Erosion wear test method
By simulating the erosion of the experimental pipeline and the two-way tension of the specimen, combined with multi-phase fluid erosion, the problem of material erosion under complex working conditions in oil and gas fields was solved, reasonable experimental data was obtained, and safety production and production efficiency were improved.
Patent Information
- Application Number
- CN202010906197.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-09-01
AI Technical Summary
Existing technology is difficult to effectively simulate the complex erosion and wear conditions of pipeline materials in oil and gas fields during fracturing construction, reverse drainage, well killing and blowout, etc., resulting in safety accidents, reduced output, and increased costs.
An experimental pipeline with the same material as the actual failed pipeline was used to simulate erosion, and the bidirectional tension of the specimen and multi-phase fluid erosion were combined to simulate complex working conditions to obtain reasonable experimental data.
It has realized the research on the erosion and wear laws of materials under complex working conditions, provided effective data to guide on-site safe production, and improved safety and production efficiency.
Smart Images

Figure CN114112760B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas resource development, and in particular to an erosion and wear test method. Background Art
[0002] Erosion wear refers to a type of wear phenomenon in which the surface of a material is damaged when it is impacted by small and loose flowing particles. Its definition can be described as the loss of surface material when a solid surface is in contact with a fluid containing solid particles and moves relative to it. The fluid carrying the solid particles can be a high-speed airflow (called sandblasting erosion) or a liquid flow (called mud erosion). Erosion wear is a common form of wear in modern industrial production and one of the important reasons for the damage and scrapping of equipment and its components.
[0003] The entire process of oil and gas field exploration and development involves a large number of multiphase flow conditions. Erosion failure of tools and equipment can lead to safety accidents, reduced production, increased costs and other consequences. Among them, safety risks mainly exist in equipment and pipeline erosion and corrosion failure in fracturing construction (solid phase erosion, vibration fatigue, internal pressure exceeding 100MPa), backflow (high sand content, high flow rate, high internal pressure), well killing and blowout (gas-liquid-solid three-phase high pressure, high-speed erosion), high-pressure gas well sand production and other links.
[0004] However, current research on material erosion is mostly focused on a single fluid erosion condition, that is, the erosion of the specimen is completed by impacting the multiphase fluid onto the specimen at a certain speed and angle through a nozzle. It is impossible to simulate the complex conditions of pipeline material erosion failure in links such as fracturing construction, backflow, well killing and blowout, and high-pressure gas well sand production, and obtain reasonable and effective experimental data to guide on-site safety production. Summary of the invention
[0005] The purpose of the present invention is to provide an erosion and wear test method to address the above problems, which can simulate the complex working conditions of pipelines and obtain reasonable and effective experimental data for guiding on-site safe production.
[0006] In order to achieve the above object, the present invention provides an erosion wear test method, the method comprising:
[0007] S1. Obtain the failure point, internal pressure and erosion parameters of the actual failed pipeline;
[0008] S2, using a pipeline of the same material as the actual failed pipeline and proportionally reduced as the first experimental pipeline, simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the failure point of the first experimental pipeline;
[0009] S3, using a visual pipeline of the same size as the first experimental pipeline as the second experimental pipeline, simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the erosion parameters of the second experimental pipeline at the failure point;
[0010] S4. Take the specimen as the experimental subject, apply bidirectional tension to the specimen along two vertical axes to simulate the internal pressure of the pipeline, and spray erosion medium onto one side surface of the specimen according to the erosion parameters at the failure point to perform an erosion experiment.
[0011] Optionally, the erosion parameters of the actual failed pipeline include erosion medium parameters and erosion velocity, wherein the erosion medium parameters include the type and physicochemical properties of sand-carrying fluid, the type and physicochemical properties of solid particles, and sand content.
[0012] Optionally, the erosion parameters at the failure point include erosion medium parameters, erosion angle and erosion speed, wherein the erosion medium parameters include the type and physicochemical properties of sand-carrying fluid, the type and physicochemical properties of solid particles and sand content.
[0013] Optionally, the erosion angle is determined according to the erosion angle of the streamline with the largest proportion in the erosion cloud map of the second experimental pipeline.
[0014] Optionally, the erosion rate is determined according to an erosion rate of solid particles in the erosion medium at the failure point of the second experimental pipeline.
[0015] Optionally, the erosion velocity of the solid phase particles in the erosion medium at the failure point of the second experimental pipeline is measured by a PIV velocity measurement module arranged outside the second experimental pipeline.
[0016] Optionally, the sand content is determined according to the number of solid particles in the erosion medium that impact the failure point of the second experimental pipeline within a certain period of time.
[0017] Optionally, the number of solid particles in the erosion medium that impact the failure point of the second experimental pipeline within a certain period of time is measured by a solid particle impact detection module that is arranged at the failure point on the inner wall of the second experimental pipeline and has an area and shape similar to the failure point.
[0018] Optionally, the method includes: performing vibration fatigue treatment on the test piece before S4.
[0019] Optionally, the method comprises: performing corrosion aging treatment on the test piece before S4.
[0020] Optionally, the method comprises: performing a temperature reduction treatment on the test piece before S4.
[0021] Optionally, the erosion medium is a gas-solid two-phase, liquid-solid two-phase, or gas-liquid-solid three-phase multiphase fluid.
[0022] Optionally, the method includes: after S4, recovering the erosion medium, separating the liquid in the erosion medium for recycling, and separating the solid phase particles in the erosion medium for analyzing the physicochemical properties of the particles.
[0023] The erosion and wear experimental method of the present invention can obtain the failure point of the experimental pipeline and the erosion parameters at the failure point by simulating the actual pipeline erosion through the experimental pipeline on the one hand; on the other hand, by applying bidirectional tension to the specimen along the two vertical axes of the specimen respectively, the high internal pressure load borne by the pipeline during fracturing construction, backflow, well killing and blowout can be simulated, and at the same time, the specimen is subjected to multiphase flow erosion according to the erosion parameters at the failure point in conjunction with the erosion module, which can more accurately simulate actual complex working conditions, realize the study of the erosion and wear laws of materials under the coupling conditions of complex working conditions, thereby obtaining reasonable and effective experimental data for guiding on-site safety production.
