Electronic device housing and preparation method thereof, and electronic device

By forming chemical bond connections in the coating layer of the electronic device shell, the problem of poor bonding force between the UV texture layer and the coating layer is solved, and a better appearance effect and a thinner shell structure are achieved, which meets the lightness and fitting Require.

CN114096092BActive Publication Date: 2024-11-01GUANGDONG OPPO MOBILE TELECOMMUNICATIONS CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111370977.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-11-01
Estimated Expiration
2041-11-18

AI Technical Summary

Technical Problem

When the existing electronic equipment shell transfers the UV texture layer on the coating layer, the bonding force between the UV texture layer and the coating layer is poor, resulting in poor appearance effect and increased thickness of the composite film layer, making it difficult to meet the trend of lightweighting and fitting. Require.

Method used

A chemical bond connection is formed between the first coating layer and the second UV texture layer. By adding a coupling agent to the UV material of the second UV texture layer, it reacts chemically with the first coating layer, and improves binding force. Reduce the use of intermediate layers, simplify the process and reduce costs.

Benefits of technology

The bonding strength between the second UV texture layer and the first coating layer is significantly improved, the overall thickness of the composite film layer and the shell is thinned, the appearance effect is improved, the folds and bubbles are avoided, and the market competitiveness is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114096092B_ABST
    Figure CN114096092B_ABST
Patent Text Reader

Abstract

The present application discloses an electronic device housing, a preparation method thereof, and an electronic device. The electronic device housing comprises: a housing body; a first UV texture layer, the first UV texture layer being arranged on one side of the housing body; a first coating layer, the first coating layer being arranged on a surface of the first UV texture layer away from the housing body; a second UV texture layer, the second UV texture layer being arranged on a surface of the first coating layer away from the housing body, wherein the second UV texture layer comprises a coupling agent, and the first coating layer and the coupling agent are chemically bonded. Thus, not only can the bonding strength between the second UV texture layer and the first coating layer be significantly improved, and the problem of poor bonding strength of the transfer UV glue on the coating layer can be solved; the overall thickness of the electronic device housing can also be thinned on the basis of achieving a better appearance effect, and the bonding effect of the texture layer and the coating layer with the electronic device housing body can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of material technology, and specifically relates to an electronic device housing and a preparation method thereof, and an electronic device. Background Art

[0002] At present, many studies are devoted to making textures and coatings on the outer surface of the shell of terminal products such as mobile phones to improve the appearance of the outer surface of the shell, such as brightness, glare, color, etc. For example, UV glue can be used to make texture patterns on the outer surface of the shell through inkjet printing and UV transfer, and combined with coating to achieve better appearance expression. However, when a UV texture layer is directly formed on the coating, there is a problem of poor bonding between the UV texture layer and the coating. Summary of the invention

[0003] In one aspect of the present application, the present application proposes an electronic device housing. The electronic device housing comprises: a housing body; a first UV texture layer, the first UV texture layer is arranged on one side of the housing body; a first coating layer, the first coating layer is arranged on the surface of the first UV texture layer away from the housing body; a second UV texture layer, the second UV texture layer is arranged on the surface of the first coating layer away from the housing body, wherein the second UV texture layer comprises a coupling agent, and the first coating layer and the coupling agent are chemically bonded. Thus, not only can the bonding strength between the second UV texture layer and the first coating layer be significantly improved, and the problem of poor bonding force of transferring UV glue on the coating layer can be solved; but also the overall thickness of the electronic device housing can be thinned on the basis of achieving a better appearance effect, and the bonding effect of the texture layer and the coating layer with the electronic device housing body can be improved.

[0004] In another aspect of the present application, the present application proposes a method for preparing an electronic device housing. The method comprises: providing a housing body; transferring a first UV texture layer on one side of the housing body; forming a first coating layer on the surface of the first UV texture layer away from the housing body; transferring a second UV texture layer on the surface of the first coating layer away from the housing body, wherein the UV adhesive for forming the second UV texture layer comprises a coupling agent, and the first coating layer and the coupling agent are chemically bonded. Therefore, the method is not only simple in process and low in cost, but also has good bonding strength between the second UV texture layer and the first coating layer of the electronic device housing, the overall thickness of the electronic device housing is thin, and a good appearance effect can be achieved.

[0005] In another aspect of the present application, the present application proposes an electronic device. The electronic device includes: the electronic device housing described above, or an electronic device housing made by the method for preparing an electronic device housing described above; a display screen assembly, the display screen assembly is connected to the electronic device housing, and an installation space is defined between the display screen assembly and the electronic device housing, wherein the housing body in the electronic device housing is arranged away from the installation space; and a main board, the main board is arranged in the installation space and is electrically connected to the display screen assembly. Thus, the electronic device has all the features and advantages of the electronic device housing described above and the method for preparing the electronic device housing described above, which will not be repeated here. In general, the electronic device has a better appearance effect and good appearance expression, which can further enhance the overall appearance effect of the electronic device and enhance its market competitiveness.

[0006] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0008] Figure 1 It is a structural schematic diagram of a single-layer PET single-grain single-coated film in the related art.

[0009] Figure 2 It is a schematic diagram of the structure of a double-layer PET double-grain double-coated sheet in the related art.

[0010] Figure 3 It is a schematic structural diagram of an electronic device housing according to an embodiment of the present application.

[0011] Figure 4 It is a schematic structural diagram of a first coating layer in an electronic device housing according to an embodiment of the present application.

[0012] Figure 5 It is a structural schematic diagram of an electronic device housing according to another embodiment of the present application.

[0013] Figure 6 It is a schematic structural diagram of an electronic device housing according to yet another embodiment of the present application.

[0014] Figure 7 The present invention is a flowchart of a method for preparing an electronic device housing according to an embodiment of the present application.

[0015] Figure 8 The present invention is a flowchart of a method for preparing an electronic device housing according to another embodiment of the present application.

[0016] Fig. 9 It is a schematic diagram of the appearance structure of an electronic device housing according to an embodiment of the present application.

[0017] Fig.10 This is a transmission electron microscope image of a partial structure of an electronic device housing prepared according to Example 3 of the present application.

[0018] Fig.11 This is an XPS signal diagram of the P element at the Al2O3-phosphate interface obtained by performing XPS characterization on the contact interface between the first coating layer and the second UV texture layer in Example 1 of the present application using X-ray photoelectron spectroscopy.

[0019] Fig.12 This is an XPS signal diagram of the P element at the TiO2-phosphate interface obtained by performing XPS characterization on the contact interface between the first coating layer and the second UV texture layer in Example 2 of the present application using X-ray photoelectron spectroscopy.

[0020] Fig.13 This is an XPS signal diagram of the P element at the SiO2-phosphate interface obtained by performing XPS characterization on the contact interface between the first coating layer and the second UV texture layer in Comparative Example 1 of the present application using X-ray photoelectron spectroscopy.

