Molded polyurethane hydrogel
By forming polyurethane hydrogel in organic polar solvents, the problems of allergic reactions, oil-based sensitivity and insufficient elasticity of existing condom materials are solved, and a high elasticity and durability polyurethane hydrogel condom is achieved, reducing the The risk of disease transmission.
Patent Information
- Application Number
- CN202080046224.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-06-27
AI Technical Summary
Existing condom materials such as latex and polyurethanes have allergic reactions, oil-based lubricant sensitivity, high friction coefficient, insufficient elasticity, easy slippage or rupture, resulting in inconvenience in use and increased risk of disease transmission.
A polyurethane solution with a molecular weight between 40,000 and 500,000 is formed in an organic polar solvent containing less than 40% water, applied to the mold and dried to form a polyurethane film, and then contacted with a swelling agent to form a polyurethane hydrogel for manufacturing with improved Elastic and durable condoms.
It achieves high elasticity, durability and hypoallergenicity of polyurethane hydrogels, reduces the risk of disease transmission, and improves the use experience and protective effect of condoms.
Smart Images

Figure GDA0004364191440000211 
Figure GDA0004364191440000231 
Figure GDA0004364191440000241
Abstract
Description
Technical Field
[0001] The present technology relates to polyether-based polyurethane hydrogel and polyester-based polyurethane hydrogel and their use in condoms.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims priority from Australian Provisional Patent Application No. 2019902307, which is incorporated in its entirety by cross-reference. Background Art
[0004] Condoms are often thought of as a contraceptive, but they also serve an important health function by acting as a physical barrier to reduce or prevent sexually transmitted diseases such as herpes, chlamydia, syphilis, gonorrhea, hepatitis, human papillomavirus (HPV), trichomoniasis, and acquired immunodeficiency syndrome (AIDS) caused by the human immunodeficiency virus (HIV).
[0005] Although condoms also use other materials, such as nitrile, nitrile rubber, polyurethane, AT-10 resin (polyethylene resin) and polyisoprene, they are usually made of latex. The disadvantages of latex condoms and gloves are the inherent allergic reactions to the material and the sensitivity of latex rubber to oil-based lubricants, which lead to possible damage and disease transmission. In addition, like other commonly used materials, latex has a high coefficient of friction, which can lead to reported sensory loss during use. This causes a reduction in the use of condoms and increases the possibility of disease transmission. Polyurethane has some advantages over latex in that it can be used with oil-based lubricants, is less allergic than latex, and has no odor. However, polyurethane condoms are not as elastic as latex and are more likely to slip or break, deform or wrinkle.
[0006] Protective gloves are usually made of latex rubber, nitrile or nitrile rubber (a synthetic copolymer of acrylonitrile and butadiene), polyvinyl alcohol and neoprene. These materials provide different protection against materials such as organic solvents, inorganic compounds and other hazardous materials, but provide limited thermal and physical protection.
[0007] The present inventors have developed a method for producing molded polyurethane hydrogels that are substantially impermeable to biologics and have sufficient strength and durability to be used in the manufacture of barrier devices such as condoms and gloves. Summary of the invention
[0008] In a first aspect, there is provided a method for producing a molded polyurethane hydrogel, the method comprising:
[0009] forming a first solution of at least one polyurethane having a molecular weight between about 40,000 and about 500,000 in an organic polar solvent containing less than about 40% (v / v) water and water;
[0010] applying a layer of the first solution to a mold;
[0011] drying the layer of the first solution to form a polyurethane film on the mold; and
[0012] The polyurethane film is contacted with the swelling agent under conditions where the film forms a polyurethane hydrogel having a swelling agent content between about 1% and about 95%.
[0013] In one embodiment, the molecular weight of the polyurethane is about 40,000 to about 50,000, or 50,000 to about 75,000, or 75,000 to about 100,000, or 100,000 to about 125,000, about 125,000 to about 150,000, about 150,000 to about 175,000, about 175,000 to about 200,000, about 200,000 to about 225,000, about 225,000 to about 250,000, about From about 250,000 to about 275,000, from about 275,000 to about 300,000, from about 300,000 to about 325,000, from about 325,000 to about 350,000, from about 350,000 to about 375,000, from about 375,000 to about 400,000, from about 400,000 to about 425,000, from about 425,000 to about 450,000, from about 450,000 to about 475,000, or from about 475,000 to about 500,000.
[0014] In a preferred embodiment, the polyurethane has a molecular weight of about 150,000 to about 350,000.
[0015] In one embodiment, the polyurethane is derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate.
[0016] In one embodiment, the polyurethane is a polyether-based polyurethane or a polyester-based polyurethane.
[0017] In one embodiment, the polyether-based polyurethane is derived from the polymerization of 4,4′-dicyclohexylmethane diisocyanate and a polyether.
[0018] In one embodiment, the polyether comprises 1 to 35 ether groups.
[0019] In one embodiment, the polyester-based polyurethane is derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate and polyester.
[0020] In one embodiment, the polyester comprises from 1 to 35 ethyl ester groups.
[0021] In one embodiment, the polyurethane may have methyl and / or hydroxyl end groups.
[0022] In one embodiment, the organic polar solvent is selected from the group consisting of ethanol, methanol, isopropanol, butanol, tetrahydrofuran, dimethylformamide, dimethyl sulfoxide, acetone, acetonitrile and any combination thereof.
[0023] In one embodiment, the organic polar solvent is ethanol.
[0024] In one embodiment, the ratio of water to the organic polar solvent is selected from about 5:95, about 10:90, about 15:85, about 20:80, about 25:75, about 30:70, about 35:65, or about 40:60.
[0025] In one embodiment, the ratio of water to organic polar solvent is about 10:90.
[0026] In one embodiment, the swelling agent is selected from at least one of water, ethylene glycol solution, hydroxyethyl cellulose solution, paraben-based solution, ethylene glycol-based solution, glycerin-based solution, oil-based solution or silicone-based solution.
[0027] In one embodiment, the swelling agent comprises one or more of a spermicide, a lubricant, an antiviral agent, an antifungal agent, an antibacterial agent, a prebiotic, a probiotic, a microbiome enhancer, a flavor compound, an aroma compound, a sensory enhancer, a sterilant, or a disinfectant.
[0028] In one embodiment, the polyurethane film is in contact with the swelling agent for about 1 second to about 30 seconds. In some embodiments, the polyurethane film is in contact with the swelling agent for up to 24 hours, such as about 15 minutes, about 30 minutes, about 45 minutes, about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, or about 24 hours.
[0029] In one embodiment, the temperature of the swelling solution is about 20° C. to about 90° C. For example, the temperature may be about 20° C., about 25° C., about 30° C., about 35° C., about 40° C., about 45° C., about 50° C., about 55° C., about 60° C., about 65° C., about 70° C., about 75° C., about 80° C., about 85° C., or about 90° C.
[0030] In one embodiment, the method further comprises:
[0031] In an organic polar solvent containing less than about 40% (v / v) water and water, a molecular weight of about 40,000 to about 50,000, or 50,000 to about 75,000, or 75,000 to about 100,000, or 100,000 to about 125,000, about 125,000 to about 150,000, about 150,000 to about 175,000, about 175,000 to about 200,000, about 200,000 to about 225,000, about 225,000 to about 250,000, a second solution of a polyurethane of between about 250,000 and about 275,000, about 275,000 and about 300,000, about 300,000 and about 325,000, about 325,000 and about 350,000, about 350,000 and about 375,000, about 375,000 and about 400,000, about 400,000 and about 425,000, about 425,000 and about 450,000, about 450,000 and about 475,000, or about 500,000;
[0032] applying a layer of the second solution to the polyurethane film on the mold;
[0033] drying the layers of the second solution, wherein the layers form a polyurethane film on the mold; and
[0034] The polyurethane film is contacted with the swelling agent under conditions where the film forms a polyurethane hydrogel having a swelling agent content between about 1% and about 95%.
