Transition Metal Chelated Polyol Blends for Polyurethane Polymers

By introducing liquid transition metal chelated polyol blends into polyurethane materials, the problem of smoke and toxic gas emissions during the combustion process of polyurethane materials has been solved, resulting in polyurethane foam with low smoke and high thermal stability, suitable for building insulation and other applications.

CN114127144BActive Publication Date: 2024-11-22DOW GLOBAL TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080049778.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-08
Publication Date
2024-11-22
Estimated Expiration
2040-07-08

AI Technical Summary

Technical Problem

Existing polyurethane materials emit a lot of smoke and toxic gases during combustion, and traditional flame retardants may increase smoke opacity, so it is necessary to improve combustion performance and reduce smoke toxicity.

Method used

Polyurethane polymers are formed by using liquid transition metal chelate polyol blends and isocyanate reactive compositions. By adding transition metal ions and nitrogen-based chelating agents, the reaction ratio and composition are optimized to form polyurethane foams with improved smoke performance.

Benefits of technology

It significantly reduces HCN and CO emissions, improves the thermal stability and low-smoke properties of polyurethane foam, while maintaining or improving other properties such as antifungal, antimicrobial, odor-resistant, and frictional resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003459809210000121
    Figure BDA0003459809210000121
  • Figure BDA0003459809210000281
    Figure BDA0003459809210000281
  • Figure BDA0003459809210000291
    Figure BDA0003459809210000291
Patent Text Reader

Abstract

The present disclosure provides a liquid transition metal chelate polyol blend, which can be used in an isocyanate reactive composition and a reaction mixture to form a polyurethane polymer. The liquid transition metal chelate polyol blend comprises a polyol, a transition metal compound having a transition metal ion, and a chelating agent having a nitrogen-based chelating portion, wherein the molar ratio of nitrogen in the nitrogen-based chelating portion of the liquid transition metal chelate polyol blend to the transition metal ion is 8:1 to 1:1 (nitrogen mole: transition metal ion mole).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to a polyurethane polymer, and more particularly to a polyurethane polymer having improved burning / smoke properties. Background Art

[0002] Since the 1960s, polyurethane rigid (PUR) foam has been used in construction as a high-performance insulation material. Continuous technological development in Europe and the United States has given rise to a next-generation product called polyisocyanurate rigid (PIR) foam. Both PUR and PIR are polyurethane polymers made from two reactants, isocyanates (e.g., diphenyl methyl diisocyanate, MDI) and polyols. While for PUR, isocyanates and polyols are implemented in a balanced ratio equivalent to equivalent weights, excess isocyanates are used in the production process of PIR. The isocyanate part reacts with itself, and the resulting PIR is a highly cross-linked synthetic material with a cyclic isocyanurate structure. The high degree of bonding and the ring structure ensure the high thermal stability of rigid PIR foam. PIR also has excellent thermal stability and dimensional stability.

[0003] PIR foams are also characterized by very good fire resistance due to the inherent charring properties, which in turn is related to the excellent thermal stability of the isocyanurate chemical structure. To further enhance the char formation, phosphorus-based flame retardants are usually added. When building products such as insulating transition metal panels or insulating boards are exposed to fire, the insulating PIR core quickly forms an adherent char that helps protect the underlying materials. This means that only a limited portion of the available combustible insulation materials are exposed to the fire, and these materials actually contribute to the release of heat and smoke.

[0004] The combustion performance of combustible thermosets is a complex issue. For example, halogenated flame retardants are very effective in reducing heat release, but may worsen opacity. Dow patent publication US 2014 / 0206786 A1 describes the use of triethyl phosphate (TEP) as a smoke suppression additive compared to traditional halogenated flame retardants such as tris(2-chloroisopropyl) phosphate (TCPP). In addition, it is well known that the composition of combustion effluents (in addition to the materials themselves) depends largely on the fire conditions, particularly temperature, geometry and ventilation, including the availability of oxygen. Even though, as described above, the inherent charring properties of polyisocyanurates limit and / or delay the amount of polymer combustion (thereby limiting and / or delaying the release of heat and smoke), there is still a need to further improve the combustion / burning performance and thereby reduce opacity and smoke toxicity as much as possible.

[0005] Polyurethanes are also widely used in many coatings, adhesives, sealants and elastomers ("CASE") applications and in flexible polyurethane foams. There is a need to further improve combustion performance and thereby minimize smoke opacity and smoke toxicity, and optionally improve other properties of polyurethanes used as coatings, adhesives, sealants, elastomers and flexible foams, such as antifungal, antimicrobial, anti-odor, hardness, sound insulation and friction resistance. Summary of the invention

[0006] The present disclosure provides a liquid transition metal chelated polyol blend that can be used in isocyanate reactive compositions and reaction mixtures containing isocyanate reactive compositions for forming polyurethane polymers. The polyurethane polymers and polyurethane polymer foams of the present disclosure can have improved smoke performance with respect to the emission of hydrogen cyanide (HCN) and carbon monoxide (CO) during a pyrolysis event (e.g., a fire).