[0024] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 is a schematic diagram of an embodiment of the erosion and wear test equipment of the present invention;
[0027] Figure 2 It is a schematic diagram of an implementation mode of the cooperation between the specimen erosion unit and the multiphase fluid recovery unit in the present invention;
[0028] Figure 3 It is a schematic diagram of an implementation method of the cooperation between the specimen erosion unit and the cooling module in the present invention;
[0029] Figure 4 It is a schematic diagram of another implementation mode of the clamping force application module and the cooling module in the present invention;
[0030] Figure 5 It is a schematic diagram of the cooperation between the main pipeline and the solid phase supply module in the present invention;
[0031] Figure 6 It is a structural schematic diagram of an implementation method of the test piece in the present invention when undergoing vibration fatigue treatment;
[0032] Figure 7It is a structural schematic diagram of an implementation method of the test piece in the present invention when conducting an erosion experiment.
[0033] Description of Reference Numerals
[0034] 10-specimen erosion unit, 11-specimen, 111-temperature probe, 112-clamping hole, 113-erosion area, 12-chuck, 13-force-applying component, 14-tension sensor, 15-workbench, 16-protective cover, 161-horizontal guide rail, 162-erosion chamber, 163-opening, 17-nozzle, 18-arc guide rail, 19-liquid nitrogen tank, 191-cooling box, 20-experimental pipeline, 21-PIV speed measurement module, 22-air compressor, 23-dryer, 24-buffer tank, 25-heater, 26-gas flow meter, 27-check valve, 28-liquid storage tank, 281-agitator, 282-heating component, 29-delivery pump, 30-liquid flowmeter, 31-gas-liquid mixer, 32-main pipeline, 321-negative pressure ejector, 322-negative pressure sand suction pipe, 323-pressure sensor, 324-temperature sensor, 33-side pipeline, 34-solid phase supply module, 341-sand storage tank, 342-uniform speed sand feeder, 343-sand outlet pipe, 35-liquid collecting funnel, 36-sand settling tank, 361-sand baffle, 362-sand discharge port, 37-gas-liquid-solid separator, 371-vent valve, 38-sand collector, 39-liquid return pump, 40-data acquisition and control unit, F1~F15-valves. DETAILED DESCRIPTION
[0035] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0036] In the present invention, unless otherwise stated, directional words such as "upstream, downstream" are usually used with reference to the direction of fluid flow, and directional words "up, down, left, right, front, back" usually refer to the directions shown in the drawings. "Inside" and "outside" refer to the inside and outside relative to the outline of each component itself.
[0037] In one aspect, the present invention provides an erosion and wear test device, comprising:
[0038] A simulated erosion unit, the simulated erosion unit comprising an experimental pipeline 20, the simulated erosion unit being configured to use the experimental pipeline 20 to simulate actual pipeline erosion, so as to determine a failure point of the experimental pipeline 20 and erosion parameters at the failure point;
[0039] A specimen erosion unit 10, the specimen erosion unit 10 comprises a clamping force application module and an erosion module, the clamping force application module is used to clamp the specimen 11 and apply bidirectional tension to the specimen 11 along two vertical axes of the specimen 11, and the erosion module is used to spray a multiphase fluid onto one side surface of the specimen 11 according to the erosion parameters at the failure point to perform erosion; and
[0040] A fluid supply unit is used to supply the simulation erosion unit and the specimen erosion unit 10 with a multiphase fluid for erosion.
[0041] In the above, it can be understood that the specimen 11 has two mutually perpendicular axes, and the clamping force application module can apply tension in opposite directions (i.e., bidirectional tension) to the specimen 11 along one of the axes, and apply tension in opposite directions (i.e., another bidirectional tension) to the specimen 11 along the other axis. In other words, the clamping force application module can apply tension in four different directions to the specimen 11 within the plane where the specimen 11 is located (refer to Figure 7 The test piece 11 is a plate-like piece.
[0042] It should be noted that the magnitude and specific form of the two bidirectional tensile forces can be determined according to actual needs. For example, two bidirectional static tensile loads of different magnitudes can be applied to the specimen 11 through the clamping force application module, and two bidirectional fatigue tensile loads of different magnitudes with a certain frequency and difference can also be applied to the specimen 11.
[0043] During the experiment, a photograph of the failure point of the actual failed pipeline on site can be obtained, and the wall thickness loss law in the erosion and wear process can be calculated through the operation time, the amount of sand-carrying fluid, the amount of sand (i.e., the solid phase particle content) and the pipeline wall thickness loss. Then, the experimental pipeline 20 is used to simulate the actual pipeline erosion, and the failure point (puncture hole or the most severely worn position) and the wall thickness loss law of the experimental pipeline 20 are obtained and compared with the actual failed pipeline on site. The failure point of the experimental pipeline 20 is determined, and the erosion parameters at the failure point are determined, such as the fluid erosion speed at the failure point and the sand content of the fluid actually acting on the failure point; then, the specimen 11 is subjected to load erosion by the specimen erosion unit 10, and the erosion parameters at the failure point determined by the simulated erosion unit are used for erosion, thereby making the erosion experiment more accurate and more in line with actual working conditions.
[0044] It should be noted that during the on-site construction process, the load acting on the pipeline exists in the form of internal pressure, and it is difficult to directly apply a load to the pipeline to simulate the internal pressure of the pipeline during the experiment. Therefore, the test piece 11 that can apply a load is used as the experimental subject, and the internal pressure load of the pipeline is converted into axial tension and annular tension according to the thin-walled cylinder theory. The two bidirectional tensions applied to the test piece 11 along the two perpendicular axes of the test piece 11 are used to simulate the above-mentioned axial tension and annular tension. In addition, the simulated erosion unit is used to provide accurate erosion parameters for the test piece erosion unit 10.