[0035] In one embodiment, the polyurethane comprises -CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2, where
[0036] n is an average independently selected from any number between 1 and 35; and
[0037] m is an average value independently selected from any number between 15-500.
[0038] In some embodiments, the relationship between n and m may be a proportional relationship.
[0039] In some embodiments, the ratio of n to m may be from about 1:0.1 to about 1:75.
[0040] In some embodiments, the at least one polyurethane in the second solution is different from the at least one polyurethane in the first solution.
[0041] In one embodiment, the method further comprises applying subsequent layers of the first solution or the second solution to the polyurethane film on the mold to increase thickness or impart specific properties to the polyurethane film.
[0042] In one embodiment, the method further comprises applying a subsequent layer of the first solution or the second solution to the portion of the polyurethane film on the mold to increase thickness or create specific features on the portion of the polyurethane film.
[0043] The particular features formed from the subsequent layer may have a different modulus, tensile strength, and / or linear expansion range than the hydrogel formed by the layer to which the subsequent layer is applied.
[0044] In one embodiment, either or both of the molecular weight and n:m of the at least one polyurethane in the first solution is different from the molecular weight and / or n:m of the at least one polyurethane in the second solution.
[0045] In one embodiment, additional subsequent layers are applied to increase the thickness to a predetermined value.
[0046] In one embodiment, the molded polyurethane hydrogel has a linear expansion range of about 1% to about 100%.
[0047] In one embodiment, the molded polyurethane hydrogel has a tensile strength of about 1 MPa to about 100 MPa, about 1 MPa to about 20 MPa, about 20 MPa to about 40 MPa, about 20 MPa to about 60 MPa, about 40 MPa to about 60 MPa, about 60 MPa to about 80 MPa, about 80 MPa to about 100 MPa.
[0048] In preferred embodiments, the molded polyurethane hydrogel has a tensile strength of about 20 MPa to 40 MPa, for example, 20 MPa, 22 MPa, 24 MPa, 26 MPa, 28 MPa, 30 MPa, 32 MPa, 34 MPa, 36 MPa, 38 MPa, or about 40 MPa.
[0049] In one embodiment, the molded polyurethane hydrogel has an elongation at break ranging from about 200% to about 2000%.
[0050] In one embodiment, the molded polyurethane hydrogel has a shear modulus of at least one of about 50% modulus of about 80 kPa to about 15 MPa, about 100% modulus of about 200 kPa to about 15 MPa, and about 300% modulus of about 700 kPa to about 15 MPa.
[0051] In a second aspect, there is provided a molded polyurethane hydrogel condom produced by the first aspect.
[0052] In a third aspect, a molded polyurethane hydrogel condom is provided, wherein the polyurethane hydrogel comprises one or more polyurethanes having a molecular weight between about 40,000 and about 500,000 and a swelling agent in an amount between about 1% and about 95%, preferably between about 40% and about 70%.
[0053] In one embodiment, the molecular weight of the polyurethane is from about 40,000 to about 50,000, or from 50,000 to about 75,000, or from 75,000 to about 100,000, or from 100,000 to about 125,000, from about 125,000 to about 150,000, from about 150,000 to about 175,000, from about 175,000 to about 200,000, from about 200,000 to about 225,000, from about 225,000 to about 250,000, or from about From about 250,000 to about 275,000, from about 275,000 to about 300,000, from about 300,000 to about 325,000, from about 325,000 to about 350,000, from about 350,000 to about 375,000, from about 375,000 to about 400,000, from about 400,000 to about 425,000, from about 425,000 to about 450,000, from about 450,000 to about 475,000, or from about 475,000 to about 500,000.
[0054] In one embodiment, the polyurethane is derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate.
[0055] In one embodiment, the polyurethane is a polyether-based polyurethane or a polyester-based polyurethane.
[0056] In one embodiment, the polyether-based polyurethane is derived from the polymerization of 4,4′-dicyclohexylmethane diisocyanate and a polyether.
[0057] In one embodiment, the polyether comprises 1 to 35 ether groups.
[0058] In one embodiment, the polyester-based polyurethane is derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate and polyester.
[0059] In one embodiment, the polyester comprises from 1 to 35 ethyl ester groups.
[0060] In one embodiment, the molded polyurethane hydrogel condom has a linear expansion range of about 1% to about 100%, a tensile strength of about 1 MPa to about 100 MPa, and an elongation at break range of about 200% to about 2000%. Preferably, the condom has a linear expansion range of about 1% to about 100%, a tensile strength of about 1 MPa to about 40 MPa, and an elongation at break range of about 200% to about 750%; and at least one of a 50% modulus of about 80 kPa to about 15 MPa, a 100% modulus of about 200 kPa to about 15 MPa, and a 300% modulus of about 700 kPa to about 15 MPa.
[0061] In one embodiment, the condom is substantially impermeable to biological agents having an average diameter of 30 nm or greater.
[0062] In one embodiment, the condom is substantially impermeable to biological agents having an average diameter of 30 nm or greater at a simulated use pressure of up to 10 kPa applied to the condom, for example, the use pressure may be up to about 1 kPa, up to about 2 kPa, up to about 3 kPa, up to about 4 kPa, up to about 5 kPa, up to about 6 kPa, up to about 7 kPa, up to about 8 kPa, up to about 9 kPa, or up to about 10 kPa.
[0063] In one embodiment, the condom has a burst volume of about 5L to about 50L.
[0064] In one embodiment, the condom has a burst pressure of about 0.75 kPa to about 5 kPa, about 1 kPa to about 5 kPa, such as 1.3 kPa to about 3.6 kPa, preferably 1.6 kPa to 3.6 kPa.
[0065] definition
[0066] In this application document, unless the context clearly requires otherwise, the word "comprise" or variations such as "comprises" or "comprising" will be understood to mean including the stated elements, integers or steps, or groups of elements, integers or steps, but not excluding any other elements, integers or steps, or groups of elements, integers or steps.
[0067] In this application document, the term "consisting of" means consisting of only.
[0068] Any discussion of documents, acts, materials, appliances, articles and the like included in this application is for the purpose of providing context for the technology. It is not to be taken as an admission that any or all of these matters form part of the prior art base or are common general knowledge in the field relevant to the technology as they existed before the priority date of each claim of this application.
[0069] Unless the context requires otherwise or specifically stated, an integer, step or element described herein as a singular integer, step or element expressly encompasses both the singular and the plural form of the integer, step or element.
[0070] In the context of this application document, the terms "a" and "an" are used to refer to the grammatical object of one or more (ie, at least one) items. For example, with respect to "an element", it means one element or a plurality of elements.
[0071] In the context of this application document, the term "about" refers to numbers or values, which should not be regarded as absolute numbers or values, but include the range of variation above or below the numbers or values understood by those skilled in the art, including the range of variation within the typical error range or instrument limitations. In other words, the use of the term "about" is understood to refer to the range or approximation that a person skilled in the art or skilled in the art considers to be equivalent to the numerical value in the context of achieving the same function or result.
[0072] Those skilled in the art will recognize that the technology described herein is susceptible to changes and modifications other than those specifically described. It should be understood that the technology includes all such changes and modifications. For the avoidance of doubt, the technology also includes all steps, features and compounds mentioned or referred to in the application documents, either individually or collectively, and any combination and all combinations of any two or more of the steps, features and compounds.
[0073] In order to more clearly understand the present technology, preferred embodiments will be described with reference to the following drawings and examples. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 is an example of a load-elongation curve for a hydrogel produced using a polymer comprising polymer A. The condom has a double wall thickness of 0.125 mm and a width of 58 mm. The width of the sample ring is 20 mm.
[0075] Figure 2 is an example of a load-elongation curve for a hydrogel produced using a polymer comprising polymer B. The condom has a double wall thickness of 0.148 mm and a width of 53 mm. The width of the sample ring is 20 mm.
[0076] Description of Embodiments
[0077] The present invention is based on methods for producing molded polyurethane hydrogels (polyether-based or polyester-based). The hydrogels prepared by these methods have many properties, such as linear expansion, tensile strength, elongation at break, modulus, and impermeability to biological agents, which alone or in combination make them suitable for use in barrier devices such as condoms and gloves.
