A method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials

By mixing and alkali-thermal activating solid waste raw materials, a linear prediction model was established, which solved the problem of the difficulty in predicting the active silicon-aluminum ratio of solid waste raw materials, and realized efficient and economical prediction of the active silicon-aluminum ratio and guidance for geopolymer preparation.

CN114113183BActive Publication Date: 2024-11-12WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111356972.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-16
Publication Date
2024-11-12
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

In existing technologies, the complex composition of solid waste raw materials and the low content of active silicon and aluminum components lead to technical problems that make it difficult to effectively predict and promote the preparation of geopolymers.

Method used

By obtaining at least two silicon-aluminum raw materials, mixing them and performing alkaline thermal activation treatment, a linear prediction model for the molar ratio of silicon-aluminum in the raw materials and the molar ratio of active silicon-aluminum is established. The linear equation is then used to fit and predict the active silicon-aluminum ratio under different ratios.

Benefits of technology

It enables efficient prediction of the active silicon-aluminum ratio in solid waste raw materials, simplifies the operation process, reduces testing costs, has a wide range of applications, and shows significant fitting effect, thus guiding the preparation process of geopolymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114113183B_ABST
    Figure CN114113183B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for predicting the active silicon-aluminum ratio of alkali-heat activated geopolymer raw materials, comprising the following steps: determining the silicon content and aluminum content in the silicon-aluminum raw materials; mixing the silicon-aluminum raw materials in different proportions to obtain n groups of mixed raw materials, and calculating the raw material silicon-aluminum molar ratio of the n groups of mixed raw materials; subjecting the mixed raw materials to alkali-heat activation treatment to obtain activated materials, and testing the raw material active silicon-aluminum content in the activated materials, and calculating the raw material active silicon-aluminum molar ratio of the n groups of mixed raw materials; establishing a prediction model of the raw material silicon-aluminum molar ratio and the raw material active silicon-aluminum molar ratio; predicting the raw material active silicon-aluminum molar ratio of the silicon-aluminum raw materials at different proportions according to a linear equation. The method for predicting the active silicon-aluminum ratio of alkali-heat activated geopolymer raw materials proposed by the present invention can be applied to various raw materials for preparing geopolymers, has a simple operation process, is convenient to operate, is economical and efficient, has a wide range of applications, and has great guiding value for the alkali activation treatment of raw materials and the geopolymer preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of geopolymer preparation, and in particular to a method for predicting the active silicon-aluminum ratio of alkali-heat-activated geopolymer raw materials. Background Art

[0002] Geopolymers are new inorganic polymer materials synthesized by the reaction between aluminosilicates and alkali metal compounds at or near ambient temperature. They are considered to be the third generation of cement after lime and ordinary Portland cement. Due to their simple production process, low environmental impact, excellent mechanical properties, durability, high temperature resistance, and ability to solidify heavy metal ions, they are used as a fast emerging material for various building materials, refractory ceramics, composite materials, matrices for fixing toxic wastes, and many other materials.

[0003] Natural mineral raw materials such as kaolin are widely used as raw materials for the preparation of geopolymers. In recent years, the research focus of raw materials for the preparation of geopolymers has shifted from pure natural materials to waste materials and by-products (such as fly ash, metallurgical slag, mining waste, etc.) for environmental protection and economic benefits.

[0004] The process of geopolymer formation is controlled by many internal and external parameters, and the silicon-aluminum component in the material is a major factor affecting its structure and performance. The silicon-aluminum component will affect the type and quantity of the generated silicon-aluminum gel product, and thus affect the structure and performance of the geopolymer. For natural high silicon-aluminum active metakaolin, the reactive silicon-aluminum component is not much different from the silicon-aluminum component in the material. However, for solid waste raw materials, the wide range of sources leads to the heterogeneity of silicon-aluminum raw materials, and the silicon-aluminum components therein are often less reactive. Therefore, how to predict and calculate the active silicon-aluminum ratio in low silicon-aluminum active raw materials is an important issue that needs to be solved in the later preparation and promotion of geopolymers. Summary of the invention

[0005] In view of this, it is necessary to provide a method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials, so as to solve the technical problems in the prior art that the solid waste raw materials have complex compositions, low content of active silicon-aluminum components, and difficulty in promoting the preparation of geopolymers from different solid waste raw materials.