[0045] On the one hand, the erosion and wear test equipment of the present invention simulates the actual pipeline erosion by using the experimental pipeline 20, so as to obtain the failure point of the experimental pipeline 20 and the erosion parameters at the failure point; on the other hand, by applying bidirectional tension to the test piece 11 along the two vertical axes of the test piece 11, the high internal pressure load borne by the pipeline during fracturing construction, backflow, well killing and blowout can be simulated. At the same time, the test piece 11 is subjected to multiphase flow erosion according to the erosion parameters at the failure point in cooperation with the erosion module, which can more accurately simulate the actual complex working conditions, realize the study of the erosion and wear laws of materials under the coupling conditions of complex working conditions, thereby obtaining reasonable and effective experimental data for guiding on-site safety production.
[0046] Specifically, Figure 1 As shown, the simulated erosion unit may include a PIV velocity measurement module 21 and a solid phase particle impact detection module. The PIV velocity measurement module 21 is used to measure the erosion velocity at the failure point of the experimental pipeline 20 during the erosion process of the experimental pipeline 20. The solid phase particle impact detection module is used to measure the number of solid phase particle impacts per unit time at the failure point of the experimental pipeline 20 during the erosion process of the experimental pipeline 20, so as to determine the sand content at the failure point. During the experiment, a solid phase particle impact detection module having an area and shape substantially similar to that of the failure point is installed at the inner wall of the failure point of the experimental pipeline 20 to detect the number of solid phase particles impacting the failure point within a certain period of time, so as to obtain the sand content; a PIV velocity measurement module 21 is set on one side outside the experimental pipeline 20 to detect the actual velocity of the solid phase particles impacting the inner wall of the experimental pipeline 20, so as to obtain the erosion velocity.
[0047] Among them, Figure 1As shown, the experimental pipeline 20 can be a section of elbow pipe. The experimental pipeline 20 can be divided into a metal elbow pipe and a visual fiberglass elbow pipe (made of transparent fiberglass material) according to its function. The metal elbow pipe is a proportional restoration of the actual elbow pipe on site. Its main function is to completely simulate the erosion working condition for the experiment, and to qualitatively determine the failure point by comparing with the failed pipeline on site, and to conduct a preliminary quantitative study on the erosion wear law. The metal elbow pipe is set to be detachable, so as to facilitate the naked eye observation, electronic scanning morphology and measurement of wall thickness (volume) loss after the experiment and compare it with the original state before the experiment; the visual fiberglass elbow pipe is the same size as the metal elbow pipe, and its main function is to cooperate with the PIV velocity measurement module 21 and the solid phase particle impact detection module to determine the precise erosion parameters such as erosion velocity and sand content for the erosion experiment of the specimen erosion unit 10.
[0048] It should be noted that, in the actual process, the liquid flow rate is not necessarily equal to the solid phase particle velocity. The use of the PIV velocity measurement module 21 can determine the actual flow rate of the solid phase particles under the actual working condition liquid flow rate, thereby determining the flow rate of the fluid in the erosion experiment of the specimen erosion unit 10 (i.e., the actual flow rate of the solid phase particles); moreover, in actual field practice, erosion and wear failure must be caused by a point or a small area being worn out, resulting in pipeline perforation. Therefore, it is impossible that all solid phase particles will hit the failure point to cause erosion and wear. The solid phase particle impact detection module is used to determine the number of solid phase particles that hit the failure point within a certain period of time, thereby determining the sand content of the fluid in the erosion experiment of the specimen erosion unit 10.
[0049] In the present invention, the erosion and wear test equipment may further include a vibration fatigue unit, and the vibration fatigue unit is used to perform vibration fatigue treatment on the test piece 11 to simulate the vibration fatigue of the actual working condition of the pipeline.
[0050] During the experiment, the specimen 11 is usually subjected to vibration fatigue treatment before the erosion test. Therefore, the shape of the specimen subjected to vibration fatigue treatment can be different from that of the specimen subjected to erosion test to facilitate the vibration fatigue treatment. For example, during the vibration fatigue treatment, the specimen 11 can be Figure 6 The specimen 11 may be provided with a clamping hole 112 for clamping the specimen; when conducting an erosion test, the specimen treated with vibration fatigue may be cut into Figure 7 The cross-shaped specimen shown or Figure 3 The square specimen shown is used to facilitate clamping, force application and erosion of the specimen.
[0051] In actual field conditions, corrosive media such as hydrogen sulfide may exist in the erosive medium (i.e., multiphase fluid). Therefore, the loss of pipeline materials cannot be entirely caused by erosion and wear, and corrosion may also exist. However, due to the highly toxic nature of the corrosive medium, it cannot be used in the erosion experiment. Therefore, the erosion and wear test equipment may also include a corrosion aging unit, which is used to perform corrosion aging treatment on the specimen 11 to achieve the purpose of simulating the corrosive gas in the erosive medium on site.
[0052] Wherein, the corrosion aging unit may include an alloy steel high temperature and high pressure electrochemical reactor.
[0053] In addition, the erosion and wear test equipment may also include an electrochemical unit for measuring the proportion of corrosion in the material loss of the specimen. In this way, the amount of material loss caused by pure erosion, pure corrosion, and erosion-corrosion coupling in a multiphase fluid erosion environment can be determined, so that the multiphase fluid performance can be adjusted in a targeted manner to prevent the corrosion of the multiphase fluid from exacerbating the erosion and wear rate of the material.