[0021] Fig.14 It is an XPS signal diagram of the P element at the Si-phosphate interface obtained by performing XPS characterization on the contact interface between the first coating layer and the second UV texture layer in Comparative Example 2 of the present application using X-ray photoelectron spectroscopy.

[0022] Fig.15 The comparison diagram is a spectrum analysis of the contact interface between the Al2O3 layer of the neutron coating layer and the second UV texture layer in Comparative Example 4 and Example 5 of the present application using a transmission electron microscope (wherein, Fig.15 (a) is the structure and energy spectrum of the first coating layer and the second UV texture layer in Comparative Example 4 at low magnification, (b) is the structure and energy spectrum of the first coating layer and the second UV texture layer in Comparative Example 4 at high magnification, c) is the structure and energy spectrum of the first coating layer and the second UV texture layer in Example 5 at low magnification, and (d) is the structure and energy spectrum of the first coating layer and the second UV texture layer in Example 5 at high magnification).

[0023] Description of reference numerals:

[0024] Shell body: 10; first UV texture layer: 20; first coating layer: 30; second UV texture layer: 40; second coating layer: 50; ink layer: 60; optical adhesive layer: 70; PET film: 80; sub-coating layer in contact with the second UV texture layer 40: 31; low-refractive-index sub-coating layer not in contact with the second UV texture layer: 32; high-refractive-index sub-coating layer not in contact with the second UV texture layer: 33; electronic device shell: 100. DETAILED DESCRIPTION

[0025] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.

[0026] In one aspect of the present application, the present application provides an electronic device housing. According to an embodiment of the present application, reference is made to Figure 3 It is understood that the electronic device housing 100 includes: a housing body 10, a first UV texture layer 20, a first coating layer 30 and a second UV texture layer 40. Among them, the first UV texture layer 20 is arranged on one side of the housing body 10; the first coating layer 30 is arranged on the surface of the first UV texture layer 20 away from the housing body 10; the second UV texture layer 40 is arranged on the surface of the first coating layer 30 away from the housing body 10; the second UV texture layer 40 includes a coupling agent, and there is a chemical bond connection between the first coating layer 30 and the coupling agent. It should be noted that the chemical bond connection is achieved by the chemical reaction between the first coating layer material and the coupling agent to form a new chemical bond. For example, when phosphate ester is used as a coupling agent and Al2O3 exists in the area where the first coating layer contacts the second UV texture layer, the phosphate ester will react chemically with Al2O3 to form an Al-P bond, and the Al-P bond can improve the interface bonding force between the first coating layer and the second UV texture layer.

[0027] According to the embodiments of the present application, the decorative films currently available on the market are generally single-layer PET single-grain single-coating films and double-layer PET double-grain double-coating films. The single-layer PET single-grain single-coating film has only one layer of texture and one layer of coating (with Figure 1 For example, one side of the PET layer A is only provided with a UV texture layer B and a coating layer C), which is limited in terms of brightness, color and glare effect, and has problems of single effect and insufficient expression, which is not enough to support the current high-end, fashionable and high-quality appearance. To improve the appearance, a double-layer PET double-texture double-coated sheet can be used. For specific solutions, please refer to Figure 2It is understood that the UV1 texture layer B1 is transferred onto the PET raw material A1, and the coating layer C1 is made on the UV1 texture layer B1, the UV2 texture layer B2 is transferred onto the PET raw material A2, and the coating layer C2 is made on the UV2 texture layer B2, and then the ink layer is made on the coating layer C2, and the PET raw material A1 and the PET raw material A2 are laminated, which can be specifically achieved by the OCA layer D. The schematic diagram of the structure after lamination is shown as follows Figure 2 As shown, although this solution has a significant improvement in appearance, it requires the use of two layers (PET) of film for compounding, the process is more complicated, the use of raw materials is doubled, and the cost will increase significantly. At the same time, due to the addition of a layer of PET raw material, the overall thickness of the film increases, which is inconsistent with the current trend of thinner and lighter products such as mobile phones. More importantly, due to the increase in the thickness of the film, the difficulty of bonding with substrates such as glass increases. When bonding glass with a larger angle, it is easy to produce bonding wrinkles and bubbles. Therefore, there are certain limitations in its application. In view of this, the inventor found that the UV2 texture layer can be directly transferred on the coating layer C1 to reduce the use of the intermediate layer. Specifically, a double-texture double-plating solution can be used on the same side of the shell body to overcome the above problems, that is, the first UV texture layer, the first coating layer, the second UV texture layer, and the second coating layer can be formed in sequence on the same side of the shell body. However, the inventor found in practice that:

[0028] Combination Figure 3It is understood that the bonding force between the first UV texture layer 20 and the first coating layer 30 is usually guaranteed, but the bonding force between the first coating layer 30 and the second UV texture layer 40 is the difficulty and main risk point of the lamination process. This is because when the first coating layer 30 is produced after the first layer of UV texture 20 is transferred, the ion source inside the coating machine will activate the texture surface before coating, so that active groups such as hydroxyl and carboxyl groups are generated on the UV texture surface, so that chemical bonding is generated between the UV texture layer and the coating layer, which is beneficial to improve the bonding force with the coating layer. At the same time, the ion source treatment will also increase the roughness of the texture surface, which can enhance the physical riveting effect with the coating layer, thereby enhancing the bonding force between the UV texture and the coating layer. In addition, the coating layer has a certain kinetic energy during deposition, which can also increase the bonding force between the UV texture and the coating layer; however, it is difficult to affect the stable and strong bonding force between the second UV texture layer 40 and the first coating layer 30. In order to improve the bonding strength between the second UV texture layer and the first coating layer, an intermediate layer can be formed between the first coating layer and the second UV texture layer. For example, an optical resin layer can be pre-formed on the first coating layer so that the resin layer forms excellent bonding strength with the first coating layer, and then the second UV texture layer is transferred to the surface of the optical resin layer. Although this solution can solve the problem of interlayer bonding strength well, it adds an extra intermediate layer, which not only increases the process cost, but also the silk-screening or spraying of the intermediate layer (such as the optical resin layer) will have an adverse effect on the yield. The inventor has found through a large number of experimental verifications that physical riveting and / or chemical bonding can be directly formed between the second UV texture layer 40 and the first coating layer 30. For example, a component that can react chemically with the first coating layer to produce chemical bonding can be directly added to the UV adhesive that forms the second UV texture layer to greatly enhance the bonding force between the second UV texture layer and the first coating layer. This solution can not only effectively solve the problem of poor bonding force between the first coating layer and the second UV texture layer, but also eliminate the need for an intermediate layer, thereby reducing the overall thickness of the composite film layer and the shell, while also simplifying the process and reducing costs. More importantly, when the composite film layer including the first UV texture layer, the first coating layer, and the second UV texture layer is transferred as a whole to the shell body by transfer printing, the overall thickness of the composite film layer is thinner due to the reduction in the use of the intermediate layer. When bonding a shell body with a larger angle, such as a glass substrate, the same bonding effect as a single-layer PET single-texture single-coated film sheet can be achieved, thereby avoiding the generation of bonding wrinkles and bubbles. Therefore, the electronic device shell described in the present application can not only significantly improve the bonding strength between the second UV texture layer and the first coating layer, solving the problem of poor bonding force of the UV glue transferred on the coating layer; it can also reduce the overall thickness of the composite film layer and the overall thickness of the electronic device shell on the basis of achieving a better appearance effect. When a double texture layer structure is formed on the same side of the shell body by transfer, the bonding effect between the composite film layer and the electronic device shell body can also be improved.