[0006] The present invention provides a method for predicting the active silicon-aluminum ratio of an alkali-heat-activated geopolymer raw material, comprising the following steps:

[0007] Obtain at least two silicon-aluminum raw materials, and determine the silicon content and aluminum content of each silicon-aluminum raw material;

[0008] Mix at least two silicon and aluminum raw materials in different proportions to obtain n groups of mixed raw materials, and calculate the raw material silicon and aluminum molar ratios of the n groups of mixed raw materials, which are recorded as M1, M2, M3...Mn;

[0009] The mixed raw materials are subjected to alkali heat activation treatment to obtain activated materials, and the raw material active silicon and aluminum contents in the activated materials are tested to calculate the raw material active silicon and aluminum molar ratios of n groups of mixed raw materials, which are recorded as N1, N2, N3...Nn;

[0010] Establish a prediction model of MN for the raw material silicon-aluminum molar ratio and the raw material active silicon-aluminum molar ratio, and perform linear equation fitting on M1, M2, M3...Mn and the corresponding N1, N2, N3...Nn;

[0011] The active silicon-aluminum molar ratio of the raw materials at different ratios of the at least two silicon-aluminum raw materials is predicted according to the linear equation.

[0012] Compared with the prior art, the present invention has the following beneficial effects:

[0013] The method for predicting the active silicon-aluminum ratio of alkali-heat-activated geopolymer raw materials proposed in the present invention can effectively establish a prediction model for the active silicon-aluminum ratio of the raw materials through only a small amount of sampling tests, and can be applied to various raw materials for preparing geopolymers. The operation process is simple and convenient, and the subsequent large amount of test calculation costs and procedures can be omitted. It is economical and efficient, and has a wide range of applications.

[0014] The active silicon-aluminum ratio prediction model and the corresponding linear equation proposed in the present invention have high goodness of fit and significant fitting effect, and have great guiding value for the alkali activation treatment of raw materials and the preparation process of geopolymers. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The relationship between the raw material silicon-aluminum molar ratio M and the active silicon-aluminum molar ratio N and the linear fitting equation of Example 1 of the present invention;

[0016] Figure 2 The relationship between the raw material silicon-aluminum molar ratio M and the active silicon-aluminum molar ratio N and the linear fitting equation of Example 2 of the present invention;

[0017] Figure 3 It is the relationship between the raw material silicon-aluminum molar ratio M and the active silicon-aluminum molar ratio N and the linear fitting equation of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0019] The present invention provides a method for predicting the active silicon-aluminum ratio of an alkali-heat-activated geopolymer raw material, comprising the following steps:

[0020] S1. Obtain at least two silicon-aluminum raw materials, and determine the silicon content and aluminum content in each of the silicon-aluminum raw materials;

[0021] S2, mixing the at least two silicon-aluminum raw materials mentioned above in different proportions to obtain n groups of mixed raw materials, and calculating the raw material silicon-aluminum molar ratios of the n groups of mixed raw materials, recorded as M1, M2, M3...Mn;

[0022] S3, subjecting the mixed raw materials to alkali heat activation treatment to obtain activated materials, and testing the raw material active silicon and aluminum content in the activated materials, and calculating the raw material active silicon and aluminum molar ratios of n groups of mixed raw materials, recorded as N1, N2, N3...Nn;

[0023] S4, establish a prediction model MN of the raw material silicon-aluminum molar ratio and the raw material active silicon-aluminum molar ratio, and perform linear equation fitting on M1, M2, M3...Mn and the corresponding N1, N2, N3...Nn, and the fitting equation is y=A+B*x;

[0024] S5. Predicting the active silicon-aluminum molar ratio of the at least two silicon-aluminum raw materials at different proportions based on the linear equation.

[0025] In the present invention, the silicon-aluminum raw material in step S1 includes solid waste silicon-aluminum raw materials. Further, the solid waste silicon-aluminum raw materials include at least two of fly ash, shale vanadium extraction tailings, silica ash, blast furnace slag, granite powder, limestone powder, and sludge.

[0026] In the present invention, the silicon-aluminum raw material in step S1 also includes a natural silicon-aluminum raw material. Further, the natural silicon-aluminum raw material can be metakaolin or the like.

[0027] In some specific embodiments of the present invention, three different silicon-aluminum raw materials are selected to prepare the mixed raw material.