[0054] In the present invention, the fluid supply unit may include a gas phase supply module, a liquid phase supply module, a solid phase supply module 34 and a gas-liquid mixer 31. The solid phase supply module 34 is used to add sand to the sand-carrying fluid supplied by the gas phase supply module and / or the liquid phase supply module to form a multiphase fluid for erosion. The gas-liquid mixer 31 is used to mix the gas supplied by the gas phase supply module and the liquid supplied by the liquid phase supply module when the sand-carrying fluid is a gas-liquid two-phase.
[0055] It should be noted that the sand-carrying fluid may be in gas phase, liquid phase or gas-liquid two-phase. When the sand-carrying fluid is in gas phase or liquid phase, sand (i.e., solid phase particles) may be added directly by the solid phase supply module 34 without passing through the gas-liquid mixer 31; when the sand-carrying fluid is in gas-liquid two-phase, sand may be added by the solid phase supply module 34 after being mixed by the gas-liquid mixer 31.
[0056] In order to achieve the above situation, Figure 1 As shown, the fluid supply unit may include a main pipeline 32, which is connected to the erosion module and the experimental pipeline 20 respectively (for supplying multiphase fluid for erosion to the erosion module and the experimental pipeline 20), and a gas-liquid mixer 31 is arranged on the main pipeline 32. The gas phase supply module, the liquid phase supply module and the solid phase supply module 34 are respectively connected to the main pipeline 32, and the gas phase supply module and the liquid phase supply module are located upstream of the gas-liquid mixer 31, and the solid phase supply module 34 is located downstream of the gas-liquid mixer 31. The fluid supply unit also includes a bypass pipeline 33 connected to the main pipeline 32 and in parallel with the gas-liquid mixer 31, and a valve for controlling the on and off of the bypass pipeline 33 is provided on the bypass pipeline 33.
[0057] During use, when the sand-carrying fluid is in gas phase or liquid phase, the gas-liquid mixer 31 is closed, and the valves F3 and F6 on the side pipe 33 are opened, so that the gas or liquid flows to the downstream of the gas-liquid mixer 31 through the side pipe 33; when the sand-carrying fluid is in gas-liquid two-phase, the gas-liquid mixer 31 is opened, and the valves F3 and F6 on the side pipe 33 are closed, so that the gas and liquid enter the gas-liquid mixer 31 and mix.
[0058] According to an embodiment of the gas phase supply module of the present invention, Figure 1 As shown, the gas phase supply module may include an air compressor 22, a dryer 23, a buffer tank 24 and a heater 25 connected in sequence, the air compressor 22 is used to produce gas, the dryer 23 is used to dry the produced gas, the buffer tank 24 is used to store the dried gas and discharge the gas after regulating the pressure, and the heater 25 is used to heat and control the temperature of the pressure-regulated gas. The gas phase supply module may also include a gas flow meter 26 and a one-way valve 27 located downstream of the heater 25. The gas flow meter 26 is used to measure the flow rate of the gas, and the one-way valve 27 is used to prevent the gas from flowing back. As a result, the gas phase supply module can stably provide gas with a certain flow rate, temperature and pressure.
[0059] The buffer tank 24 has a pressure reducing valve for adjusting the outlet gas pressure. The heater 25 can be any device capable of heating the gas, for example Figure 1 As shown, the heater 25 is a section of heating tube.
[0060] According to an embodiment of the liquid phase supply module of the present invention, Figure 1 As shown, the liquid phase supply module includes a liquid storage tank 28 and a delivery pump 29 which are connected to each other. The liquid storage tank 28 is used to store liquid and includes an agitator 281 capable of stirring the liquid (stirring can prevent the liquid from solidifying) and a heating component 282 for heating the liquid. The delivery pump 29 is used to deliver the liquid in the liquid storage tank 28 at a certain pressure and flow rate.
[0061] Among them, Figure 1 As shown, the liquid phase supply module may further include a liquid flow meter 30 located downstream of the delivery pump 29. The liquid flow meter 30 is used to measure the flow rate of the liquid.
[0062] According to one embodiment of the solid phase supply module of the present invention, Figure 5As shown, the solid phase supply module 34 includes a sand storage tank 341, a uniform speed sand feeder 342 and a sand outlet pipe 343. The outlet of the sand storage tank 341 is connected to the inlet of the uniform speed sand feeder 342, and the outlet of the uniform speed sand feeder 342 is connected to the sand outlet pipe 343. The main pipeline 32 is provided with a negative pressure ejector 321 and a negative pressure sand suction pipe 322 connected to the negative pressure ejector 321. The inlet of the negative pressure sand suction pipe 322 is correspondingly arranged to the outlet of the sand outlet pipe 343, so that the sand discharged from the sand outlet pipe 343 falls into the negative pressure sand suction pipe 322 under the action of gravity and is sucked into the main pipeline 32 by the negative pressure generated by the sand-carrying fluid flowing in the main pipeline 32 in the negative pressure ejector 321 to mix with the sand-carrying fluid to form a multiphase fluid.
[0063] Among them, Figure 5 As shown, the negative pressure ejector 321 is a large diameter pipe section arranged on the main pipeline 32, and the negative pressure sand suction pipe 322 is connected to the negative pressure ejector 321 and is arranged to extend upward from the negative pressure ejector 321. When in use, the solid phase particles in the sand storage tank 341 are discharged downward at a uniform speed through the uniform speed sand feeder 342, and fall into the negative pressure sand suction pipe 322 through the sand outlet pipe 343 under the action of gravity. The high-speed sand-carrying fluid in the main pipeline 32 generates negative pressure when flowing through the negative pressure ejector 321, and the solid phase particles falling into the negative pressure sand suction pipe 322 are sucked into the main pipeline 32 for mixing.
[0064] In the present invention, in order to realize the recycling and reuse of the fluid, the erosion and wear test equipment may further include a fluid recovery unit, and the fluid recovery unit is used to recover the multiphase fluid in the specimen erosion unit 10 and the simulated erosion unit.