[0029] It is understood that the shell body described in the present application includes but is not limited to a glass shell, a ceramic shell, a metal shell and a plastic shell. In addition, it should be noted that the "composite film layer" described in the present application includes but is not limited to a first UV texture layer, a first coating layer, and a second UV texture layer arranged on the same side of the shell body, and may further include one or more of other coating layers, ink layers, PET films, and OCA adhesive layers, etc., arranged on the same side of the shell body.

[0030] According to some embodiments of the present application, the type of coupling agent in the second UV texture layer 40 is not particularly limited, and those skilled in the art can select it according to actual needs, as long as the coupling agent can react chemically with at least a portion of the first coating layer 30 to form a chemical bond connection. However, considering factors such as the bonding force between the coupling agent and the UV adhesive, the toughness and strength of the second UV texture layer 40, the coupling agent can be an organic coupling agent, and specifically can include at least one selected from phosphates, titanates, aluminates, and borates. At this time, the material of the first coating layer 30 in contact with the second UV texture layer 40 can include at least one selected from Al2O3, ZrO2, Ti3O5, and Nb2O5, so that the active groups of the coupling agent (such as phosphate groups, titanate groups, etc.) can react chemically with the first coating layer 30 to produce chemical bonds, and the other end of the coupling agent can undergo a polymerization reaction with the resin in the UV adhesive that forms the second UV texture layer 40. , thereby greatly improving the bonding strength between the first coating layer 30 and the second UV texture layer 40. Taking phosphate ester as an example, the mechanism of the coupling agent reacting with the material of the first coating layer 30 to improve the bonding strength includes: the structure of the phosphate ester compound contains various organic substituent groups and phosphate groups that can produce acid-base reactions with metal inorganic substrates. The organic groups can be alkyl, aliphatic and aromatic hydrocarbons, or organic segments with hydroxyl and carboxylic acid groups. Due to the high activity of phosphate groups, the chemical reaction between phosphate groups and the metal surface can produce slight corrosion on the surface of the metal substrate, thereby achieving the purpose of improving the bonding strength; among them, the mechanism of action of titanate, aluminate and borate is similar to that of phosphate ester. For another example, the coupling agent can be phosphate ester or titanate ester alone, or phosphate ester and titanate ester can be used simultaneously. Furthermore, the specific types of phosphates, titanates, aluminates and borates are not particularly limited, and those skilled in the art can flexibly select according to actual conditions. For example, the phosphate may include at least one selected from dipentaerythritol pentaacrylate phosphate, methacrylate oxydecyl dihydrogen phosphate, nonylphenol polyether phosphate, styrene polyether phosphate and fatty alcohol ether phosphate, and the titanate may include at least one selected from monoalkoxy titanate, chelate titanate and ligand titanate.

[0031] According to some further embodiments of the present application, the first coating layer 30 may include a plurality of stacked sub-coating layers, Figure 4 It is understood that the first coating layer 30 may include a sub-coating layer 31 in contact with the second UV texture layer 40, and a sub-coating layer not in contact with the second UV texture layer 40 (for example, it may include a low refractive index sub-coating layer 32 and a high refractive index sub-coating layer 33, etc.), wherein the material of the sub-coating layer 31 in contact with the second UV texture layer 40 may include at least one selected from Al2O3, ZrO2, Ti3O5 and Nb2O5. The inventors have found that the above materials can react chemically with phosphates, titanates, aluminates or borates to produce chemical bonds, and that the formation of the above materials only in the sub-coating layer 31 in direct contact with the second UV texture layer 40 can greatly improve the bonding force between the first coating layer 30 and the second UV texture layer 40, while not affecting the expected optical effect of the first coating layer 30. Furthermore, the material of the sub-coating layer 31 in contact with the second UV texture layer 40 may include only at least one selected from Al2O3, ZrO2, Ti3O5 and Nb2O5, without containing other materials, thereby further improving the bonding strength between the first coating layer 30 and the second UV texture layer 40; further, the sub-coating layer 31 in contact with the second UV texture layer 40 may be an Al2O3 layer. The inventors have found that Si and SiO2 will not chemically react with phosphates, titanates, aluminates and borates to form new chemical bonds, while compared with Ti3O5, the signal of the new chemical bond formed by the chemical reaction of Al2O3 with phosphates is stronger, and the effect of improving the bonding strength between the first coating layer 30 and the second UV texture layer 40 is more significant. It is understandable that the material of the sub-coating layer in the first coating layer 30 that is not in direct contact with the second UV texture layer 40 is not particularly limited, and those skilled in the art can flexibly select it according to actual conditions. For example, the material of each sub-coating layer in the first coating layer 30 that is not in direct contact with the second UV texture layer 40 can be independently selected from at least one of Al2O3, ZrO2, Ti3O5, Si and SiO2; for another example, referring to Figure 4 As shown, in the direction away from the shell body 10, multiple sub-coating layers in the first coating layer 30 that are not in direct contact with the second UV texture layer 40 can adopt a scheme of alternating stacking of low-refractive-index sub-coating layers 32 and high-refractive-index sub-coating layers 33. For example, SiO2 sub-coating layers and Ti3O5 sub-coating layers can be alternately stacked, and an Al2O3 sub-coating layer is prepared on the last Ti3O5 sub-coating layer to contact the second UV texture layer, which can further help to obtain better optical interference and appearance effects such as brightness, glare, and color.

[0032] According to some other embodiments of the present application, the thickness of the sub-coating layer 31 in the first coating layer 30 that is in direct contact with the second texture layer 40 may be no less than 10 nm, for example, may be 10 to 50 nm, specifically 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or 50 nm, etc. The inventors found that if the thickness of the sub-coating layer 31 that is in direct contact with the second texture layer 40 is too small, it is difficult to effectively improve the bonding force between the first coating layer 30 and the second UV texture layer 40. By controlling the thickness of the sub-coating layer 31 that is in direct contact with the second texture layer 40 to be no less than 10 nm, the second texture layer 40 and the first coating layer 30 can have a higher bonding force. According to the specific example of the present application, by controlling the thickness of the sub-coating layer to be no less than 10 nm, the adhesion of the texture layer in the final electronic device casing can reach 4B or above in the 100-grid test. Furthermore, taking into account factors such as cost and manufacturing efficiency, the thickness of the sub-plating layer 31 in the first plating layer 30 that is in direct contact with the second texture layer 40 can be set to 10-50 nm.