[0028] In the present invention, in step S1, the chemical composition of the silicon-aluminum raw material is tested by an X-ray fluorescence spectrometer to obtain the mass fraction of the silicon and aluminum components of the silicon-aluminum raw material, and the corresponding silicon content and aluminum content are calculated.

[0029] In the present invention, in step S2, n is greater than 4, preferably 4-20, and more preferably 6-10.

[0030] In the present invention, the alkali used for alkali thermal activation in step S3 is sodium hydroxide or potassium hydroxide, and the mass ratio of the alkali to the mixed material is 5% to 40%, further 10% to 30%, and further 15% to 25%.

[0031] In the present invention, the temperature of the alkali thermal activation in step S3 is 350°C to 750°C, further 500°C to 600°C, further 550°C to 600°C; the time of the alkali thermal activation is 0.5 to 4h, further 1 to 3h, further 1 to 2h.

[0032] In the present invention, the step S3 of testing the raw material active silicon and aluminum content in the activated material includes: taking the activated material and fully stirring it in an alkaline solution to obtain a turbid liquid, filtering the turbid liquid to obtain a filtrate and a filter residue, and testing the active molar silicon and aluminum content in the filtrate to determine the raw material active silicon and aluminum content in the activated material.

[0033] In some preferred embodiments of the present invention, the liquid-solid ratio of the alkaline solution to the activated material is 10:1 to 100:1 mL / g, further 40:1 to 60:1 mL / g, further 45:1 to 50:1 mL / g; the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution, and the concentration of the alkaline solution is 2 mol / L to 10 mol / L, further 6 mol / L to 8 mol / L; the stirring rate is 150 to 300 rpm, further 200 to 250 rpm; the stirring time is 1 to 3 h, further 2 to 3 h.

[0034] In some more preferred embodiments of the present invention, testing the active molar content of silicon and aluminum in the filtrate includes: after the filtrate is fixed to a certain volume to obtain a fixed volume solution, testing the active molar content of silicon and aluminum in the fixed volume solution, and finally determining the active molar content of silicon and aluminum in the filtrate. In this process, the ratio of the fixed volume to the activated material is 200:1 to 1000:1 mL / g, further 500:1 to 1000:1 mL / g, and further 750:1 to 1000:1 mL / g.

[0035] In the present invention, in step S4, y represents the molar ratio of active silicon to aluminum, x represents the molar ratio of raw silicon to aluminum, A and B are constants, and R 2 is the goodness of fit of the equation, R 2 The closer the value is to 1, the better the fit.

[0036] In the present invention, in step S5, predicting the raw material active silicon-aluminum molar ratio of at least two silicon-aluminum raw materials in different proportions according to the linear equation includes: calculating the raw material silicon-aluminum molar ratio of the mixed raw material in any proportion of the above-mentioned at least two silicon-aluminum raw materials, and substituting it into the fitting equation to calculate the corresponding active raw material silicon-aluminum molar ratio.

[0037] Example 1

[0038] A method for predicting the active silicon-aluminum ratio of an alkali-heat-activated geopolymer raw material comprises the following steps:

[0039] (1) The chemical composition of shale vanadium extraction tailings, fly ash, and silica fume was tested using an X-ray fluorescence spectrometer to obtain the mass fraction of silicon and aluminum in the silicon and aluminum raw materials. The results are shown in Table 1;

[0040] (2) The mass ratios of the three raw materials were 100:0:4, 90:10:4, 80:20:4, 70:30:4, 60:40:4, and 50:50:4 to obtain 6 groups of mixed raw materials, and the molar ratios of silicon and aluminum of the 6 groups of mixed raw materials were calculated respectively, which were recorded as M1, M2, M3, M4, M5, and M6. The results are shown in Table 2;

[0041] (3) The above 6 groups of mixed raw materials were mixed and stirred evenly with NaOH accounting for 25% of the mass of each group of mixed raw materials, and then subjected to alkaline heat activation treatment at 550°C for 1 hour. After cooling at room temperature, an activated material was obtained; 1 g of the activated material was stirred in 50 mL of a 6 mol / L NaOH solution at room temperature for 2 hours at a stirring speed of 200 rpm to obtain a turbid liquid; the turbid liquid was filtered to obtain a filtrate and a filter residue, and the filtrate was fixed to a volume to obtain 1000 mL of a fixed volume solution, and the active molar silicon-aluminum content in the fixed volume solution was tested, and the silicon-aluminum molar ratio of the active raw material was recorded as N1, N2, N3, N4, N5, and N6. The results are shown in Table 2;

[0042] (4) A prediction model MN for the molar ratio of silicon to aluminum in the raw material and the molar ratio of silicon to aluminum in the active raw material was established, and a linear equation was fitted for M1, M2, M3, M4, M5, M6 and the corresponding N1, N2, N3, N4, N5, N6. The fitting equation was y = A + B*x, and the experimental fitting equation was solved to obtain y = 1.20 + 0.90x.