[0065] Specifically, Figure 1 and Figure 2 As shown, the fluid recovery unit may include a sand settling tank 36 and a gas-liquid-solid separator 37. The fluid outlets of the specimen erosion unit 10 and the experimental pipeline 20 may be respectively connected to the fluid inlet of the sand settling tank 36. The fluid outlet of the sand settling tank 36 is connected to the fluid inlet of the gas-liquid-solid separator 37. The sand settling tank 36 is used to deposit solid phase particles in the multiphase fluid. The gas-liquid-solid separator 37 is used to separate the multiphase fluid from the sand settling tank 36. The gas-liquid-solid separator 37 has a gas outlet, a liquid outlet and a solid outlet. A vent valve 371 may be provided at the gas outlet of the gas-liquid-solid separator 37. The separated gas may be emptied through the vent valve 371. The liquid outlet of the gas-liquid-solid separator 37 is connected to the liquid storage tank 28 so that the separated liquid enters the liquid storage tank 28 for recycling. A liquid return pump 39 may be provided between the gas-liquid-solid separator 37 and the liquid storage tank 28. The liquid discharged from the gas-liquid-solid separator 37 may be pumped into the liquid storage tank 28 through the liquid return pump 39. The fluid recovery unit may further include a sand collector 38 , and the solid outlet of the gas-liquid-solid separator 37 may be in communication with the sand collector 38 .
[0066] Among them, Figure 1 and Figure 2 As shown, a plurality of sand baffles 361 can be tiltedly arranged in the sand settling tank 36 , the fluid inlet of the sand settling tank 36 is located at the lower part of the sand settling tank 36 , the fluid outlet of the sand settling tank 36 is located at the upper part of the sand settling tank 36 , and a sand discharge port 362 is arranged at the bottom of the sand settling tank 36 .
[0067] During the experiment, the multiphase fluid entering the sand settling tank 36 spreads upward and is finally discharged from the fluid outlet. During this period, a plurality of sand baffles 361 can block some solid particles flowing upward with the liquid flow. Most of the solid particles remain in the sand settling tank 36 under the dual effects of their own gravity and the sand baffles 361.
[0068] The solid phase particles in the sand collector 38 and the sand settling tank 36 can be collected together for particle physicochemical property analysis.
[0069] In the present invention, in order to ensure the smooth application of two bidirectional pulling forces, Figure 7 As shown, the specimen 11 is preferably designed to be cross-shaped, and the central area of the surface of one side of the specimen 11 is formed as an erosion zone 113 (the erosion zone 113 is the core area of the specimen 11, and its function is to withstand the erosion wear of the multiphase fluid while loading the bidirectional tensile load), and the four ends of the specimen 11 are formed as four clamping ends. In order to enhance the firmness and reliability of the specimen clamping, the clamping ends can be provided with clamping holes 112. In this case, the clamping force application module can clamp the four clamping ends respectively and clamp along the two vertical axes (i.e. Figure 7 The horizontal axis and vertical axis shown in the figure apply bidirectional tension to the specimen 11 respectively.
[0070] In the present invention, Figure 2-Figure 4 As shown (it should be noted that Figure 2 and Figure 3 The clamping force-applying components at the front and rear sides and at the upper and lower sides are omitted in the figure respectively), the clamping force-applying module may include four clamps 12 and four force-applying components 13 respectively connected to the four clamps 12, the four clamps 12 are used to clamp the specimen 11 along four vertical directions respectively (for example, clamp four clamping ends), and the four force-applying components 13 are used to apply tension to the four clamps 12 respectively. During the experiment, the clamps 12 clamp the specimen 11 and stretch it outward (i.e., away from the erosion zone 113) to apply a tensile load.
[0071] It should be noted that the clamp 12 and the force-applying component 13 described in the present invention may adopt any appropriate structure as long as they can achieve their functions. For example, the force-applying component 13 may be a hydraulic tensioner, which applies tension to the specimen 11 through hydraulic action; Figure 4As shown, the chuck 12 may include a groove for the clamping end of the specimen 11 to be inserted into and two clamping arms for defining the groove, and the clamping end can be clamped and loosened by the chuck 12 by controlling the distance between the two clamping arms. As for how to control and adjust the distance between the two clamping arms, any known method in the prior art may be adopted, for example, bolts may be provided on the two clamping arms, and the bolts may be controlled by screwing the bolts, and the bolts may pass through the clamping hole 112.
[0072] In addition, the clamping force module may further include four tension sensors 14, which are respectively connected between the four force applying components 13 and the four clamps 12. The four tension sensors 14 are used to monitor the tension load applied to the test piece 11.
[0073] In the present invention, Figure 2 As shown, the specimen erosion unit 10 may also include a workbench 15 and a protective cover 16 whose interior is formed as an erosion chamber 162. The clamping force module, the erosion module and the protective cover 16 are all installed on the workbench 15. The clamping force module is arranged in the erosion chamber 162. The bottom of the protective cover 16 is provided with an opening 163 for the multiphase fluid in the erosion chamber 162 to be discharged. Accordingly, the position of the workbench 15 corresponding to the opening 163 is also formed into an opening shape. By providing the protective cover 16, splashing of liquid flow and solid phase particles can be prevented. In order to facilitate observation of the experiment, the protective cover 16 can be set to be transparent and visible.
[0074] In the above case, if Figure 2 As shown, the fluid recovery unit may also include a liquid collecting funnel 35, which is arranged below the opening 163. The multiphase fluid that impacts the test piece 11 will all fall into the liquid collecting funnel 35. The outlet of the liquid collecting funnel 35 is connected to the fluid inlet of the sand settling tank 36 to pass the collected multiphase fluid into the sand settling tank 36.
