0013] Specifically, the first aging stage:
[0014] The boost current can be listed as: mA / only, mA / only, mA / only, mA / only, mA / only, mA / piece, etc.
[0015] The boosted voltage values include: U+20V, U+23V, U+25V, U+28V, U+30V, U+33V, U+35V, U+38V, U+40V, and the like.
[0016] The constant pressure time can be listed as: 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min, 100min, 105min, 110min, 115min, 120min, and the like.
[0017] The aging temperature may be 25°C, 30°C, 35°C, 40°C, 45°C, 40°C, 55°C, and the like.
[0018] According to the embodiment provided by the present invention, the positive first aging stage is completely discharged after the end of the positive second aging stage, and the positive second aging stage is started. The positive second aging stage is a high temperature aging stage. The relevant parameters include: the boost current is mA / capacitor, the boosted voltage value is U, and the voltage is kept constant for 180 to 240 minutes, and the constant voltage temperature is 85℃ to 95℃; where C is the rated capacity of the capacitor and U is the rated voltage of the capacitor.
[0019] Specifically, the second aging stage:
[0020] The boost current can be listed as: mA / only, mA / only, mA / only, mA / only, mA / only, mA / piece, etc.
[0021] The constant pressure time can be listed as: 180min, 185min, 190min, 195min, 200min, 205min, 210min, 215min, 220min, 225min, 230min, 235min, 240min, and the like.
[0022] The aging temperature can be exemplified by 85°C, 90°C, 95°C, and the like.
[0023] According to the embodiment provided by the present invention, the positive second aging stage is completely discharged after the end of the positive third aging stage, and the positive third aging stage is a normal temperature aging stage. The relevant parameters include: the aging current is mA / capacitor, the boosted voltage value is U, and the voltage is kept constant for 30 to 120 minutes at a temperature of 25 to 55°C; where C is the rated capacity of the capacitor and U is the rated voltage of the capacitor.
[0024] Specifically, the three aging stages are:
[0025] The boost current can be listed as: mA / only, mA / only, mA / only, mA / only, mA / only, mA / piece, etc.
[0026] The constant pressure time can be listed as: 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min, 100min, 105min, 110min, 115min, 120min, and the like.
[0027] The aging temperature may be 25°C, 30°C, 35°C, 40°C, 45°C, 40°C, 55°C, and the like.
[0028] After the forward aging is completed, the positive and negative electrodes are reversed for reverse aging. The reverse aging includes a reverse aging stage 1, a non-pressurized stage, and a reverse aging stage 2. The reverse aging stage 1 is a boost stage, and the reverse aging stage 2 is a constant pressure stage.
[0029] Specifically, in the reverse aging stage of reverse aging, the voltage is first boosted to the set voltage, and then the voltage is kept constant for a period of time. After the reverse aging stage, it is discharged to 0V; in the no-voltage stage, 0V is maintained for a period of time; in the reverse aging stage, the voltage is boosted to the set voltage (consistent with the set voltage in the reverse aging stage), and then the voltage is kept constant for a period of time. After the reverse aging stage, it is discharged to 0V, and the reverse aging ends.
[0030] According to the implementation mode provided by the present invention, the anti-aging stage is a boost stage, and the relevant parameters include: the boost current is 1 to 10 mA / unit, the boosted voltage value is 15 to 50 V, the voltage is kept constant for 5 to 15 minutes, and the temperature is 25 to 55°C.
[0031] Specifically, the reverse aging stage:
[0032] The boost current may be 1 mA / battery, 2 mA / battery, 3 mA / battery, 4 mA / battery, 5 mA / battery, 6 mA / battery, 7 mA / battery, 8 mA / battery, 9 mA / battery, 10 mA / battery, and the like.
[0033] The boosted voltage values include: 15V, 20V, 25V, 30V, 35V, 40V, 45V, 50V, and the like.
[0034] The constant pressure time can be listed as: 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, and the like.
[0035] The aging temperature may be 25°C, 30°C, 35°C, 40°C, 45°C, 40°C, 55°C, and the like.
[0036] According to the embodiment provided by the present invention, the non-pressurized stage is: after the reverse-aging stage, discharge to 0V, no pressure is applied, and maintained at 0V for 5-10 minutes, such as 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc. The function is to absorb the gas generated in the reverse-aging stage.
[0037] According to the implementation mode provided by the present invention, the anti-second aging stage is a constant voltage stage, and the relevant parameters include: the boost current is 1 to 10 mA / unit, the boosted voltage value is 15 to 50 V, the voltage is kept unchanged, the constant voltage is 30 to 60 minutes, and the temperature is 25 to 55°C.