[0043] (5) Calculate the raw material silicon-aluminum molar ratio of the mixed raw material at any ratio of the above three raw materials, and substitute it into the fitting equation to calculate the corresponding active raw material silicon-aluminum molar ratio.

[0044] See also Figure 1 In the fitting equation obtained by this embodiment, R 2 The value is 0.994, and the goodness of fit is good, indicating that this method can well predict the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials.

[0045] Table 1 Chemical composition of shale vanadium extraction tailings, fly ash and silica fume in Example 1

[0046]

[0047] Table 2 The mass ratio of tailings, fly ash and silica ash in Example 1 and the molar ratio of raw silicon and aluminum and the molar ratio of active silicon and aluminum

[0048]

[0049] Example 2

[0050] A method for predicting the active silicon-aluminum ratio of an alkali-heat-activated geopolymer raw material comprises the following steps:

[0051] (1) The chemical composition of fly ash, granite powder and sludge was tested using an X-ray fluorescence spectrometer to obtain the mass fraction of silicon and aluminum in the silicon and aluminum raw materials. The results are shown in Table 3;

[0052] (2) The mass ratios of the three raw materials are 80:10:10, 60:20:20, 40:30:30, 20:40:40, 40:50:10, 20:60:20, 20:70:10, and 10:80:10 to obtain 8 groups of mixed raw materials, and the molar ratios of silicon and aluminum of the 8 groups of mixed raw materials are calculated, which are recorded as M1, M2, M3, M4, M5, M6, M7, and M8. The results are shown in Table 4;

[0053] (3) The above 8 groups of mixed raw materials were mixed and stirred evenly with NaOH accounting for 15% of the mass of each group of mixed raw materials, and subjected to alkaline heat activation treatment at 600°C for 2h. After cooling at room temperature, an activated material was obtained. 2g of the activated material was stirred in 90mL of 8mol / L NaOH solution at room temperature for 3h at a stirring speed of 250rpm / min to obtain a turbid liquid. The turbid liquid was filtered to obtain a filtrate and a filter residue. The filtrate was fixed to volume to obtain 1500mL of a fixed volume solution. The molar content of active silicon and aluminum in the fixed volume solution was tested, and the molar ratio of silicon and aluminum in the active raw material was recorded as N1, N2, N3, N4, N5, N6, N7, and N8. The results are shown in Table 4.

[0054] (4) A prediction model MN for the molar ratio of silicon to aluminum in the raw material and the molar ratio of silicon to aluminum in the active raw material was established, and a linear equation was fitted for M1, M2, M3, M4, M5, M6, M7, M8 and the corresponding N1, N2, N3, N4, N5, N6, N7, N8. The fitting equation was y = A + B*x, and the experimental fitting equation was solved to obtain y = 1.09 + 0.73x.

[0055] (5) Calculate the raw material silicon-aluminum molar ratio of the mixed raw material at any ratio of the above three raw materials, and substitute it into the fitting equation to calculate the corresponding active raw material silicon-aluminum molar ratio.

[0056] See also Figure 2 In the fitting equation obtained by this embodiment, R 2 The value is 0.992, and the goodness of fit is good, indicating that this method can well predict the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials.

[0057] Table 3 Chemical composition of fly ash, granite powder and sludge in Example 2

[0058]

[0059] Table 4 Raw material silicon-aluminum molar ratio and active silicon-aluminum molar ratio of fly ash, granite powder and sludge in Example 2

[0060]

[0061] Comparative Example 1

[0062] Except that the alkaline heat activation treatment at 550°C for 1h in step (3) of Example 1 is replaced by mechanical activation, the rest is the same as Example 1. The replaced step (3) is: the above 6 groups of mixed raw materials are placed in a ball mill, the material filling rate of the ball mill is 33%, and the ball milling time is 2h; 1g of the activated material is stirred in 50mL of 6mol / L NaOH solution at room temperature for 2h, the stirring speed is 200rpm, and a turbid liquid is obtained after stirring; the turbid liquid is filtered to obtain a filtrate and a filter residue, the filtrate is fixed to a volume to obtain 1000mL of a fixed volume solution, the active molar silicon-aluminum content in the fixed volume solution is tested, and the silicon-aluminum molar ratio of the active raw material is recorded as N1, N2, N3, N4, N5, and N6. The results are shown in Table 5.