[0078] The methods disclosed herein require forming a solution of polyurethane in water and an organic polar solvent. A layer of the solution is then applied to a mold, for example, by dipping the mold into the solution. Once the layer is applied, it is dried and forms a polyurethane film on the mold. Additional layers of the polyurethane solution or a different solution (e.g., using a different polyurethane) may then be applied. Once these layers are dried, the film may be contacted with a swelling agent (e.g., an aqueous solution that may contain a buffer, a salt, and / or a preservative). The swelling agent infiltrates the film to form a polyurethane hydrogel, which typically has a swelling agent content of between about 1% and about 95%, but for water-based swelling agents, the content is typically around 30-90%. For oil-based or silicone-based swelling agents, the hydrogel typically has a swelling agent content of between about 0.1% and about 30%, for example, between about 0.1% and about 10%, after contact with the swelling agent for 24 hours.
[0079] Polyurethane
[0080] As used herein, the term "polyurethane" refers to a polymer obtained by the reaction of an isocyanate and an alcohol, wherein the isocyanate contains two or more isocyanate functional groups.
[0081] A variety of polyurethanes are useful in the methods described herein. Suitable polyurethanes include those derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate, the polymerization of 4,4'-dicyclohexylmethane diisocyanate and a polyether, the polymerization of 4,4'-dicyclohexylmethane diisocyanate and a polyester, or any combination thereof.
[0082] In one embodiment, the polyurethane is a hydrophilic polyurethane block copolymer, such as a hydrophilic polyurethane block copolymer comprising 4,4′-dicyclohexylmethane diisocyanate. The hydrophilic polyurethane block copolymer may comprise repeating ether groups, such as at least 1 to 50 repeating ether groups.
[0083] In another embodiment, the hydrophilic polyurethane block copolymer is a polyether-based polyurethane. For example, the hydrophilic polyurethane block copolymer comprises 4,4′-dicyclohexylmethane diisocyanate and ethyl ether. The hydrophilic polyurethane block copolymer may comprise 4,4′-dicyclohexylmethane diisocyanate and repeating ethyl ether groups, such as at least four repeating ethyl ether groups. In another embodiment, the hydrophilic polyurethane block copolymer comprises 4,4′-dicyclohexylmethane diisocyanate and 1 to 35 repeating ethyl ether groups.
[0084] The hydrophilic polyurethane block copolymer may include repeating ethyl ester groups, for example, the hydrophilic polyurethane block copolymer may include at least 1 to 35 repeating ethyl ester groups.
[0085] In another embodiment, the hydrophilic polyurethane block copolymer is a polyester-based polyurethane. For example, the hydrophilic polyurethane block copolymer comprises 4,4′-dicyclohexylmethane diisocyanate and ethyl ester. The hydrophilic polyurethane block copolymer may comprise 4,4′-dicyclohexylmethane diisocyanate and repeating ethyl ester groups, such as at least four repeating ethyl ester groups. In another embodiment, the hydrophilic polyurethane block copolymer comprises 4,4′-dicyclohexylmethane diisocyanate and 1 to 35 repeating ethyl ester groups.
[0086] In one embodiment, the molecular weight of the polyurethane is between about 40,000 and about 500,000, for example, the molecular weight may be about 40,000 to about 50,000, or 50,000 to about 75,000, or 75,000 to about 100,000, or 100,000 to about 125,000, about 125,000 to about 150,000, about 150,000 to about 175,000, about 175,000 to about 200,000, about 200,000 to about 225,000, or about 225,000. In some embodiments, the present invention relates to a method for preparing an aqueous solution of at least one molecule of the present invention, wherein the aqueous solution has a molecular weight of 0 to about 250,000, about 250,000 to about 275,000, about 275,000 to about 300,000, about 300,000 to about 325,000, about 325,000 to about 350,000, about 350,000 to about 375,000, about 375,000 to about 400,000, about 400,000 to about 425,000, about 425,000 to about 450,000, about 450,000 to about 475,000, or about 475,000 to about 500,000.
[0087] In one embodiment, the molecular weight of the hydrophilic polyurethane block copolymer is from about 40,000 to about 50,000, or from 50,000 to about 75,000, or from 75,000 to about 100,000, or from 100,000 to about 125,000, from about 125,000 to about 150,000, from about 150,000 to about 175,000, from about 175,000 to about 200,000, from about 200,000 to about 225,000, from about 225,000 to about 25,000. In some embodiments, the present invention relates to a method for preparing an aqueous solution of at least one molecule of the present invention, wherein the aqueous solution has a molecular weight of at least one molecule of the present invention and the aqueous solution has a molecular weight of at least one molecule of the present invention. In some embodiments, the aqueous solution has a molecular weight of at least one molecule of the present invention and the aqueous solution has a molecular weight of at least one molecule of the present invention.
[0088] In one embodiment, the molecular weight of the polyester-based polyurethane is from about 40,000 to about 50,000, or from 50,000 to about 75,000, or from 75,000 to about 100,000, or from 100,000 to about 125,000, from about 125,000 to about 150,000, from about 150,000 to about 175,000, from about 175,000 to about 200,000, from about 200,000 to about 225,000, from about 225,000 to about 250,000, or from about From about 250,000 to about 275,000, from about 275,000 to about 300,000, from about 300,000 to about 325,000, from about 325,000 to about 350,000, from about 350,000 to about 375,000, from about 375,000 to about 400,000, from about 400,000 to about 425,000, from about 425,000 to about 450,000, from about 450,000 to about 475,000, or from about 475,000 to about 500,000.
[0089] In one embodiment, the molecular weight of the polyether-based polyurethane is from about 40,000 to about 50,000, or from 50,000 to about 75,000, or from 75,000 to about 100,000, or from 100,000 to about 125,000, from about 125,000 to about 150,000, from about 150,000 to about 175,000, from about 175,000 to about 200,000, from about 200,000 to about 225,000, from about 225,000 to about 250,000, from about From about 250,000 to about 275,000, from about 275,000 to about 300,000, from about 300,000 to about 325,000, from about 325,000 to about 350,000, from about 350,000 to about 375,000, from about 375,000 to about 400,000, from about 400,000 to about 425,000, from about 425,000 to about 450,000, from about 450,000 to about 475,000, or from about 475,000 to about 500,000.
[0090] In one embodiment, the polyurethane comprises CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2-: wherein n is independently selected from any number of 1-35, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35; and m is independently selected from any number of 15-500, for example, 15, 25, 50, 75, 100, 125, 150, 175, 200, 225, 250, 275, 300, 325, 350, 375, 400, 425, 450, 475 or 500.
[0091] In some embodiments, one or both of n and m are average values.
[0092] In one embodiment, n is an average of 1.5 and m is 10-20, such as 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20. In one embodiment, m is 15.
[0093] In one embodiment, n is an average of 4 and m is an average of 100-120, such as 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119 or 120. In one embodiment, m is 108.
[0094] In one embodiment, n is an average of 5 and m is an average of 105-130, such as 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129 or 130. In one embodiment, m is 110.
[0095] In one embodiment, n is an average of 34, and m is an average of 75-85, such as 75, 76, 77, 78, 79, 80, 81, 82, 83, 84 or 85. In one embodiment, m is 80.
[0096] In one embodiment, n is an average of 4 and m is an average of 180-220, such as 180, 182, 184, 186, 190, 192, 194, 196, 198, 200, 202, 204, 206, 208, 210, 212, 214, 216, 218 or 220.
[0097] In one embodiment, n is an average value of 30.5, and m is an average value of 140-160, such as 140, 142, 148, 150, 152, 154, 156, 158 or 160.
[0098] In one embodiment, n is an average of 7 and m is an average of 200-240, such as 200, 202, 204, 206, 208, 210, 212, 214, 216, 218, 220, 222, 224, 226, 228, 230, 232, 234, 236, 238 or 240.