[0038] Specifically, the second aging stage:
[0039] The boost current may be 1 mA / battery, 2 mA / battery, 3 mA / battery, 4 mA / battery, 5 mA / battery, 6 mA / battery, 7 mA / battery, 8 mA / battery, 9 mA / battery, 10 mA / battery, and the like.
[0040] The boosted voltage values include: 15V, 20V, 25V, 30V, 35V, 40V, 45V, 50V, and the like.
[0041] The constant pressure time can be exemplified as: 30 min, 35 min, 40 min, 45 min, 50 min, 60 min, and the like.
[0042] The aging temperature may be 25°C, 30°C, 35°C, 40°C, 45°C, 40°C, 55°C, and the like.
[0043] Compared with the prior art, the present invention has the following technical effects:
[0044] The present invention adds a reverse aging process after the capacitor is forward aged. After reverse aging, defects in the cathode foil and cathode lead foil of the capacitor are effectively repaired, which can greatly reduce the hydration risk of the cathode foil, effectively reduce the charge in the positive and negative electrode regions, reduce the polarization effect of the capacitor, and effectively weaken the generation of the regenerative voltage of the capacitor, thereby extending the life of the capacitor and reducing the harm caused by the regenerative voltage. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the forward aging process diagram;
[0046] Figure 2 is a reverse aging process diagram; and
[0047] Figure 3 It is the regeneration voltage curve. DETAILED DESCRIPTION
[0048] Unless otherwise specified, all scientific and technological terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. All patents and publications related to the present invention are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, that is, including the contents specified in the present invention, but does not exclude contents in other aspects.
[0049] The embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings and examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0050] Implementation
[0051] 1. Experimental process
[0052] The normal manufacturing process of aluminum electrolytic capacitors with specifications of 450V820μF 35*50: cutting, winding, impregnation, and assembly into capacitors.
[0053] Group A was aged according to the normal process, that is, only forward aging was performed. The forward aging process was as follows: Figure 1 As shown;
[0054] After forward aging, group B returns to room temperature (e.g., 25°C) and then performs reverse aging. The reverse aging process is as follows: Figure 2 shown.
[0055] The forward aging and reverse aging processes are specifically as follows:
[0056] Forward aging process:
[0057] Positive aging stage: the boost current is 9.1mA / pcs, the voltage is raised to 470V, and the voltage is kept constant for 30min, the temperature is 55℃;
[0058] Positive 2 aging stage: boost current is 9.1mA / pcs, voltage is raised to 450V, and the voltage is kept constant for 180min, temperature is 85℃;
[0059] Positive three aging stage: the boost current is 9.1mA / pcs, the voltage is increased to 450V, and the voltage is kept constant for 30min, the temperature is 25℃.
[0060] Reverse aging process:
[0061] Reverse aging stage: the boost current is 3mA / pcs, the voltage is raised to 25V, and the voltage is kept constant for 10min, the temperature is 55℃;
[0062] No-pressurization stage: no pressurization, maintain 0V for 10min;
[0063] Reverse aging stage: boost current is 3mA / pcs, raise voltage to 25V, and keep the voltage constant for 30min, room temperature.
[0064] 2. Performance Testing
[0065] After the two groups were aged, various performance tests were carried out.
[0066] (1) Take 4 products from each group A and B, and place them at room temperature for 30 days. Test the regeneration voltage value every day and take the average value to draw the regeneration voltage curve, such as Figure 3 As shown;
[0067] (2) Take 4 products from each group A and B, respectively, and carry out load test in a 125℃ oven for 1000h, then test the loss and bulging degree of the products and disassemble and analyze the hydration of the cathode foil, see Table 1 for details;
[0068] (3) Four products from each group A and B were taken for load test in a 125°C oven to examine the life test time and valve failure of the two products. The leakage time and leakage amount of the two products were counted, as shown in Table 1.
[0069] Table 1
[0070]
[0071] From Table 1 and Figure 3 It can be seen that after group A and group B were placed in the warehouse with an open circuit for a period of time, the regeneration voltage of group A was significantly higher than that of group B; group A reached the regeneration voltage peak in about 23 days, and group B reached the regeneration voltage peak in about 13 days, and group A was significantly higher than group B; this shows that reverse aging can effectively reduce the regeneration voltage of the product.
[0072] As shown in Table 1, after the two groups of products were subjected to a 125℃ 1000h load test, the loss and bulging degree of group A products were significantly higher than those of group B. Disassembly analysis found that the cathode foils of the four products in group A all showed varying degrees of hydration and blackening, while the cathode foils of all products in group B were normal; this indicates that the reverse aging process can effectively solve the problem of cathode foil hydration and gas production.