[0033] According to some other embodiments of the present application, in the UV glue forming the second UV texture layer 40, the mass content of the coupling agent can be 0.5-2wt%, for example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2wt%, etc. The inventors found that too much or too little content of the coupling agent in the UV glue forming the second UV texture layer 40 is not conducive to improving the bonding force between the second UV texture layer 40 and the coating layer. Taking phosphate ester as an example, when the content of phosphate ester in the UV glue forming the second UV texture layer 40 is too little, the chemical reaction occurring when the second UV texture layer 40 contacts the first coating layer 30 is limited, and it is difficult to form an effective chemical Chemical bonding; if the content of phosphate ester is too much, since the phosphate ester monomer and the UV glue forming the second UV texture layer 40 are not well soluble in each other, as the proportion of phosphate ester added increases, the reaction of phosphate ester with the first coating layer 30 (such as Al2O3 sub-coating layer) has reached a maximum value, and the remaining phosphate ester will be in a free state in the UV glue. The phosphate ester free on the surface of the UV glue cannot fully participate in the cross-linking reaction during UV curing due to the inhibition of oxygen. The remaining free phosphate ester monomer on the surface of the UV glue will affect the bonding force between the second UV texture layer 40 and the coating layer, among which the effect on the bonding force between the second coating layer 50 and the second UV texture layer 40 is more significant. In the present application, by controlling the mass content of the coupling agent in the UV glue forming the second UV texture layer 40 to be 0.5-2wt%, it is more conducive to significantly improving the bonding force between the second UV texture layer and the coating layer.

[0034] According to some other embodiments of the present application, the UV glue forming the second UV texture layer 40 may include a coupling agent, a photoinitiator and a resin monomer, wherein, in the UV glue, the mass content of the coupling agent may be 0.5-2wt%, and the mass content of the photoinitiator may be 1.5-5wt%. For example, the mass content of the photoinitiator may be specifically 1.5wt%, 1.8wt%, 2.1wt%, 2.4wt%, 2.7wt%, 3wt%, 3.3wt%, 3.6wt%, 3.9wt%, 4.2wt%, 4.5wt%, 4.8wt% or 5wt%, etc., thereby making the UV glue forming the second UV texture layer have good curing performance. In addition, it should be noted that, in the UV adhesive forming the second UV texture layer, the specific types of photoinitiators and resin monomers are not particularly limited, and those skilled in the art can flexibly choose according to actual conditions. For example, the photoinitiator may include photoinitiator 184 (i.e., 1-hydroxy-cyclohexyl-phenyl ketone) and / or photoinitiator TPO (2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide)), wherein photoinitiator 184 can be used in the surface curing system, and the effect is excellent when used in combination with photoinitiator TPO; and photoinitiator TPO has a wide wavelength absorption range, which is suitable for curing systems with thick film layers. For another example, the resin monomer can include both a low-functionality (functional group number is 1 to 3) resin monomer and a high-functionality (functional group number is not less than 4) resin monomer, wherein the low-functionality resin monomer can be used to increase the toughness of the second UV texture layer, and the high-functionality resin monomer can be used to increase the crosslinking density and increase the strength of the second UV texture layer; for another example, the resin monomer can include both difunctional polyurethane acrylate and hexafunctional polyurethane acrylate, or can further include nine-functional polyurethane acrylate, thereby making the second UV texture layer have both good strength and toughness. For another example, the UV glue forming the second UV texture layer can further include a resin monomer that can reduce the viscosity of the glue and the internal stress of the UV texture layer, such as isobornyl acrylate, and a resin monomer that can be copolymerized with the acrylate monomer to obtain an acrylic resin with active hydroxyl groups in the side chain, such as hydroxyethyl methacrylate (HEMA), thereby further improving the bonding force between the second UV texture layer and the first coating layer.

[0035] According to some other embodiments of the present application, reference Figure 5As shown, the electronic device housing 100 may further include a second coating layer 50 and an ink layer 60, wherein the second coating layer 50 is disposed on the side of the second UV texture layer 40 away from the housing body 10; the ink layer 60 is disposed on the side of the second coating layer 50 away from the housing body 10, thereby further improving the appearance effects of the electronic device housing such as brightness, glare, and color. It can be understood that the second coating layer 50 may also include a plurality of stacked sub-coating layers, and the material forming the second coating layer 50 may be the same as or different from the material forming the first coating layer 30; the stacking arrangement of the plurality of sub-coating layers in the second coating layer 50 may be the same as or different from that of the first coating layer 30. In addition, the thickness of the ink layer 60 is not particularly limited, and those skilled in the art can flexibly select according to actual needs. For example, the thickness of the ink layer can be 25 to 45 μm, and for example, it can be 25 μm, 30 μm, 35 μm, 40 μm or 45 μm, etc.; it can be understood that the ink layer 60 can be a single-layer setting or a multi-layer stacking setting, wherein the multi-layer stacking setting can achieve better shielding, decoration and light leakage prevention effects; in addition, there is no restriction on the color of the ink layer 60, and those skilled in the art can flexibly select according to actual conditions, for example, it can be white, black, gray or other colors, as long as it can prevent light leakage and does not affect the appearance color effect.

[0036] According to some other embodiments of the present application, the total thickness of the first coating layer 30 and the total thickness of the second coating layer 50 are not particularly limited, and those skilled in the art can flexibly select according to actual conditions. For example, the total thickness of the first coating layer 30 and the total thickness of the second coating layer 50 can be the same or different, and the total thickness of the two can be 50 to 1000 nm independently, for example, they can be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 850 nm, 900 nm or 950 nm, etc. Thus, the electronic device housing can have better appearance effects such as brightness, glare, and color under the premise of having a thin overall thickness.

[0037] According to some other embodiments of the present application, the texture of the first UV texture layer 20 and the texture of the second UV texture layer 40 may be the same or different. For example, the two may be independently selected from one or more of lens texture, bullet texture, S texture, etc. Those skilled in the art may flexibly select according to actual conditions to achieve the desired appearance effect; in addition, it can be understood that the thickness of the first UV texture layer 20 and the second UV texture layer 40 may be the same or different.

[0038] According to some other embodiments of the present application, in the electronic device housing 100, the type of the housing body 10 is not particularly limited, and those skilled in the art can flexibly select it according to the actual situation. For example, the material of the housing body 10 includes but is not limited to glass, ceramic, metal or plastic, etc.; for another example, the housing body 10 can be a transparent material, such as at least one selected from PET, PC, PMMA, PE and glass; for another example, taking plastic material as an example, the housing body 10 can be a single-layer structure formed by one of PET, PC, PMMA, PE and other materials or a composite layer single-layer structure formed by multiple composites, or a multi-layer stacked structure formed by one or more of PET, PC, PMMA and PE, etc. When the housing body is made of glass, ceramic or metal, it can also have a structure similar to the housing body of the above-mentioned plastic material. Based on the consideration of reducing the overall thickness of the electronic device housing, the housing body 10 can be selected as a single-layer structure. It can be understood that in the electronic device housing, the housing body 10 can be either a soft housing body or a hard housing body.