[0099] In one embodiment, the end groups of the polyurethane are independently selected from methyl and hydroxyl groups.
[0100] Water and organic polar solvents
[0101] The method disclosed herein requires forming a polyurethane solution in water and an organic polar solvent. The polyurethane may be dissolved in the solvent before adding water, or the polyurethane may be dissolved in the water and the organic polar solvent.
[0102] The polar solvent can be a protic solvent or an aprotic solvent. The solvent can be any lower aliphatic alcohol or a chlorinated solvent. For example, the solvent can be selected from the group consisting of ethanol, methanol, isopropanol, butanol, tetrahydrofuran, dimethylformamide, dimethyl sulfoxide, acetone, acetonitrile and any combination thereof.
[0103] The ratio of water to the organic solvent may be about 5:95, about 10:90, about 15:85, about 20:80, about 25:75, about 30:70, about 35:65, or about 40:60.
[0104] The water and organic solvent used to prepare the polyurethane solution can be at room temperature or elevated temperature, for example, between about 25°C to about 60°C. For example, the water and organic solvent can be heated to about 25°C, about 30°C, about 35°C, about 40°C, about 45°C, about 50°C, about 55°C, or about 60°C.
[0105] The concentration of polyurethane in water and organic polar solvent is between about 1% and about 20% (w / v), for example, the concentration can be about 1% (w / v), about 2% (w / v), about 3% (w / v), about 4% (w / v), about 5% (w / v), about 6% (w / v), about 7% (w / v), about 8% (w / v), about 9% (w / v), about 10% (w / v), about 11% (w / v), about 12% (w / v), about 13% (w / v), about 14% (w / v), about 15% (w / v), about 16% (w / v), about 17% (w / v), about 18% (w / v), about 19% (w / v), or about 20% (w / v). In one embodiment, polyurethane has a concentration of about 6% (w / v).
[0106] Mould
[0107] The method disclosed herein requires that the polyurethane solution be applied to a mold. Any mold shape can be used to prepare articles such as condoms, gloves, films or other designs and appliances. In some embodiments, existing appliances (e.g., condoms) can be used as molds.
[0108] For example, the mold can be a core mold, a casting mold, a plate mold or a sheet mold. In the embodiment of producing condoms, the mold can be a cylindrical mold or a penis mold.
[0109] In some embodiments, the mold is glass, ceramic (eg, TiN), plastic, metal, or a combination of coatings or materials.
[0110] In one embodiment, the mold is heated. For example, the mold may be heated to any temperature up to about 90°C using convection, infrared, electromagnetic induction, or conduction.
[0111] The polyurethane solution is applied to the mold to form a layer of the solution on at least a portion of the mold. For example, the mold can be immersed in the solution, or by spraying, pouring, injecting, brushing or rolling the solution onto or in the mold, or by any combination of these methods.
[0112] The polyurethane solution may be applied to the mold at room temperature, or may be heated prior to application to the mold. For example, the polyurethane solution may be heated (with or without stirring) to a temperature of about 37°C prior to application to the mold.
[0113] In some embodiments, the mold is stationary while the solution is applied. In other embodiments, the mold is in motion while the polyurethane solution is applied.
[0114] In one embodiment, the mold is immersed in the polyurethane solution at a speed of about 1 mm / s to about 1000 mm / s. For example, the immersion speed can be about 1 mm / s, about 50 mm / s, about 100 mm / s, about 200 mm / s, about 300 mm / s, about 400 mm / s, about 500 mm / s, about 600 mm / s, about 700 mm / s, about 800 mm / s, about 900 mm / s, or about 1000 mm / s.
[0115] In one embodiment, the mold is removed from the polyurethane solution at a speed of 1 mm / s to about 1000 mm / s. For example, the removal speed may be about 1 mm / s, about 50 mm / s, about 100 mm / s, about 200 mm / s, about 300 mm / s, about 400 mm / s, about 500 mm / s, about 600 mm / s, about 700 mm / s, about 800 mm / s, about 900 mm / s, or about 1000 mm / s.
[0116] Varying the immersion speed and / or withdrawal speed can be used to control the thickness of the polyurethane film.
[0117] After the polyurethane solution layer is applied to the mold, the solution is dried to form a film on the mold. Drying can be achieved by evaporation in the open atmosphere or in an oven or evaporator.
[0118] In some embodiments, drying can be performed while the mold is stationary. In other embodiments, drying can be performed while the mold is in motion.
[0119] In some embodiments, the mold is heated to facilitate drying. For example, the mold can be heated to a maximum of about 90°C using convection, infrared, electromagnetic induction, or conduction.
[0120] The polyurethane solution can be dried at room temperature or at an elevated temperature, for example from about 25° C. to about 90° C. The elevated temperature can be about 25° C., about 30° C., about 35° C., about 37° C., about 40° C., about 45° C., about 55° C., about 60° C., about 65° C., about 70° C., about 75° C., about 80° C., about 85° C., or about 90° C.
[0121] Once the film is formed on the mold, a polyurethane solution can be additionally applied. In some embodiments, a variety of polyurethane solutions can be used. For example, a first polyurethane solution (e.g., using a polyurethane with a molecular weight between about 40,000 and about 500,000) can be applied. The same solution or a different solution (using a polyurethane with a molecular weight between about 40,000 and about 500,000) can be used for a second application. The polyurethane solution can be further applied. For example, there can be two, three, four, five, six or more cycles to apply a polyurethane solution and dry the solution. In this way, any number of disclosed polyurethane solutions can be used to prepare a multilayer polyurethane film on a mold.
[0122] In some embodiments, the polyurethane solution can be applied to the entire mold or a portion of the mold. For example, the polyurethane solution can be applied to a portion of the mold or to a portion of the polyurethane film on the mold to increase the film thickness on the portion of the mold, or to produce specific features, such as ribs, on the polyurethane film on the mold or the portion of the mold.
[0123] Each layer of the multilayer polyurethane film may have different physical properties. For example, a polyurethane solution by itself may, for example, be too fragile to make a condom, but have desirable qualities (e.g., a skin-like feel) and may be used in combination with one or more other polyurethane solutions to prepare a multilayer polyurethane film on a mold. One or more layers may provide at least one property of tensile strength, linear expansion, and modulus, with other layers providing, for example, a skin-like feel or a moist skin-like feel.
[0124] In one embodiment, the condom is formed from at least two different polyurethane solutions, for example forming an inner layer and an outer layer of different polyurethanes. In this embodiment, each layer has properties that provide a different feel on both sides of the condom. For example, the different polyurethanes may have different moduli, tensile strengths, linear expansion ranges, and / or elongation at break.
[0125] In some embodiments, the use of different polymer solutions may require adhesion between the layers. The adhesion can be achieved by applying the polyurethane solution to the dry film so that a part of the dry film becomes solubilized or the applied solution diffuses into the dry film. Alternatively, an adhesive can be applied to the film before applying additional polyurethane solution.
[0126] In some embodiments, the polymer solution can be molded into a non-hydrogel material as a layer of structure and / or feature. For example, the polymer solution can be molded into latex, polyisoprene, non-hydrated polyurethane, and other typical or atypical materials for devices including condoms.
[0127] The polymer solution can be applied to all or part of the interior or exterior of a non-hydrogel material, such as the inside, interior, or exterior of a device such as a condom.
[0128] The initial polymer film or multilayer film may be dried prior to application of a subsequent polyurethane solution. Alternatively, a subsequent amount of polyurethane solution may be applied without drying the prior application.
[0129] In some embodiments, can utilize the repeated application of polyurethane solution to produce the polyurethane film of predetermined thickness, for example, about 50 microns to about 200 microns.This predetermined thickness can be about 10 microns, about 20 microns, about 30 microns, about 40 microns, about 50 microns, about 60 microns, about 70 microns, about 80 microns, about 90 microns, about 100 microns, about 110 microns, about 120 microns, about 130 microns, about 140 microns, about 150 microns, about 160 microns, about 170 microns, about 180 microns, about 190 microns or about 200 microns.In some embodiments, this predetermined thickness is about 70 microns to about 80 microns.