[0075] In the present invention, the erosion module includes a nozzle 17, the nozzle 17 is arranged toward the one side surface of the specimen 11, the angle between the spray direction of the nozzle 17 and the one side surface is adjustable, and the distance between the nozzle 17 and the one side surface is adjustable. Through the above arrangement, the erosion angle and erosion distance of the specimen 11 can be adjusted.
[0076] In order to achieve an adjustable angle between the spray direction of the nozzle 17 and the one side surface, according to an embodiment of the present invention, Figure 2As shown, the erosion module may include an arc-shaped guide rail 18, the axial direction (i.e., the front-to-back direction) of the arc-shaped guide rail 18 is parallel to the one side surface (i.e., the left side of the specimen 11), and the nozzle 17 is mounted on the arc-shaped guide rail 18 and can be locked and moved along the arc-shaped guide rail 18 to adjust the angle between the injection direction and the one side surface. That is, in this embodiment, the nozzle 17 is set to be angle-adjustable. In other embodiments, the specimen 11 may also be set to be angle-adjustable.
[0077] Among them, locking of the nozzle 17 on the arc guide rail 18 can be achieved in a variety of ways, for example, using a bolt (or a fixing pin) connecting the nozzle 17 and the arc guide rail 18. When the angle of the nozzle 17 needs to be adjusted, the bolt can be removed, and after the nozzle 17 is moved to the desired angle, the bolt can be installed to fix the nozzle 17 on the arc guide rail 18.
[0078] In order to achieve an adjustable distance between the nozzle 17 and the one side surface, according to an embodiment of the present invention, as Figure 2 As shown, the specimen erosion unit 10 includes a horizontal guide rail 161 (see Figure 2 The clamping force applying module is mounted on the horizontal guide rail 161 and can be locked and moved along the horizontal guide rail 161 to adjust the distance between the one side surface of the specimen 11 and the nozzle 17. That is, in this embodiment, the specimen 11 is configured to be position-adjustable. In other embodiments, the nozzle 17 can also be configured to be position-adjustable.
[0079] The locking of the clamping force application module on the horizontal guide rail 161 can be achieved in a variety of ways, which can be the same as the locking method of the above-mentioned middle nozzle 17 on the arc guide rail 18 .
[0080] In the present invention, in order to realize the installation and movement of the entire clamping and force-applying module on the horizontal guide rail 161, the various components of the clamping and force-applying module can be integrated together through a bracket or a housing to form a whole.
[0081] In some low-temperature construction conditions, the temperature of the pipeline is relatively low, such as carbon dioxide mixed phase fracturing construction, which is an emerging shale oil and gas production increase measure. It is a reservoir transformation process implemented by injecting liquid carbon dioxide and chemicals in a plug-type manner. Its principle is to first increase the formation pressure, dredge the pore channels, open the microcracks, and form a CO2 film to reduce the damage of subsequent water-based fracturing fluids by pre-placing sufficient liquid CO2. Then, a large amount of high-pressure slick water and a high-temperature resistant low-concentration guar fracturing fluid system are used to press open the formation and connect the microcracks to form a complex high-permeability fracture network structure to achieve the purpose of increasing production. Compared with conventional hydraulic fracturing, carbon dioxide mixed phase fracturing adds a carbon dioxide pre-cooling cycle link, which belongs to low-temperature construction (-20℃~-40℃), and its high-pressure manifold erosion failure risk is more serious than conventional hydraulic fracturing. In order to simulate the low-temperature conditions during carbon dioxide mixed phase fracturing, the specimen erosion unit may also include a cooling module, which is configured to be able to cool the specimen 11.
[0082] Specifically, Figure 3 As shown, the cooling module may include a liquid nitrogen tank 19, which is connected to a clamp 12 for clamping the specimen 11 to cool the specimen 11 by delivering liquid nitrogen to the clamp 12. A temperature measuring probe 111 may be provided on the specimen 11 to measure the temperature of the specimen 11.
[0083] In addition, if Figure 4 In the embodiment shown, the cooling module may further include a cooling box 191 , which is connected to the liquid nitrogen tank 19 , and the chuck 12 is passed through the cooling box 191 . The low temperature in the cooling box 191 may be conducted to the specimen 11 through the chuck 12 , thereby achieving cooling of the specimen 11 .
[0084] In the present invention, the connecting pipelines between the various components in the erosion and wear test equipment may be provided with valves for controlling the on-off of the pipelines, such as Figure 1 In addition, in order to facilitate the experiment and improve the efficiency, the erosion wear test equipment may also include a data acquisition and control unit 40, which may be electrically connected to other components in the equipment to realize the operation control of other components, as well as the monitoring and collection of various experimental parameters.
[0085] Another aspect of the present invention provides an erosion wear test method, the method comprising:
[0086] S1. Obtain the failure point, internal pressure and erosion parameters of the actual failed pipeline;
[0087] S2, using a pipeline of the same material as the actual failed pipeline and proportionally reduced as the first experimental pipeline (i.e., the metal elbow mentioned above), simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the failure point of the first experimental pipeline;
[0088] S3, using a section of a visualized pipeline of the same size as the first experimental pipeline as the second experimental pipeline (i.e., the visualized FRP elbow mentioned above), simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the erosion parameters of the second experimental pipeline at the failure point;
[0089] S4. Take the specimen 11 as the experimental subject, apply bidirectional tension to the specimen 11 along the two vertical axes of the specimen 11 to simulate the internal pressure of the pipeline, and spray the erosion medium onto one side surface of the specimen 11 (i.e., the erosion zone 113 mentioned above) according to the erosion parameters at the failure point to perform an erosion experiment.
[0090] In the above, the erosion parameters of the actual failed pipeline include erosion medium (i.e., multiphase fluid) parameters and erosion velocity, wherein the erosion medium parameters include the type and physicochemical properties of the sand-carrying fluid, the type and physicochemical properties of the solid phase particles, and the sand content. The erosion parameters at the failure point of the first experimental pipeline include erosion medium parameters, erosion angle, and erosion velocity, wherein the erosion medium parameters include the type and physicochemical properties of the sand-carrying fluid, the type and physicochemical properties of the solid phase particles, and the sand content.