[0073] As shown in Table 1, two bottom valves of Group A products leaked during the 125℃ 2250h life test, while Group B products were able to complete the 125℃ 3000h life test. This indicates that the reverse aging process can effectively reduce the gas generation caused by the hydration of the cathode foil.
[0074] In the description of this specification, the description with reference to the terms "some embodiments", "other embodiments", "embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0075] Although the embodiments and examples of the present invention have been shown and described above, it is to be understood that the above embodiments and examples are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments and examples within the scope of the present invention.
Claims
1. A reverse aging method for aluminum electrolytic capacitors, characterized in that: include: Forward aging of aluminum electrolytic capacitors; After the forward aging is completed, the positive and negative electrodes of the capacitor are reversely connected to the aging power supply for reverse aging; The reverse aging includes a reverse aging stage, a non-pressurized stage and a reverse aging stage; The reverse aging process includes: the reverse aging stage of reverse aging first boosts the voltage to a set voltage, then maintains a constant voltage for a period of time, and discharges to 0V after the reverse aging stage ends; Set the voltage to 15~50V; In the non-pressurized stage, 0V is maintained for a period of time; In the reverse aging stage, the voltage is boosted to the set voltage, and then kept constant for a period of time. After the reverse aging stage is over, it is discharged to 0V and the reverse aging is over; the set voltage is 15~50V.
2. The reverse aging method for aluminum electrolytic capacitors according to claim 1, characterized in that: The forward aging includes a positive first aging stage, a positive second aging stage and a positive third aging stage.
3. The reverse aging method of aluminum electrolytic capacitor according to claim 2, characterized in that: The forward aging process includes: in the first positive aging stage of forward aging, the voltage is first increased to a value higher than the rated voltage, and then the voltage is maintained constant for a period of time, and the voltage is discharged to 0V after the first positive aging stage ends; in the second positive aging stage, the voltage is increased to the rated voltage again, and then the voltage is maintained constant at high temperature for a period of time, and the voltage is discharged to 0V after the second positive aging stage ends; in the third positive aging stage, the voltage is increased to the rated voltage again, and the voltage is maintained constant at room temperature for a period of time, and the voltage is discharged to 0V after the third positive aging stage ends, thereby completing the forward aging.
4. The reverse aging method for aluminum electrolytic capacitors according to claim 2 or 3, characterized in that: The positive first aging stage is the boost stage, and the relevant parameters include: the boost current is ~ mA / capacitor, the boosted voltage value is U+20~U+40 V, and the voltage is kept constant for 30~120 minutes, and the temperature is 25~55℃; among them, C is the rated capacity of the capacitor, and U is the rated voltage of the capacitor.
5. The reverse aging method for aluminum electrolytic capacitors according to claim 2 or 3, characterized in that: After the positive first aging stage is completed, the discharge is complete, and the positive second aging stage begins. The positive second aging stage is a high temperature aging stage. The relevant parameters include: the boost current is ~ mA / capacitor, the boosted voltage value is U, and the voltage is kept constant for 180~240min, and the constant voltage temperature is 85~95℃; among them, C is the rated capacity of the capacitor, and U is the rated voltage of the capacitor.
6. The reverse aging method for aluminum electrolytic capacitors according to claim 2 or 3, characterized in that: After the positive second aging stage is completed, the discharge is complete, and the positive third aging stage begins. The positive third aging stage is a normal temperature aging stage. The relevant parameters include: the boost current is ~ mA / capacitor, the boosted voltage value is U, and the voltage is kept constant for 30~120min, and the temperature is 25~55℃; where C is the rated capacity of the capacitor and U is the rated voltage of the capacitor.
7. The reverse aging method for aluminum electrolytic capacitors according to claim 1, characterized in that: The reverse aging stage is a boost stage, and the relevant parameters include: the boost current is 1-10 mA / unit, the boosted voltage value is 15-50 V, the voltage is kept constant for 5-15 minutes, and the temperature is 25-55° C.
8. The reverse aging method of aluminum electrolytic capacitor according to claim 1, characterized in that: The non-pressurized stage is: discharging to 0V after the reverse aging stage, and maintaining at 0V for 5-10 minutes.
9. The reverse aging method of aluminum electrolytic capacitor according to claim 1, characterized in that: The reverse aging stage is a constant voltage stage, and the relevant parameters include: the boost current is 1-10 mA / unit, the boosted voltage value is 15-50 V, the voltage is kept constant for 30-60 minutes, and the temperature is 25-55° C.