[0130] Swelling agent
[0131] The methods disclosed herein require contacting the polyurethane film or multilayer polyurethane films with a swelling agent under conditions such that the film forms a polyurethane hydrogel.
[0132] The swelling agent may contain water or consist of water. In other embodiments, the swelling agent is one or more of water, an aqueous solution, an ethylene glycol solution, a hydroxyethylcellulose solution, a paraben-based solution, an ethylene glycol-based solution, a glycerin-based solution, an oil-based solution, or a silicone-based solution. In some embodiments, the swelling agent may be one or more of these solutions.
[0133] In one embodiment, the swelling agent is water.
[0134] The swelling agent may include a spermicide, a lubricant, an antiviral agent, an antifungal agent, an antibacterial agent, a prebiotic, a probiotic, a microbiome enhancer, a flavor compound, an aroma compound, a sensory enhancer, a sterilant, or a disinfectant.
[0135] The polymer film may be immersed in the swelling agent and immediately removed. Alternatively, the polymer film or material may be immersed in the swelling agent and allowed to contact the swelling agent for a period of time before removal. The polymer film or material may remain on the mold while in contact with the swelling agent, or the polymer film may be removed from the mold before contacting the swelling agent.
[0136] In some embodiments, the polyurethane film is contacted with the swelling agent for about 1 second to about 60 seconds, and may be further contacted with the swelling agent immediately or later.
[0137] In other embodiments, the polyurethane film is contacted with the swelling agent overnight to a maximum of about 24 hours. For example, the polyurethane film is contacted with the swelling agent for about 15 minutes, about 30 minutes, about 45 minutes, about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, or about 24 hours.
[0138] In some embodiments, the polyurethane film is contacted with the swelling agent until the maximum swelling of the polyurethane hydrogel is reached. In some cases, this may take more than 24 hours.
[0139] In one embodiment, the temperature of the swelling agent is room temperature or about 20° C. to about 90° C. Increasing the temperature of the swelling agent can shorten the time required for the polyurethane film to swell into a polyurethane hydrogel. Therefore, the temperature of the swelling agent can be about 20° C., about 25° C., about 30° C., about 35° C., about 40° C., about 45° C., about 50° C., about 55° C., about 60° C., about 65° C., about 70° C., about 75° C., about 80° C., about 85° C., or about 90° C.
[0140] Polyurethane hydrogel
[0141] The polyurethane hydrogel formed by contacting the polyurethane film with the swelling agent may have a swelling agent content between about 1% and about 95%, such as about 1%, about 5%, about 10%, about 15%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, or about 95%. In some embodiments, the swelling agent content is about 45%, about 50%, or about 55%, for example, about 54%. In some embodiments, the hydrogel has a swelling agent content close to or equal to the water content of the skin. The general water content of the skin is about 64%, so in some embodiments, the swelling agent content of the polyurethane hydrogel is about 60% to about 70%, for example, about 64%.
[0142] In some embodiments, the swelling agent is oil-based or silicone-based. In these embodiments, the polyurethane hydrogel formed by contacting the polyurethane film with a silicone-based or oil-based swelling agent preferably has a swelling agent content between about 0.1% and about 30%, such as about 1%, about 2%, about 4%, about 8%, about 10%, about 12%, about 14%, about 16%, about 18%, about 20%, about 22%, about 24%, about 26%, about 28%, or about 30%. For example, after contacting with the swelling agent for 24 hours, the polyurethane hydrogel may have a silicone-based or oil-based swelling agent content between about 0.1% and about 10%, such as about 0.1%, about 0.5%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10%.
[0143] In some embodiments, the swelling agent is a mixture or hybrid of swelling agents of two or more bases. For example, in some embodiments, the swelling agent is a hybrid of water and silicone.
[0144] The polyurethane hydrogel forms prepared by the methods disclosed herein possess a number of properties that make them suitable for use in applications such as condoms, including suitable linear expansion properties, tensile strength, modulus, the ability to stretch sufficiently before breaking, yet impermeable to biologics and permeable to small molecules.
[0145] These properties can be adjusted by selecting one or more of the following factors: polymer type, molecular weight range, average molecular weight, n:m range of each polymer, or by mixing two or more polymers. In some embodiments, polymers with higher molecular weights produce stronger but harder and less flexible hydrogels, and polymers with lower molecular weights produce hydrogels that are more easily broken (weaker) but softer and more flexible. Therefore, by blending multiple polymers, selecting polymers with one or more specific average molecular weights, molecular weight distributions, and n:m, hydrogels can be prepared by the methods described herein to have a desired range of properties (linear expansion, tensile strength, modulus, stretchability, impermeability) suitable for a specific application (e.g., condoms). In addition to the amount and type of swelling agent in the hydrogel, these properties affect the user's experience of the hydrogel, that is, they affect the "feel" of the hydrogel.
[0146] In one embodiment, the properties can be adjusted by using polymers with different n and m values or a specific n:m. For example, n:m affects the amount of swelling of the hydrogel, which in turn affects the modulus, which in turn is related to the feel of the hydrogel. It is important to note that while modulus is an important factor affecting the feel of the hydrogel, other properties and factors such as swelling agent content and type can also affect the feel.
[0147] In some embodiments, n:m is 1:0.1 to 1:75. For example, suitable n:m includes 1:21-26 (corresponding to A in Example 1), 1:25-30 (corresponding to B in Example 1), 1:6.67-13.33 (corresponding to C in Example 1), 1:2.2-2.5 (corresponding to D in Example 1), 1:4.59-5.25 (corresponding to E in Example 1), 1:28.57-34.30 (corresponding to F in Example 1). Assuming that in some embodiments, n and m are average values, n:m also represents the ratio of the average value n to the average value m.
[0148] In some embodiments, the ratio of n to m is about 1 and any number between 0.1-75, such as 1:0.1, about 1:0.5, about 1:1, about 1:5, about 1:10, about 1:15, about 1:20, about 1:25, about 1:30, about 1:35, about 1:40, about 1:45, about 1:50, about 1:55, about 1:60, about 1:65, about 1:70, or about 1:75.
[0149] "Linear expansion" refers to the ratio of the change in length of a material to its initial length. In one embodiment, the polyurethane hydrogel film or material has a linear expansion between about 1% and 100%, such as about 10%, about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, or about 100%.
[0150] The term "tensile strength" refers to the maximum force that a sample withstands before damage. The tensile strength is the ratio of the maximum force to the initial cross-sectional area of the sample. In one embodiment, the hydrogel material has a tensile strength between about 1 MPa and about 100 MPa, such as about 3 MPa, about 4 MPa, about 5 MPa, about 6 MPa, about 7 MPa, about 8 MPa, about 9 MPa, about 10 MPa, about 11 MPa, about 12 MPa, about 13 MPa, about 14 MPa, about 15 MPa, about 16 MPa, about 17 MPa, about 18 MPa, about 20 MPa, about 25 MPa, about 30 MPa, about 35 MPa, about 40 MPa, about 45 MPa, about 50 MPa, about 55 MPa, about 60 MPa, about 65 MPa, about 70 MPa, about 75 MPa, about 80 MPa, about 85 MPa, about 90 MPa, about 95 MPa, or about 100 MPa.
[0151] As used herein, the term "modulus" refers to the force at a specific elongation value, which is related to the hardness of the material. In one embodiment, the hydrogel material has a 50% modulus of about 80 kPa to about 15 MPa, a 100% modulus of about 200 kPa to about 15 MPa, and a 300% modulus of about 700 kPa to 15 MPa.
[0152] In one embodiment, the 50% modulus is about 80 kPa to 15 MPa, for example 80 kPa, 100 kPa, 500 kPa, 750 kPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 13 MPa, 14 MPa, or 15 MPa.
[0153] In one embodiment, the 100% modulus is about 200 kPa to about 15 MPa, for example 200 kPa, 250 kPa, 500 kPa, 750 kPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 13 MPa, 14 MPa, or 15 MPa.