[0091] For the convenience of description, the erosion parameters of the actual failed pipeline are referred to as actual erosion parameters, and the erosion parameters at the failure point of the first experimental pipeline are referred to as experimental erosion parameters.
[0092] It should be noted that the type and physicochemical properties of the sand-carrying fluid and the type and physicochemical properties of the solid phase particles in the actual erosion parameters are the same as the type and physicochemical properties of the sand-carrying fluid and the type and physicochemical properties of the solid phase particles in the experimental erosion parameters, and the actual erosion rate and the actual sand content are different from the experimental erosion rate and the experimental sand content. Since the specimen 11 is a plane, it needs to be eroded at a certain angle to simulate the erosion direction of the pipeline, so the experimental erosion parameters also include the erosion angle.
[0093] Specifically, the erosion angle of the test piece 11 can be determined according to the erosion angle of the streamline with the largest proportion in the erosion cloud diagram of the second experimental pipeline.
[0094] The experimental erosion rate can be determined according to the erosion rate of the solid phase particles in the experimental erosion medium at the failure point of the second experimental pipeline. The erosion rate of the solid phase particles in the experimental erosion medium at the failure point of the second experimental pipeline can be measured by a PIV velocity measurement module 21 arranged outside the second experimental pipeline (see Figure 1 ).
[0095] The experimental sand content can be determined according to the number of solid phase particles in the experimental erosion medium that impact the failure point of the second experimental pipeline within a certain period of time. The number of solid phase particles in the experimental erosion medium that impact the failure point of the second experimental pipeline within a certain period of time can be measured by a solid phase particle impact detection module that is set at the failure point on the inner wall of the second experimental pipeline and has an area and shape similar to the failure point.
[0096] In the present invention, the method may further include: performing a vibration fatigue treatment on the specimen 11 before S4 to simulate the vibration fatigue working condition of the pipeline; performing a corrosion aging treatment on the specimen 11 before S4 to simulate the corrosion working condition of the pipeline; performing a cooling treatment on the specimen 11 before S4 to simulate the low temperature working condition of the pipeline.
[0097] In the present invention, the erosion medium is a multiphase fluid of gas-solid two-phase, liquid-solid two-phase or gas-liquid-solid three-phase.
[0098] In the present invention, the method may further include: after S4, recovering the erosion medium, separating the liquid in the erosion medium for recycling, and separating the solid phase particles in the erosion medium for particle physicochemical performance analysis.
[0099] The erosion and wear test method of the present invention can be carried out using the above-mentioned erosion and wear test equipment.
[0100] Combine the following Figure 1 The erosion wear test method of the present invention is described in detail, and the method comprises:
[0101] Take photos of the actual failed pipeline in the target work area by taking photos on site to determine the failure point, measure the average internal pressure of the actual failed pipeline, and obtain the actual erosion parameters of the actual failed pipeline;
[0102] Prepare a first experimental pipeline made of the same material as the actual failed pipeline and in a proportionally smaller size (covering the failure point of the actual failed pipeline) and connect it to Figure 1 In the erosion wear test equipment shown;
[0103] Conduct air tightness test on the experimental equipment, specifically open valves F1, F2, F3, F6, start the air compressor 22 and buffer tank 24, stabilize the pressure at 10MPa for 15min and the pressure drop is 0.1MPa, then it is determined to meet the safety experiment requirements;
[0104] Prepare corresponding multiphase fluid according to actual erosion medium parameters (taking the sand-carrying fluid as liquid as an example, the specific operation is: open valves F3-F6, F15, F10, F12, F13, start the delivery pump 29, pump the sand-carrying liquid in the liquid storage tank 28 into the main pipeline 32, open valve F7 and the uniform sand feeder 342, so that the solid phase particles in the sand storage tank 341 are uniformly sucked into the negative pressure ejector 321, observe the liquid flow meter 30 and the sand feeding speed, and wait until the liquid flow rate is stable, the sand output speed is stable, and the liquid and solid phases are evenly mixed), and pass it to the first experimental pipeline at the actual erosion speed to erode the first experimental pipeline, obtain the failure point of the first experimental pipeline, and use CFD software to perform corresponding numerical simulation calculations. When the failure point of the first experimental pipeline coincides with the failure point of the actual failed pipeline and the failure point of the numerical simulation, it is considered that the three are equivalent, thereby determining the failure point of the first experimental pipeline;
[0105] The first experimental pipeline is removed from the equipment, and a second experimental pipeline of the same size and shape as the first experimental pipeline is prepared. A solid phase particle impact detection module with a similar area and shape to the failure point of the first experimental pipeline is set at the inner wall of the second experimental pipeline corresponding to the failure point of the first experimental pipeline. The second experimental pipeline is connected to Figure 1 In the erosion and wear test equipment shown, a PIV velocity measurement module 21 is installed inside the second test pipeline, and the second test pipeline is eroded according to the same erosion parameters as the first test pipeline. The sand content and erosion velocity of the second test pipeline at the failure point are measured by the solid phase particle impact detection module and the PIV velocity measurement module 21 respectively, and the erosion angle is determined by the erosion cloud map of the second test pipeline;
[0106] According to the vibration fatigue and corrosion aging conditions of the actual failed pipeline, the vibration fatigue unit and the corrosion aging unit are used to perform vibration fatigue treatment and corrosion aging treatment on the specimen 11 respectively, and then the specimen 11 is cut into a cross shape for easy clamping and force application;
[0107] According to the thin-walled cylinder theory, the tensile load parameters are determined (the internal pressure of the pipeline is converted into the corresponding annular tensile force and axial tensile force), the specimen 11 is loaded into the clamping force module, and two mutually perpendicular bidirectional tensile loads are applied to the specimen 11;
[0108] According to the above erosion angle, the angle between the spray direction of the nozzle 17 and the erosion area 113 of the test piece 11 is adjusted;
[0109] The corresponding multiphase fluid is prepared according to the experimental sand content, and is sprayed from the nozzle 17 to the erosion area 113 of the test piece 11 at the experimental erosion speed and the above-mentioned erosion angle to carry out the erosion wear experiment.