[0039] According to some other embodiments of the present application, in the electronic device housing 100, reference Figure 5 It is understood that the first UV texture layer 20 can be directly formed on one side of the shell body 10, and then the first coating layer 30 is formed on the surface of the first UV texture layer 20 away from the shell body 10, and the second UV texture layer 40 is transferred on the surface of the first coating layer 30 away from the shell body 10; or, refer to Figure 6It is understood that the first UV texture layer 20 can also be transferred to one side of the PET film 80 in advance with the help of the PET film 80, and then the first coating layer 30 is formed on the surface of the first UV texture layer 20 away from the PET film 80, and the second UV texture layer 40 is transferred on the surface of the first coating layer 30 away from the PET film 80, and finally the first UV texture layer 20, the first coating layer 30 and the second UV texture layer 40 are transferred as a whole to one side of the shell body 10 through the PET film 80, that is, the electronic device shell 100 can further include a PET film 80, and the PET film 80 can be arranged on the side of the first UV texture layer 20 close to the shell body 10; further, when the PET film is used to transfer each texture layer and the coating layer as a whole When transferring to the shell body, an optical adhesive layer 70 can be used to achieve the bonding of the PET film 80 and the shell body 10, that is, the electronic device shell 100 can also include an optical adhesive layer 70 (such as an OCA layer), and the optical adhesive layer 70 can be arranged on the side of the PET film 80 close to the shell body 10 and bonded to the shell body 10, wherein, before using the PET film to transfer the various texture layers and the coating layers as a whole to the shell body, the optical adhesive layer 70 can be pre-formed on the side of the PET film 80 close to the shell body 10, and the optical adhesive layer 70 can be covered by a release film. When the shell body 10 of the electronic device shell 100 is bonded to the PET film 80, the release film can be torn off and the bonding of the two can be achieved through the optical adhesive layer 70.

[0040] Based on the same inventive concept, in another aspect of the present application, the present application proposes a method for preparing an electronic device housing. Figure 7 As shown, the method includes:

[0041] 01: Provide the shell body

[0042] According to an embodiment of the present application, a shell body 10 is provided, wherein the material and structure of the shell body 10 have been described in detail above and will not be repeated here. Specifically, the shell body 10 can be a glass substrate, a ceramic substrate or a plastic substrate, wherein the preparation process of the shell body 10 is not particularly limited, and those skilled in the art can flexibly select according to actual conditions.

[0043] 02: Transfer the first UV texture layer on one side of the shell body

[0044] According to the embodiments of the present application, the UV adhesive used to form the first UV texture layer 20 can be directly transferred to the shell body 10 to form a texture pattern through a texture mold, or the UV adhesive used to form the first UV texture layer 20 can be transferred to the shell body 10 through a substrate such as a PET film, wherein the texture pattern, thickness and curing energy of the first UV texture layer 20 are not particularly limited, and those skilled in the art can flexibly select according to actual conditions. For example, the thickness of the first UV texture layer 20 can be 12±2μm, and the curing energy of the first UV texture layer 20 can be 1500mj / cm 2 In addition, before the UV adhesive is transferred to one side of the shell body 10 , the shell body 10 may be surface treated in advance to remove impurities on the surface of the shell body.

[0045] In addition, the composition of the UV adhesive (hereinafter referred to as the first UV adhesive) used to form the first UV texture layer 20 in the present application is not particularly limited, and those skilled in the art can flexibly select it according to actual conditions. For example, according to a specific example of the present application, the first UV adhesive may include: a resin monomer and a photoinitiator, wherein the resin monomer may include isobornyl acrylate, difunctional polyurethane acrylate, hexafunctional polyurethane acrylate and hydroxyethyl methacrylate, wherein the photoinitiator may include 1-hydroxy-cyclohexyl-phenyl ketone and / or 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide).

[0046] 03: Forming a first coating layer on the surface of the first UV texture layer away from the shell body

[0047] According to the embodiment of the present application, the first coating layer 30 can be made by magnetron sputtering or evaporation coating, etc. The total thickness of the first coating layer 30 formed on the surface of the first UV texture layer 20 can be 50 to 1000 nm, and the film structure can be specifically designed according to the requirements of color and brightness; in addition, the coating material of the first coating layer 30 is not particularly limited, and those skilled in the art can flexibly choose according to the actual situation, as long as the surface material of the first coating layer 30 away from the shell body 10 includes at least one selected from Al2O3, ZrO2, Ti3O5 and Nb2O5. Among them, the specific structure, material and thickness of the first coating layer 30 have been described in detail above, and will not be repeated here.

[0048] 04: The second UV texture layer is transferred on the surface of the first coating layer away from the shell body. The UV adhesive forming the second UV texture layer includes a coupling agent, and there is a chemical bond connection between the first coating layer and the coupling agent.

[0049] According to an embodiment of the present application, a UV adhesive for forming a second UV texture layer 40 (hereinafter referred to as the second UV adhesive) can be transferred to the first coating layer 30 through a texture mold to form a texture pattern, wherein the texture pattern, thickness and curing energy of the second UV texture layer 40 are not particularly limited, and those skilled in the art can flexibly select according to actual conditions. For example, the thickness of the second UV texture layer 40 can be 12±2μm, and the curing energy of the second UV texture layer 40 can be 1500mj / cm 2 . It should be emphasized that the second UV adhesive used to form the second UV texture layer 40 is doped with a coupling agent, and the coupling agent can react chemically with the first coating layer 30 to form a chemical bonding connection. Specifically, based on the total mass of the second UV adhesive, the amount of the coupling agent added can be 0.5-2wt%. According to a specific example of the present application, the basic composition of the second UV adhesive can be the same as that of the first UV adhesive, and the second UV adhesive can be obtained by simply adding a coupling agent to the first UV adhesive. Among them, the specific type and amount of the coupling agent, as well as the specific composition of the UV adhesive forming the second UV texture layer, have been described in detail above and will not be repeated here. According to a specific example of the present application, when the coupling agent includes a phosphate ester, the phosphate ester monomer can also include dipentaerythritol pentaacrylate phosphate (molecular formula is shown in formula (I)):

[0050]

[0051] According to the embodiments of the present application, reference Figure 8 As shown, the method for preparing an electronic device housing of the present application may also include:

[0052] 05: Form a second coating layer on the side of the second UV texture layer away from the shell body

[0053] According to an embodiment of the present application, the second coating layer 50 can be prepared by processes such as magnetron sputtering or evaporation coating. The total thickness of the second coating layer 50 formed on the surface of the second UV texture layer 40 can be 50 to 1000 nm, and the film layer structure can be specifically designed according to requirements such as color and brightness; in addition, the coating material of the second coating layer 50 is not particularly limited, and those skilled in the art can flexibly choose according to actual conditions. It should be noted that the surface material of the second coating layer 50 away from the shell body 10 is not particularly limited, and those skilled in the art can flexibly choose according to actual conditions. Among them, the specific structure, material and thickness of the second coating layer 50 have been described in detail above and will not be repeated here.