[0154] In one embodiment, the 300% modulus is about 700 kPa to 15 MPa, such as 700 kPa, 750 kPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 13 MPa, 14 MPa, or 15 MPa.
[0155] The term "elongation at break" refers to the maximum linear stretch of a material before sample failure. Elongation at break is defined as the percentage (%) increase in the material's length beyond its initial length.
[0156] refer to Figure 1 and Figure 2 , the elongation at break can be calculated using the load-elongation curve. Figure 1 and Figure 2 In each of the Figures, a 20 mm sample ring of a hydrogel condom produced by the process described herein (including either Polymer A or Polymer B) was tested as illustrated in the Examples. Figure 1 The condom has a double wall thickness of 0.125 mm and a width of 58 mm. Figure 2 The condom has a double wall thickness of 0.148 mm and a width of 53 mm.
[0157] In one embodiment, the hydrogel material has an elongation at break of about 200%, about 300%, about 400%, about 500%, about 600%, about 700%, about 800%, about 900%, about 1000%, about 1100%, about 1200%, about 1300%, about 1400%, about 1500%, about 1600%, about 1700%, about 1800%, about 1900%, or about 2000%.
[0158] In one embodiment, the hydrogel is substantially impermeable to biological agents, such as viruses or virus models (e.g., Φ-X174) or bacteria (e.g., E. coli). The average diameter of Φ-X174 is about 30 nm, and therefore, the hydrogel is substantially impermeable to biological agents having an average diameter of 30 nm or greater. In one embodiment, when a pressure of up to about 10 kPa is applied to the hydrogel, the hydrogel is substantially impermeable to biological agents of 30 nm or greater. The pressure may be up to about 1 kPa, up to about 2 kPa, up to about 3 kPa, up to about 4 kPa, up to about 5 kPa, up to about 6 kPa, up to about 7 kPa, up to about 8 kPa, up to about 9 kPa, or up to about 10 kPa.
[0159] In another embodiment, the hydrogel is permeable to small molecules, such as water-soluble small molecules. The inventors have demonstrated that polyurethane hydrogels are permeable to sodium fluorescein (molecular weight 376.275 g / mol) and rhodamine B (molecular weight 479.02 g / mol). Therefore, the hydrogel is permeable to water-soluble small molecules with a molecular weight of about 500 g / mol or less.
[0160] For example, when the polyurethane hydrogels described herein are used in condoms, one advantage is that they are visually transparent, which is in stark contrast to traditional latex or polyisoprene condoms.
[0161] In one embodiment, a condom formed from a polyurethane hydrogel has a linear expansion of about 40%, a swelling agent content of about 60%, a tensile strength of about 15.2 MPa, an elongation at break of about 747%, and a 50% modulus of about 2.8 MPa, a 100% modulus of about 3.6 MPa, and a 300% modulus of about 6.7 MPa.
[0162] In another embodiment, a condom formed from a polyurethane hydrogel has a linear expansion of about 30%, a swelling agent content of about 50%, a tensile strength of about 26.3 MPa, an elongation at break of about 591%, and a 50% modulus of about 2.5 MPa, a 100% modulus of about 3.3 MPa, and a 300% modulus of about 6.6 MPa.
[0163] Testing of condoms can involve inflating the condom with air to test the volume of air that can be contained within the condom before the condom bursts. When the condom bursts, the volume of air contained therein is referred to as the burst volume. In an exemplary embodiment, the hydrogel condoms described herein have a burst volume of about 5 L to 40 L. For example, the burst volume can be about 5 L, about 10 L, about 15 L, about 20 L, about 25 L, about 30 L, about 35 L, about 40 L, about 45 L, or about 50 L.
[0164] In addition, filling the condom with air also increases pressure, and the maximum air pressure at the time of bursting is called the burst pressure. In an exemplary embodiment, the hydrogel condoms described herein have a burst pressure of about 0.75 kPa to about 4 kPa. For example, the burst pressure can be about 0.75 kPa, about 1 kPa, about 1.25 kPa, about 1.5 kPa, about 1.75 kPa, about 2 kPa, about 2.25 kPa, about 2.5 kPa, about 2.75 kPa, about 3 kPa, about 3.25 kPa, about 3.5 kPa, about 3.75 kPa, about 4 kPa, about 4.25 kPa, about 4.5 kPa, about 4.75 kPa, or about 5 kPa. In some embodiments, the burst pressure can be about 1.3 kPa to about 3.6 kPa.
[0165] The polyurethane hydrogels have additional advantageous attributes, including user reports that the polyurethane hydrogel material feels like skin, feels wet, feels soft, feels like the user has no sensory loss (i.e., feels nothing), or a combination thereof. In some embodiments, the polyurethane hydrogels are visually transparent, such that visual appeal or visual stimulation is not compromised.
[0166] In some embodiments, polyurethane hydrogels conduct heat more effectively than other condom materials, allowing for less impaired transfer of body heat.
[0167] Polyurethane hydrogels may also have no objectionable odor or taste.
[0168] In some embodiments, polyurethane hydrogels are hypoallergenic, that is, they do not induce an allergic reaction.
[0169] In some embodiments, the polyurethane hydrogel is manufactured to have multiple regions with different physical properties (e.g., modulus, linear expansion, elongation at break, burst pressure, etc.). This is achieved by using different polymers for each of the multiple regions. For example, a condom can be made using a higher modulus hydrogel that feels firm on the inner surface and a lower modulus hydrogel that feels soft on the outer surface, or vice versa. Alternatively, there can be areas of modified modulus, such as a condom with a front region that has a different modulus than the modulus of the shaft; a shaft with a ring or region of modified modulus, or other properties. By using polymers of different molecular weights, n:m, or both, the device manufactured using the methods described herein can have distinct and different feelings in different aspects of the final use device; the final use device is, for example: a condom with multiple sensations that produce different sensations along the condom for either partner. In particular, the hydrogel can be skin-like.
[0170] As shown in Table 1, the properties of the polyurethane hydrogel condoms described in this article are superior to those of traditional condoms.
[0171] Table 1: Comparison of properties of typical condom materials and hydrogels
[0172] Example
[0173] Example 1: Preparation of polyurethane solution
[0174] Solvent: Ethanol and water in a ratio ranging from 60:40 to 95:5, depending on the polyurethane. 90:10 ethanol and water was selected as a ratio in which the following polymers (including each of the following AF) were easily soluble:
[0175] A:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH 2, -, where n is an average of 5 and m is approximately 105-130; or
[0176] B:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2-, where n is an average of 4 and m is about 100-120;
[0177] C:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2-, where n is an average of 1.5 and m is about 10-20;
[0178] D:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10)NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2-, where n is an average of 34 and m is about 75-85;
[0179] E:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2-, where n is an average value of 30.5 and m is about 140-160;
[0180] F:-CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n-CH2-, wherein n is an average of 7 and m is approximately 200-240.
[0181] Polymer solution: The above polymers were dissolved in solvent (ethanol: water 90:10 v / v) respectively. The polymer concentration can range from 1% w / v to 10% w / v to form the film. A concentration of 6% w / v was selected to prepare all films (see Table 2). However, for the dip coating process, the concentration can be further optimized to control the number of dips required to achieve the desired thickness and the film quality.
[0182] The mixture was stirred overnight to dissolve the polymer. Heating to 70°C increased the rate of dissolution.
[0183] The stress of the hydrogels prepared in the above examples was measured as a function of elongation using a "dog bone" shaped sample of the hydrogel at an elongation rate of 500 mm / min. The stress was calculated by finding the ratio of force to the initial cross-sectional area of the dog bone sample. The elongation is defined as the ratio of the elongated length to the initial length. The modulus was calculated by giving the stress at 50%, 100% and 300% sample elongation.