[0063] See also Figure 3 The fitting equation obtained in this embodiment is solved to obtain y=-13.52+4.15x, where R 2 The value is 0.784, and the goodness of fit is poor, indicating that this method cannot be used to predict the active Si-Al ratio of mechanically activated geopolymer raw materials.

[0064] Table 5 The mass ratio of tailings, fly ash and silica ash in comparative example 1 and the molar ratio of raw silicon and aluminum and the molar ratio of active silicon and aluminum

[0065]

[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for predicting the active silicon-aluminum ratio of an alkali-thermal activated geopolymer raw material, characterized in that: The following steps are involved: Obtaining at least two silicon-aluminum raw materials, and determining the silicon content and aluminum content of each of the silicon-aluminum raw materials; Mixing the at least two silicon and aluminum raw materials in different proportions to obtain n groups of mixed raw materials, and calculating the raw material silicon and aluminum molar ratios of the n groups of mixed raw materials, which are recorded as M1, M2, M3...Mn; The mixed raw materials are subjected to alkali heat activation treatment to obtain activated materials, and the raw material active silicon and aluminum contents in the activated materials are tested to calculate the raw material active silicon and aluminum molar ratios of n groups of mixed raw materials, which are recorded as N1, N2, N3...Nn; Establishing a prediction model for the raw material silicon-aluminum molar ratio and the raw material active silicon-aluminum molar ratio MN, and performing linear equation fitting on M1, M2, M3...Mn and the corresponding N1, N2, N3...Nn; The active silicon-aluminum molar ratio of the at least two silicon-aluminum raw materials at different ratios is predicted according to the linear equation; wherein, Testing the raw material active silicon and aluminum content in the activated material includes: taking the activated material and fully stirring it in an alkaline solution to obtain a turbid liquid, filtering the turbid liquid to obtain a filtrate and a filter residue, and testing the active molar silicon and aluminum content in the filtrate to determine the raw material active silicon and aluminum content in the activated material.

2. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 1, characterized in that: The silicon-aluminum raw materials include solid waste silicon-aluminum raw materials.

3. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 2, characterized in that: The solid waste silicon-aluminum raw materials include at least two of fly ash, shale vanadium extraction tailings, silicon ash, blast furnace slag, granite powder, limestone powder, and sludge.

4. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 1, characterized in that: The silicon-aluminum raw material also includes natural silicon-aluminum raw material.

5. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 1, characterized in that: The silicon content and aluminum content in the silicon-aluminum raw material are obtained by testing the chemical composition of the silicon-aluminum raw material using an X-ray fluorescence spectrometer.

6. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 1, characterized in that: The alkali used for alkali thermal activation is sodium hydroxide or potassium hydroxide, and the mass ratio of the alkali to the mixed material is 5% to 40%; the temperature of the alkali thermal activation is 350° C. to 750° C., and the time of the alkali thermal activation is 0.5 to 4 h.

7. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw material according to claim 1, characterized in that: The liquid-solid ratio of the alkaline solution to the activated material is 10:1 to 100:1 mL / g, the alkaline solution is a sodium hydroxide solution or a potassium hydroxide solution, the concentration of the alkaline solution is 2 mol / L to 10 mol / L, and the stirring time is 1 to 3 h.

8. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw materials according to claim 1, characterized in that: Testing the active molar content of silicon and aluminum in the filtrate includes: adjusting the filtrate to a certain volume to obtain a fixed volume solution and testing the active molar content of silicon and aluminum in the fixed volume solution, and finally determining the active molar content of silicon and aluminum in the filtrate.

9. The method for predicting the active silicon-aluminum ratio of alkali-thermal activated geopolymer raw material according to claim 8, characterized in that: The ratio of the fixed volume to the activated material is 200:1 to 1000:1 mL / g.