[0054] 06: An ink layer is formed on the side of the second coating layer away from the shell body

[0055] According to an embodiment of the present application, an ink layer 60 can be produced on the surface of the second coating layer 50 by silk screen printing or spraying, wherein the color of the ink layer 60 can be selected according to actual needs, and the thickness of the ink layer 60 can be 25 to 45 μm. The thickness, specific structure and color selection of the ink layer 60 have been described in detail above and will not be repeated here.

[0056] In addition, after screen printing or spraying the ink, the ink layer 60 can be further baked, wherein the baking temperature can be 60-90° C. and the baking time can be 30-90 min, thereby further improving the preparation efficiency and baking effect.

[0057] It is understandable that the first UV texture layer 20 can be directly transferred onto one side of the shell body 10, so that the shell body 10 and the first UV texture layer 20 are directly bonded and connected (refer to Figure 5 The shell body 10 can also be connected to the first UV texture layer 20 through the PET film 80 (reference Figure 6 Understanding), that is, the first UV texture layer 20 can be first transferred onto the PET film 80, and then the first coating layer 30 is formed on the surface of the first UV texture layer 20 away from the PET film 80, and the second UV texture layer 40 is transferred on the surface of the first coating layer 30 away from the PET film 80 (the second coating layer 50 can also be further formed on the side of the second UV texture layer 40 away from the PET film 80, and the ink layer 60 can be formed on the side of the second coating layer 50 away from the PET film 80), and finally, each texture layer and the coating layer are transferred as a whole to one side of the shell body 10 through the PET film 80, wherein, before the overall transfer of each texture layer and the coating layer is realized through the PET film, the composite film layer including the PET film, the texture layer and the coating layer can also be cut into small pieces by laser to obtain the film material size required for bonding with the shell body. Furthermore, an optical adhesive layer 70 (such as an OCA layer) and a release film covering the optical adhesive layer may be provided on the side of the PET film 80 away from the first UV texture layer 20. The release film may be retained before the PET film and the shell body are bonded together. When the overall transfer of each texture layer and the coating layer is achieved through the PET film, the release film may be torn off and the PET film and the shell body may be bonded together through the optical adhesive layer, thereby forming a double texture layer and coating structure on the same side of the electronic device shell body.

[0058] It can be understood that the method for preparing an electronic device housing in an embodiment of the present application and the electronic device housing described previously in the present application are proposed based on the same inventive concept, and all the features and advantages described for the electronic device housing described previously are also applicable to the method for preparing an electronic device housing, and will not be described one by one here.

[0059] In summary, the method for preparing the electronic device housing of the above embodiment of the present application and the electronic device housing described above have at least the following advantages: 1. The preparation process is simple and the cost is low; 2. The structure of the (prepared) electronic device housing is simple, the second UV texture layer and the first coating layer are in direct contact and the bonding strength between the two is good, and a double-layer texture double-coating structure can be formed on the same side of the housing body. On the premise of satisfying the good appearance of the electronic device housing, the use of at least one intermediate layer (such as PET film) can be reduced, and the overall thickness of the electronic device housing and the total thickness of the composite film layer formed on the same side of the housing body can be reduced, so that the composite film layer can achieve the same bonding effect as a single-layer housing body single-texture single-coating sheet when it is bonded to the electronic device housing body at a larger angle, avoiding the generation of bonding wrinkles and bubbles. 3. The appearance of the electronic device housing is good, which is more conducive to improving the overall beauty and value of the electronic device. 4. The inventive concept of improving the adhesion of the UV texture layer on the coating layer by chemical bonding can also be applied in other fields, solving industry bottlenecks and common problems.

[0060] In another aspect of the present application, the present application proposes an electronic device. The electronic device includes: the electronic device housing 100 described above, or an electronic device housing, a display screen assembly and a mainboard made by the method for preparing an electronic device housing described above, wherein the display screen assembly is connected to the electronic device housing, and an installation space is defined between the display screen assembly and the electronic device housing, wherein the housing body 10 in the electronic device housing is arranged away from the installation space; the mainboard is arranged in the installation space and is electrically connected to the display screen assembly. Thus, the electronic device has all the features and advantages of the electronic device housing described above and the method for preparing the electronic device housing described above, which will not be repeated here. In general, the electronic device has a better appearance effect and good appearance expression, which can further enhance the overall appearance effect of the electronic device and enhance its market competitiveness.

[0061] It is to be understood that the specific type of electronic device in the present application is not particularly limited, and those skilled in the art can flexibly select it according to the actual situation. For example, it can be a mobile phone, smart watch, PDA or laptop computer, etc. The above-mentioned electronic device can be any of various types of computer system devices that are mobile or portable and perform wireless communication. Specifically, the electronic device can be a mobile phone or smart phone, a portable game device, a laptop, a PDA, a portable Internet device, a music player and a data storage device, other handheld devices and devices such as watches, in-ear headphones, pendants, headphones, etc. The electronic device can also be other wearable devices (for example, head-mounted devices (HMD) such as electronic glasses, electronic clothes, electronic bracelets, electronic necklaces, electronic tattoos or smart watches). In some embodiments of the present application, with reference to Fig. 9As shown, the electronic device can be a mobile phone, wherein the electronic device housing 100 can be used as the back cover of the mobile phone. It can be understood that in addition to the electronic device housing described above, the electronic device also includes structures or components necessary for conventional electronic devices. Taking a mobile phone as an example, in addition to the electronic device housing, the mobile phone also includes a glass cover plate, a display panel, an audio processing module, a camera module, a touch screen and other structures or components necessary for conventional mobile phones.

[0062] It should be noted that in the description of the present application, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Specifically: the first UV texture layer and the second UV texture layer are only used to distinguish the two texture layers, and cannot be understood as a limitation on their importance or materials or structures. Similarly, the first coating layer and the second coating layer are only used to distinguish the two coating layers. In addition, in the present application, unless otherwise clearly specified and limited, the terms "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral whole; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of the two elements or the interaction relationship between the two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.

[0063] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0064] The general method for preparing the electronic device housing in the following examples and comparative examples:

[0065] 1.1. Provide the shell body and PET substrate. The PET substrate is the original PET film. The size of the original PET film (including the release film 125μm, the OCA layer 25μm, and the PET layer 50μm) is 300×400mm. The release film is retained during the film processing until it is torn off when it is attached to the shell body.