[0184] Table 2: Exemplary hydrogels and their general properties
[0185]
[0186] Example 2: Swelling Agent Compatibility
[0187] To investigate the swelling compatibility of polymers, a range of body care products were investigated. Polymer sheets were cast by adding 5 mL of a 6% (w / v) polymer solution to a mold. The dried sheets were cut into various shapes and measured by length. The polymers were then soaked in various swelling compounds that are commercially available sexual health products. The polymers were placed in these swelling agents for 24 hours and re-measured to determine immediate swelling compared to a control dry material.
[0188] As shown in Table 3, various polymers were investigated as well as lubricant types including water-based, silicone-based, and oil-based formulations.
[0189] Measurements of linear expansion of hydrogels swollen with various body care products were studied. Table 3 shows examples from polymer A and polymer B. Tensile strength was analyzed for each matrix type and the results showed that no lubricant-based swelling agent would reduce tensile strength. The results show that hydrogel condoms are compatible with a wider range of lubricant options than traditional latex or polyisoprene. Traditional latex or polyisoprene cannot be used with oil-based lubricants because the oil will degrade the material. In addition, the hydrogels are compatible with silicone lubricants, which are not recommended for use with silicone toys.
[0190] Table 3: Lubricant types
[0191]
[0192] Example 3: Condom prototype production:
[0193] Condom prototypes are made using a dip coating process where a cylindrical mould is dipped into a heated polymer solution. The mould is preferably made of glass or metal. The inventors have found that plastic moulds are not ideal because the polyurethane solution tends to cover the mould unevenly after dipping.
[0194] In one experiment, multiple glass or metal molds were assembled into a mold apparatus to produce multiple prototype condoms.
[0195] The polymer solution is placed in a large container, the width of which is sufficient to accommodate the mold device and the height of which is sufficient to allow for liquid displacement. The container is placed below the mold device.
[0196] Under continuous stirring, the polymer solution in the container is heated to 25°C. The mold is immersed in the polymer solution and removed at a speed of 20-200 mm / s. After the mold is removed, the polymer solution is covered to minimize solvent evaporation.
[0197] The mold to which the polymer solution has been applied is kept at room temperature for at least 5 to 10 minutes until the solvent evaporates from the coating and a polyurethane film is formed on the mold. If drying is carried out at high temperatures (e.g. in an oven or dehydrator), this time can be significantly shortened.
[0198] Repeated dipping and drying steps increase the thickness of the polyurethane film that forms the condom. Typically these polymers are dipped 1 to 6 times to make condoms.
[0199] In some cases, a series of dippings are performed using a polymer of one molecular weight and a single dipping or a series of dippings are performed using a polymer of another molecular weight to make the condom.
[0200] In one example, the condom is made of a first layer of hydrogel comprising polymer A and a second layer of hydrogel comprising polymer B. In another example, the condom is made of a first layer of hydrogel comprising polymer B and a second layer of hydrogel comprising polymer A.
[0201] Once the solvent has completely evaporated from the coated mold, the mold apparatus containing the mold can be immersed in a container filled with excess swelling agent or hydrating solution to swell the dry film to form a hydrogel.
[0202] Example 4: ISO standard condom test:
[0203] The following data are the results obtained from traditional international tests for condom standards. These tests are from ISO 23409:2011 Male condoms - Requirements and test methods for condoms made from synthetic materials and ISO 4074:2015 Natural rubber latex male condoms - Requirements and test methods for condom batch testing. The tensile test does not currently appear in ISO or ASTM protocols, but it is a useful guide for the development of alternative condom materials.
[0204] Condoms are produced by selecting Polymer A and Polymer B (as described above). Testing is performed by Enersol, an independent quality assurance testing facility and service certified to meet the requirements of ISO 17025:2017 and ISO 9001:2015, testing dimensional, tensile, burst and leakage tests.
[0205] To measure the length, the condom is stretched slightly (5% to 10%) to eliminate wrinkles caused by rolling, and then hung on a graduated mandrel. When the condom is unrolled and lies flat without any creases, the width is measured at right angles to the length of the condom. Typically, three thickness measurements are made for each condom sample, and the average value is determined. Table 4 provides the results of measurements made for condoms labeled Type A and Type B; in each case, the condom type is defined as the main component of the condom from the corresponding polymer type in Table 2.
[0206] Table 4: Condom Measurements
[0207] thickness Low(mm) Average value(mm) Height(mm) Type A condom 0.108 0.120 0.132 Type B condoms 0.08 0.122 0.190 width Low(mm) Average value(mm) Height(mm) Type A condom 57 58.5 59 Type B condoms 53 55.9 59
[0208] The tensile strength of condoms was evaluated using 20 mm wide samples cut from the middle of the condom. The test uses a constant circular motion rate to apply pressure equally to the entire cross-sectional portion (ring) of the condom, stretching the cross-sectional portion (ring) of the material until it breaks. The test measures the force required to break the material (force to break, in Newtons); the length of the material when it breaks (percent elongation, the percentage increase from the initial circumference to the final circumference); and the tensile strength at break (MPa), a method of calculating the number of Newtons using the thickness of the material and the force to break. Table 5 provides the tensile strength measurements of condoms containing polymer A or polymer B.
[0209] Table 5: Condom tensile strength
[0210] Tensile Strength Low (MPa) Average value (MPa) High (MPa) Type A condom 2.9 8.6 15.2 Type B condoms 3.4 10.5 26.3 Breaking force Low (N) Average value(N) High (N) Type A condom 6.8 20.7 35.5 Type B condoms 7.2 25.6 77.7 Material elongation Low(%) average value(%) high(%) Type A condom 421 663 763 Type B condoms 286 627 797
[0211] The burst pressure and burst volume are evaluated by inflating the condom like a balloon and measuring the volume of air and air pressure required to burst. The condom is unfolded and clamped on a rod, leaving about 150 mm to be inflated. The test instrument inflates the condom with clean, oil-free, moisture-free air at a specified rate. Table 6 provides the burst pressure of condoms containing polymer A or polymer B.
[0212] Table 6: Burst pressure of condoms
[0213] Burst pressure Low(kPa) Average value (kPa) High(kPa) Type A condom 0.70 1.02 1.30 Type B condoms 0.75 1.71 4.10 Explosion volume Low (L) Average value(L) Height (L) Type A condom 3.0 20.2 29.5 Type B condoms 1.0 15.0 37.0
[0214] Leakage testing is done using the hanging method, where condoms are filled with water, usually while hanging vertically, and an observer checks for leaks. In addition, the ends of a water-filled condom are tied and then rolled on absorbent paper, observing the moisture on the paper. Samples from different batches of condoms are tested and pass the no-hole (leak) test.
[0215] Additional condoms were made by adding layers of different polymers. In one example, a condom made of polymer A was covered with a layer of polymer B, or vice versa. In these examples, the condoms had different properties, as shown in Table 1. The mechanical property testing of the condoms met or exceeded ISO standards and was within the parameters of the mechanical test results listed above.
[0216] Example 5: Phage barrier assay
[0217] The biobarrier properties of polymer A and polymer B and the diffusion resistance when a small bacterial virus (bacteriophage Φ-X174) was used as a challenge particle were tested. The use of Φ-X174 is known as a virus penetration test and is commonly used to check the barrier properties of condoms (based on ISO 23409:2011). In these tests, a sample condom is restrained and the condom is provided with a suspension of the surrogate virus bacteriophage Φ-X174. By immersing the sample in a collection liquid, the leakage of virus particles through the sample can be detected by analyzing the collection liquid for the presence of virus particles.
[0218] Hydrogel material A and hydrogel material B were sandwiched between the donor and receptor chambers of a Franz cell. The receptor chamber contained phosphate buffered saline (PBS) and the donor chamber contained Φ-X174 bacteriophage in PBS. Samples were taken from the receptor chamber and analyzed and quantified by phage formation assay. As a positive control, the materials were damaged by puncture with a 25G needle. The test materials showed that they were not permeable to Φ-X174.
[0219] The restrained and pressurized condoms made from polymer A and polymer B were also tested. The condoms passed the viral penetration test.