[0110] During the experiment, a fluid recovery unit can be used to recover the multiphase fluid eroded into the first experimental pipeline, the second experimental pipeline and the test piece 11, and separate it into three phases. The separated gas phase is directly discharged through the vent valve 371, the separated solid phase particles are collected and wait for analysis, and the separated liquid phase is returned to the liquid storage tank 28 through the return pump 39 to continue to participate in the circulation.
[0111] After the experiment, turn off the delivery pump 29 and the liquid return pump 39, open the protective cover 16 after no more fluid flows out of the nozzle 17, remove the tensile load applied to the specimen 11, remove the specimen 11, clean it and wait for analysis; open all valves except F4, F5, F7, F8, and F11, turn on the air compressor 22 and the buffer tank 24 to purge the equipment pipeline to ensure that there is no residual liquid and solid phase.
[0112] When the erosion and wear test method is used to simulate low temperature conditions (such as carbon dioxide mixed phase fracturing construction, the pipeline temperature is -20°C), the above method also includes: before eroding the specimen 11, using a cooling module to reduce the temperature of the specimen 11 to the experimental temperature (-20°C) and maintain it for a period of time (such as 10 hours).
[0113] The erosion and wear test equipment and method of the present invention can simulate the erosion conditions (erosion medium, erosion angle, erosion speed, sand content, temperature) and load conditions (internal pressure fluctuation, vibration fatigue) faced by pipeline equipment in various links of oil and gas field development, and conduct material erosion and wear experiments based on this, so as to facilitate the evaluation and prediction of the reliability and safe service life of on-site pipeline equipment through experimental results and laws, and provide theoretical basis and experimental support for the development of safety assurance technology during large-scale fracturing construction and gas well pressure release, and reduce or even eliminate casualties and property losses directly caused by material pipeline erosion failure. The erosion and wear test equipment and method of the present invention are suitable for the field of safety technology in oil and gas resource development, and can be widely promoted and applied in onshore / offshore oil and gas drilling, large-scale fracturing and other industries, and have high economic and technical value.
[0114] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0115] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0116] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. An erosion wear test method, characterized in that: The method comprises: S1. Obtain the failure point, internal pressure and erosion parameters of the actual failed pipeline; S2, using a pipeline of the same material as the actual failed pipeline and proportionally reduced as the first experimental pipeline, simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the failure point of the first experimental pipeline; S3, using a visual pipeline of the same size as the first experimental pipeline as the second experimental pipeline, simulating pipeline erosion according to the erosion parameters of the actual failed pipeline, and determining the erosion parameters of the second experimental pipeline at the failure point; S4. Take the test piece (11) as the experimental subject, apply bidirectional tension to the test piece (11) along two vertical axes of the test piece (11) to simulate the internal pressure of the pipeline, and spray erosion medium onto one side surface of the test piece (11) according to the erosion parameters at the failure point to perform an erosion experiment.
2. The erosion wear test method according to claim 1, characterized in that: The erosion parameters of the actual failed pipeline include erosion medium parameters and erosion velocity, wherein the erosion medium parameters include the type and physicochemical properties of sand-carrying fluid, the type and physicochemical properties of solid particles, and sand content.
3. The erosion wear test method according to claim 1, characterized in that: The erosion parameters at the failure point include erosion medium parameters, erosion angle and erosion speed, wherein the erosion medium parameters include the type and physicochemical properties of sand-carrying fluid, the type and physicochemical properties of solid particles and sand content.
4. The erosion wear test method according to claim 3, characterized in that: The erosion angle is determined according to the erosion angle of the streamline with the largest proportion in the erosion cloud diagram of the second experimental pipeline.
5. The erosion wear test method according to claim 3, characterized in that: The erosion rate is determined according to the erosion rate of solid phase particles in the erosion medium at the failure point of the second experimental pipeline.
6. The erosion wear test method according to claim 5, characterized in that: The erosion velocity of the solid phase particles in the erosion medium at the failure point of the second experimental pipeline is measured by a PIV velocity measurement module (21) arranged outside the second experimental pipeline.
7. The erosion wear test method according to claim 3, characterized in that: The sand content is determined according to the number of solid particles in the erosion medium that impact the failure point of the second experimental pipeline within a certain period of time.
8. The erosion wear test method according to claim 7, characterized in that: The number of solid particles in the erosion medium that impact the failure point of the second experimental pipeline within a certain period of time is measured by a solid particle impact detection module that is arranged at the failure point on the inner wall of the second experimental pipeline and has an area and shape similar to the failure point.
9. The erosion wear test method according to any one of claims 1 to 8, characterized in that: The method comprises: before S4, performing vibration fatigue treatment on the test piece (11).
10. The erosion wear test method according to any one of claims 1 to 8, characterized in that: The method comprises: before S4, performing corrosion aging treatment on the test piece (11).
11. The erosion wear test method according to any one of claims 1 to 8, characterized in that: The method comprises: before S4, the test piece (11) is subjected to a temperature reduction treatment.
12. The erosion wear test method according to any one of claims 1 to 8, characterized in that: The erosion medium is a multiphase fluid of gas-solid two-phase, liquid-solid two-phase or gas-liquid-solid three-phase.
13. The erosion wear test method according to any one of claims 1 to 8, characterized in that: The method comprises: after S4, recovering the erosion medium, separating the liquid in the erosion medium for recycling, and separating the solid phase particles in the erosion medium for particle physicochemical performance analysis.