[0066] 1.2. Transfer the first UV adhesive to one side of the PET substrate to form the first UV texture layer. Through the texture mold, transfer the first UV adhesive to the PET substrate to form a texture pattern. The thickness of the first UV texture layer is 12±2μm, and the curing energy of the first UV texture layer is 1500mj / cm 2The composition of the first UV adhesive is shown in Table 1.

[0067] 1.3. Form a first coating layer on the surface of the first UV texture layer away from the PET substrate. The first coating layer is made on the surface of the first UV texture layer by magnetron sputtering or evaporation coating. The total thickness of the first coating layer is 50 to 1000 nm (the film structure is designed according to the color and brightness requirements). The coating material is selected according to the needs, such as SiO2, Ti3O5, Nb2O5, etc., wherein the ending layer material of the first coating layer is selected from Al2O3, ZrO2, Ti3O5 and Nb2O5, and the thickness is preferably 30 nm. The stacked structure of the first coating layer is as follows: Fig.10 As shown:

[0068] 1.4. Transfer the second UV adhesive to the surface of the first coating layer away from the PET substrate to form a second UV texture layer. Through the texture mold, transfer the second UV adhesive to the first coating layer to form a texture pattern. The thickness of the second UV texture layer is 12±2μm, and the curing energy of the second UV texture layer is 1500mj / cm 2 The second UV adhesive is based on the composition and total weight of the first UV adhesive, and phosphate is added, and the amount of phosphate added is 0.5-2wt%.

[0069] 1.5. Form a second coating layer on the side of the second UV texture layer away from the PET substrate. The second coating layer is made on the surface of the second UV texture layer by magnetron sputtering or evaporation coating. The total thickness of the second coating layer is 50 to 1000 nm (the film structure is designed according to the color and brightness requirements), and the coating material is selected according to the needs.

[0070] 1.6. Form an ink layer on the side of the second coating layer away from the PET substrate. The ink layer is made on the surface of the second coating layer by screen printing or spraying. The color of the ink layer is selected according to needs, and the thickness of the ink layer is 25 to 45 μm.

[0071] 1.7. Baking: The ink is baked after screen printing, the baking temperature is 60-90℃, and the time is 30-90min.

[0072] 1.8 Cutting: Use laser to cut the composite diaphragm into small pieces to obtain the diaphragm size required to fit the shell body.

[0073] 1.9. Lamination. Tear off the release film on the PET substrate in the composite film, so that the OCA layer of the PET film raw material is laminated with the shell body, and the overall transfer of each texture layer and coating layer is achieved.

[0074] Table 1 Composition of the first UV adhesive

[0075]

[0076]

[0077] Example 1

[0078] The first coating layer includes, in the direction away from the PET substrate (i.e., in the direction away from the shell body), the following layers stacked in sequence: a 20nm thick SiO2 layer, a 60nm thick Ti3O5 layer, a 90nm thick SiO2 layer, a 60nm thick Ti3O5 layer, an 80nm thick SiO2 layer, a 50nm thick Ti3O5 layer, and a 50nm thick sub-coating layer Al2O3 layer in direct contact with the second UV texture layer.

[0079] The thickness of the second UV texture layer was 12 μm.

[0080] The mass content of the phosphate ester in the second UV glue is 0.5wt%.

[0081] Example 2

[0082] The difference from Example 1 is that the 50 nm thick sub-plating layer directly in contact with the second UV texture layer is a Ti3O5 layer.

[0083] Comparative Example 1

[0084] The difference from Example 1 is that the 50 nm thick sub-plating layer directly in contact with the second UV texture layer is a SiO2 layer.

[0085] Comparative Example 2

[0086] The difference from Example 1 is that the 50 nm thick sub-plating layer directly in contact with the second UV texture layer is a Si layer.

[0087] Comparative Example 3

[0088] The difference from Example 1 is that the 50 nm thick sub-plating layer directly in contact with the second UV texture layer is a SiAl layer.

[0089] The electronic device housings prepared in Examples 1 to 2 and Comparative Examples 1 to 3 were evaluated:

[0090] 1) The adhesion of the second UV texture layer on the first coating layer in Examples 1 to 2 and Comparative Examples 1 to 3 was tested under the same conditions. The test results are shown in Table 2.

[0091] Test method: Adhesion test (100 grids) was conducted according to the international standard ISO 2409.

[0092] 2) XPS (X-ray photoelectron spectroscopy) was used to characterize the contact interface between the first coating layer and the second UV texture layer in Examples 1 to 2 and Examples 1 to 2. The XPS spectra are shown in Figures 11 to 14 As shown (where Figures 11 to 14In the figure, the horizontal axis is the binding energy (unit: eV), and the vertical axis is the counting rate of photoelectrons).

[0093] Table 2 Effect of material changes of the sub-coating layer in contact with the second UV texture layer on the bonding strength between the second UV texture layer and the first coating layer

[0094]

[0095] Results and Conclusions:

[0096] From the test results in Table 2, we can see that the material type of the sub-coating layer in direct contact with the second UV texture layer in the first coating layer has a significant impact on the bonding strength between the two. Compared with the more common coating materials currently, Al2O3 is the best, followed by Ti3O5, and the bonding strength of SiO2 and SiAl is very poor. Figures 11 to 14 XPS characterization shows that new chemical bonds are formed at the interface of Al2O3, Ti3O5 and the second UV texture layer. The XPS signal position shows that the P element reacts with the oxide to produce new chemical bonds, while no new chemical bonds are produced on the Si and SiO2 surfaces. In addition, the new chemical bond signal formed by Al2O3 (i.e., the binding energy of the Al-P bond) is stronger than the new chemical bond signal formed by Ti3O5, which further verifies that under the same conditions, the bonding force between the sub-coating Al2O3 layer and the second UV texture layer is better. It should be noted that Figures 11 to 14 The position of the arrow in the figure is only to distinguish different curves and does not represent the binding energy of the new chemical bond formed by the metal oxide and the phosphate; in addition, the etching distance in the figure refers to the etching depth of the contact interface between the first coating layer and the second UV texture layer.

[0097] Example 3

[0098] The difference from Example 1 is:

[0099] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0100] Example 4

[0101] The difference from Example 1 is:

[0102] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 10 nm;

[0103] The adhesion of the second UV texture layer on the first coating layer in Example 1 and Examples 3-4 was evaluated. The test results are shown in Table 3.

[0104] Table 3 Effect of thickness change of the sub-coating layer in direct contact with the second UV texture layer on the bonding strength between the second UV texture layer and the first coating layer

[0105]

[0106] Results and Conclusions:

[0107] Combined with Table 3, it can be seen that when the thickness of the Al2O3 layer in direct contact with the second UV texture layer is not less than 10nm, its thickness change has no significant effect on the bonding force between the second UV texture layer and the first coating layer. Considering the fluctuations in the coating process and equipment, the Al2O3 thickness can be set to 30nm.