[0220] In addition, hydrogel A and hydrogel B were exposed to E. coli, which causes urinary tract infections. Hydrogel material A and hydrogel material B were sandwiched between the donor and receptor chambers of a Franz cell. The receptor chamber contained phosphate buffered saline and the donor chamber contained E. coli in PBS. Samples were taken from the receptor chamber and analyzed by growing on LB agar plates, and no growth of E. coli was observed in the samples taken from the receptor chamber. As a positive control, the hydrogel materials were damaged by puncturing them with a 25G needle. The test materials showed that they were not permeable to E. coli.
[0221] Those skilled in the art will appreciate that, as shown in the specific embodiments, various changes and / or modifications may be made to the present invention without departing from the spirit or scope of the present invention as generally described. Therefore, the present embodiments are considered in all aspects to be illustrative and not restrictive.
Claims
1. A method for producing a molded polyurethane hydrogel condom, the method comprising: forming a first solution of at least one polyurethane having a molecular weight between 50,000 and 200,000 in an organic polar solvent containing less than 40% (v / v) water and water; applying a layer of the first solution to a mold; drying the layer of the first solution to form a polyurethane film on the mold; as well as contacting the polyurethane film with the swelling agent under conditions where the film forms a polyurethane hydrogel having a swelling agent content between 30% and 95%; Wherein, the polyurethane is composed of -CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHC O-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2 and methyl and / or hydroxyl end groups, wherein n is an average independently selected from any number between 1 and 35; and m is an average value independently selected from any number between 15 and 500; Wherein, the molded polyurethane hydrogel condom has a tensile strength of 20 MPa to 100 MPa.
2. The method of claim 1, wherein: The molecular weight of the polyurethane is 50,000 to 100,000.
3. The method according to claim 1 or 2, wherein: The polyurethane is derived from the polymerization of 4,4'-dicyclohexylmethane diisocyanate.
4. The method according to claim 1 or 2, wherein: The organic polar solvent is selected from the group consisting of ethanol, methanol, isopropanol, butanol, tetrahydrofuran, dimethylformamide, dimethyl sulfoxide, acetone, acetonitrile and any combination thereof.
5. The method of claim 4, wherein: The organic polar solvent is ethanol.
6. The method according to claim 1 or 2, wherein: The ratio of water to organic polar solvent is selected from 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, or 40:
60.
7. The method of claim 6, wherein: The ratio of water to organic polar solvent is 10:
90.
8. The method according to claim 1 or 2, wherein: The swelling agent is selected from at least one of water, hydroxyethyl cellulose solution, paraben-based solution, ethylene glycol-based solution, glycerin-based solution or silicone-based solution.
9. The method according to claim 1 or 2, wherein: The swelling agent is an oil-based solution.
10. The method of claim 8, wherein: The swelling agent comprises one or more of a spermicide, a lubricant, an antiviral agent, an antifungal agent, an antibacterial agent, a prebiotic, a probiotic, a flavor compound, an aroma compound, a sensory enhancer, a sterilant, or a disinfectant.
11. The method of claim 8, wherein: The swelling agent comprises a microbiome enhancing agent.
12. The method according to claim 1 or 2, wherein: The polyurethane film is contacted with the swelling agent at ambient temperature for at least 1 second.
13. The method of claim 1 or 2, further comprising: forming a second solution of at least one polyurethane having a molecular weight between 50,000 and 200,000 in an organic polar solvent containing less than 40% (v / v) water and water; applying a layer of the second solution to the polyurethane film on the mold; drying the layers of the second solution, wherein the layers form a polyurethane film on the mold; and contacting the polyurethane film with the swelling agent under conditions where the film forms a polyurethane hydrogel having a swelling agent content between 1% and 95%; Wherein, the polyurethane is composed of -CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHC O-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-O-CH2) n -CH2 and methyl and / or hydroxyl end groups, wherein n is an average independently selected from any number between 1 and 35; and m is an average value independently selected from any number between 15-500.
14. The method of claim 1, wherein: The ratio of n to m is 1:0.1 to 1:
75.
15. The method of claim 13, wherein: The ratio of n to m is 1:0.1 to 1:
75.
16. The method of claim 13, wherein: The at least one polyurethane in the second solution is different from the at least one polyurethane in the first solution.
17. The method of claim 13, further comprising applying subsequent layers of the first solution or the second solution to the polyurethane film on the mold to increase thickness or impart specific properties to the polyurethane film.
18. The method of claim 13, further comprising applying subsequent layers of the first solution or the second solution to the portion of the polyurethane film on the mold to increase thickness or create specific features on the portion of the polyurethane film.
19. The method of claim 18, wherein: The specific features formed from the subsequent layer have a different modulus, tensile strength and / or linear expansion range than the hydrogel formed by the layer to which the subsequent layer is applied.
20. The method of claim 13, wherein: Either or both of the molecular weight and n:m of the at least one polyurethane in the first solution is different from the molecular weight and / or n:m of the at least one polyurethane in the second solution.
21. The method of claim 17 or 18, wherein: Additional subsequent layers are applied to increase the thickness to a predetermined value.
22. The method of claim 1 or 2, wherein: The molded polyurethane hydrogel condom has a linear expansion range of 1% to 100%.
23. The method of claim 1 or 2, wherein: The molded polyurethane hydrogel condom has a tensile strength of 30 MPa to 60 MPa, 60 MPa to 80 MPa, or 80 MPa to 100 MPa.
24. The method of claim 1 or 2, wherein: The molded polyurethane hydrogel condom has an elongation at break ranging from 200% to 2000%.
25. The method of claim 1 or 2, wherein: The molded polyurethane hydrogel condom has a shear modulus of at least one of a 50% modulus of 80 kPa to 15 MPa, a 100% modulus of 200 kPa to 15 MPa, and a 300% modulus of 700 kPa to 15 MPa.
26. A molded polyurethane hydrogel condom produced according to the method of any one of claims 1 to 25.
27. A molded polyurethane hydrogel condom, wherein: The polyurethane hydrogel comprises a polyurethane with a molecular weight between 50,000 and 100,000 and a swelling agent with a content between 40% and 70%, wherein the polyurethane is composed of -CH2-(CH2-O-CH2) n -CH2-[O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O-(CH2CH2-O-CH2CH2)-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-NH-(C6H 10 )CH2(C6H 10 )NHCO-O-CH2CH2-O-CH2CH2-O-OCHN(C6H 10 )CH2(C6H 10 )NHCO-O] m -CH2-(CH2-OC H2) n -CH2 and methyl and / or hydroxyl end groups, wherein n is an average independently selected from any number between 1 and 35; and m is an average value independently selected from any number between 15 and 500; Wherein, the molded polyurethane hydrogel condom has a tensile strength of 20 MPa to 100 MPa.
28. The molded polyurethane hydrogel condom of claim 27, having one or more of a linear expansion range of 1% to 100%, a tensile strength range of 30 MPa to 100 MPa, and an elongation at break range of 200% to 2000%.
29. The molded polyurethane hydrogel condom of claim 27 or 28, wherein: The condom is substantially impermeable to biological agents having an average diameter of 30 nm or greater.
30. The molded polyurethane hydrogel condom of claim 27 or 28, wherein: The condom is substantially impermeable to biological agents having an average diameter of 30 nm or greater at simulated use pressures ranging from atmospheric pressure to 5 kPa.
31. The molded polyurethane hydrogel condom of claim 27 or 28 having a burst volume of 5L to 50L.
32. The molded polyurethane hydrogel condom of claim 31, wherein: The blasting volume is 5L to 40L.
33. The molded polyurethane hydrogel condom of claim 27 or 28 having a burst pressure of 0.75 kPa to 5 kPa.
34. The molded polyurethane hydrogel condom of claim 33 having a burst pressure of 1 kPa to 5 kPa.
35. The molded polyurethane hydrogel condom of claim 34, wherein: The bursting pressure is 1.3 kPa to 3.6 kPa.
36. The molded polyurethane hydrogel condom of claim 35, wherein: The bursting pressure is 1.6 kPa to 3.6 kPa.