[0108] Comparative Example 4

[0109] The difference from Example 1 is:

[0110] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0111] The mass content of the phosphate ester in the second UV glue is 0wt%.

[0112] Comparative Example 5

[0113] The difference from Example 1 is:

[0114] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0115] The mass content of the phosphate ester in the second UV glue is 2.5wt%.

[0116] Example 5

[0117] The difference from Example 1 is:

[0118] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0119] The mass content of the phosphate ester in the second UV glue is 1wt%.

[0120] Example 6

[0121] The difference from Example 1 is:

[0122] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0123] The mass content of the phosphate ester in the second UV glue is 1.5wt%.

[0124] Example 7

[0125] The difference from Example 1 is:

[0126] The thickness of the sub-coating Al2O3 layer directly in contact with the second UV texture layer is 30nm;

[0127] The mass content of the phosphate ester in the second UV glue is 2wt%.

[0128] The electronic device housings prepared in Examples 3, 5 to 7 and Comparative Examples 4 to 5 were evaluated:

[0129] 1) The adhesion between the second UV texture layer and the coating layer in Examples 3, 5 to 7 and Comparative Examples 4 to 5 was tested. The test results are shown in Table 4.

[0130] 2) Energy spectrum analysis was performed on the contact interface between the neutron coating Al2O3 layer and the second UV texture layer in Comparative Example 4 and Example 5 using a transmission electron microscope to evaluate the P element content on the surface of the Al2O3 layer. The test results are shown in Fig.15 shown.

[0131] Table 4 Effect of phosphate content on the bonding strength between the second UV texture layer and the coating layer

[0132]

[0133]

[0134] Results and Conclusions:

[0135] Combination Fig.15 As shown, the second UV texture layer does not contain phosphate. Through transmission electron microscopy characterization, it can be seen that in comparative example 4, no P element enrichment is detected on the surface of the sub-coating layer Al2O3 close to the texture layer, and only a small amount of P element is dispersed in the second UV texture layer. This is due to the formation of the photoinitiator TPO (i.e., 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide) of the second UV texture layer. In Example 5, P element is detected on the surface of Al2O3 close to the texture layer, and P element is obviously enriched at the interface between the first coating layer and the second texture layer. It can be seen from the high-magnification electron microscope image that phosphate penetrates into the shallow surface of Al2O3, which indicates that Al2O3 and phosphate react chemically.

[0136] Combined with Table 4, it can be seen that when no phosphate is added to the second UV adhesive, the bonding strength between the second UV texture layer and the first coating layer is extremely poor, and the dry grid adhesion grade is 0B; based on the total mass of the second UV adhesive, when the addition amount of phosphate varies in the range of 0.5 to 2wt%, there is no obvious difference in the bonding strength between the second UV texture layer and the first coating layer. However, based on the total mass of the second UV adhesive, when the addition amount of phosphate ester is 2.5wt%, the bonding strength between the second UV texture layer and the second coating layer decreases. This is because the phosphate ester monomer and the second UV adhesive are not well soluble in each other. As the addition ratio of phosphate ester increases, the reaction between phosphate ester and Al2O3 has reached a maximum value, and the remaining phosphate ester will be in a free state in the second UV adhesive. The free phosphate ester on the surface of the second UV adhesive cannot fully participate in the cross-linking reaction during UV curing due to the inhibition of oxygen. The remaining free phosphate ester monomer on the surface of the second UV adhesive will affect the bonding strength between the second UV texture layer and the second coating layer. Therefore, the addition amount of phosphate ester in the second UV adhesive should be controlled in the range of 0.5-2wt%.

[0137] In the description of this application, the description with reference to the terms "some embodiments", "examples", "specific examples", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradicting each other.

[0138] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. An electronic device housing, characterized in that: include: Shell body; A first UV texture layer, wherein the first UV texture layer is disposed on one side of the shell body; A first coating layer, wherein the first coating layer is disposed on a surface of the first UV texture layer away from the housing body; a second UV texture layer, the second UV texture layer being arranged on a surface of the first coating layer away from the housing body, Wherein, the second UV texture layer includes a coupling agent, and the first coating layer and the coupling agent are chemically bonded. The first coating layer includes a plurality of stacked sub-coating layers, wherein the material of the sub-coating layer in contact with the second UV texture layer includes at least one selected from the group consisting of Al2O3, ZrO2, Ti3O5 and Nb2O5.

2. The electronic device housing according to claim 1, characterized in that: The coupling agent includes at least one selected from phosphate, titanate, aluminate and borate.

3. The electronic device housing according to claim 2, characterized in that: The phosphate ester includes at least one selected from dipentaerythritol pentaacrylate phosphate, methacrylate oxydecyl dihydrogen phosphate, nonylphenol polyether phosphate, styrene polyether phosphate and fatty alcohol ether phosphate; The titanate includes at least one selected from the group consisting of monoalkoxy type titanate, chelate type titanate and ligand type titanate.

4. The electronic device housing according to claim 1, characterized in that: The thickness of the sub-coating layer in the first coating layer that is in direct contact with the second UV texture layer is not less than 10 nm.

5. The electronic device housing according to claim 1, characterized in that: The thickness of the sub-coating layer in the first coating layer that is in direct contact with the second UV texture layer is 10-50 nm.

6. The electronic device housing according to any one of claims 1 to 5, characterized in that: In the UV adhesive forming the second UV texture layer, the content of the coupling agent is 0.5-2 wt %.

7. The electronic device housing according to claim 6, characterized in that: The UV glue for forming the second UV texture layer comprises the coupling agent, a photoinitiator and a resin monomer, and the content of the photoinitiator in the UV glue is 1.5-5wt%.

8. The electronic device housing according to claim 1 or 7, characterized in that: Also includes: A second coating layer, wherein the second coating layer is arranged on a side of the second UV texture layer away from the housing body; An ink layer is arranged on a side of the second coating layer away from the shell body.

9. A method for preparing an electronic device housing according to any one of claims 1 to 8, characterized in that: include: Providing a housing body; Transferring a first UV texture layer on one side of the shell body; forming a first coating layer on a surface of the first UV texture layer away from the housing body; A second UV texture layer is transferred onto a surface of the first coating layer away from the shell body, and a UV adhesive for forming the second UV texture layer includes a coupling agent, and a chemical bond is formed between the first coating layer and the coupling agent.

10. The method according to claim 9, characterized in that Also includes: forming a second coating layer on a side of the second UV texture layer away from the housing body; An ink layer is formed on a side of the second coating layer away from the housing body.

11. An electronic device, characterized in that: include: An electronic device housing according to any one of claims 1 to 8, or an electronic device housing made by the method according to any one of claims 9 to 10; A display screen assembly, wherein the display screen assembly is connected to the electronic device housing, and an installation space is defined between the display screen assembly and the electronic device housing, wherein the housing body in the electronic device housing is arranged away from the installation space; as well as A mainboard is disposed in the installation space and is electrically connected to the display screen assembly.