[0007] The liquid transition metal chelate polyol blend of the present disclosure comprises a polyol, a transition metal compound having a transition metal ion, and a chelating agent having a nitrogen-based chelating moiety, wherein the transition metal ion from the transition metal compound is present in an amount of 0.05 weight percent (wt.%) to 10.0 wt.%, the wt.% being based on the total weight of the liquid transition metal chelate polyol blend, and wherein the liquid transition metal chelate polyol blend has 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 grams (g) of the polyol in the liquid transition metal chelate polyol blend, and the molar ratio of nitrogen in the nitrogen-based chelating moiety to transition metal ion is 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 grams (g) of the polyol in the liquid transition metal chelate polyol blend. The molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is preferably 8.0:1.0 to 1.0:1.0 (molar number of nitrogen: molar number of transition metal ions), wherein for each embodiment, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is preferably 4.0:1.0 to 1.0:1.0 (molar number of nitrogen: molar number of transition metal ions), more preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.8:1.0 to 1.0:1.0 (molar number of nitrogen: molar number of transition metal ions), and most preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.0:1.0 to 1.0:1.0 (molar number of nitrogen: molar number of transition metal ions). In various embodiments, the chelating agent is soluble in the polyol of the transition metal chelate polyol blend, wherein the liquid transition metal chelate polyol blend has 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, preferably 0.003 to 0.60 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, more preferably 0.006 to 0.40 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, and most preferably 0.01 to 0.20 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend.

[0008] In various embodiments, the polyol is an aromatic polyester polyol having an aromatic portion, the aromatic portion accounting for 5 weight percent (wt.%) to 60 wt.% of the total weight of the aromatic polyester polyol. In various embodiments, the polyester polyol is preferably an aromatic polyester polyol having an aromatic portion, the aromatic portion accounting for 10 wt.% to 40 wt.% of the total weight of the aromatic polyester polyol. In various embodiments, the polyester polyol is most preferably an aromatic polyester polyol having an aromatic portion, the aromatic portion accounting for 10 wt.% to 20 wt.% of the total weight of the aromatic polyester polyol.

[0009] For embodiments, the transition metal compound is selected from the group consisting of: transition metal carboxylates, transition metal salts, transition metal coordination compounds and combinations thereof. Preferably, the transition metal compound is a transition metal carboxylate. The transition metal ion is selected from the group consisting of: copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, cadmium, mercury, palladium, titanium, vanadium and combinations thereof. More preferably, the transition metal ion is selected from the group consisting of: copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium and combinations thereof. Most preferably, the transition metal ion is selected from the group consisting of: copper, zinc, iron, manganese, cobalt, nickel and combinations thereof. For embodiments, the transition metal compound may be selected from the group consisting of: 2-ethylhexanoic acid copper (II) (CuEH), copper (I) acetate, copper (II) acetate, copper (II) acetate monohydrate (Cu (OAc) 2H 2 O), copper (II) propionate, copper (II) isobutyrate (Cu (i-Bu) 2), cobalt (II) acetate, nickel (II) acetate, silver (I) acetate and combinations thereof.

[0010] For an embodiment, the chelating agent having a nitrogen-based chelating moiety is selected from the group consisting of a diamine chelating moiety, a triamine chelating moiety, a tetraamine chelating moiety, and combinations thereof. Preferably, the chelating agent having a nitrogen-based chelating moiety is selected from the group consisting of 2,2'-bipyridine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N',N"-pentamethyldiethylenetriamine, 2-[[2-(dimethylamino)ethyl]methylamino]ethanol, 1-[bis[3-(dimethylamino)propyl]amino-2-propanol], 1,2-ethylenediamine polymers with methyloxirane, and combinations thereof.

[0011] The present disclosure also provides an isocyanate reactive composition, which includes a liquid transition metal chelate polyol blend as provided herein, wherein the isocyanate reactive composition can be used to form a polyurethane polymer. For each embodiment, the isocyanate reactive composition may also include a polyol separated from the polyol in the liquid transition metal chelate polyol blend, wherein the isocyanate reactive composition includes 0.1 to 100 weight percent (wt.%) of the liquid transition metal chelate polyol blend and up to 99.9% of the polyol separated from the polyol of the liquid transition metal chelate polyol blend, to form an isocyanate reactive composition for polyurethane polymers, wt.% is based on the gross weight of the isocyanate reactive composition. In another embodiment, the isocyanate reactive composition of the present disclosure may optionally include a polyol (separated from the polyol in the liquid transition metal chelate polyol blend), a phosphorus flame retardant, a catalyst, a blowing agent, water, a surfactant or a combination thereof, wherein the isocyanate reactive composition can be used to form a polyurethane polymer foam. For example, an isocyanate-reactive composition as provided herein may include a blowing agent and a surfactant for forming a polyurethane polymer foam.

[0012] For each embodiment, the isocyanate reactive composition of the present disclosure may also include 0.1wt.% to 7.0wt.% phosphorus from a flame retardant compound, the flame retardant compound is preferably a halogen-free flame retardant compound, selected from the group consisting of phosphate, phosphonate, phosphinate, phosphite and a combination thereof, the wt.% of phosphorus is based on the gross weight of the isocyanate reactive composition. For each embodiment, the isocyanate reactive composition of the present disclosure includes 0.05wt.% to 10.0wt.% transition metal from a liquid transition metal chelate polyol blend, wherein the wt.% of the transition metal ion is based on the gross weight of the liquid transition metal chelate polyol blend. For such embodiments, the molar ratio of the transition metal ion to phosphorus of the isocyanate reactive composition (moles of transition metal ions: moles of phosphorus) is 0.05:1 to 5:1.

[0013] Embodiments of the present disclosure also provide a reaction mixture for forming a polyurethane polymer, wherein the reaction mixture comprises an isocyanate compound having an isocyanate moiety and an isocyanate reactive composition as provided herein, wherein the polyol comprises a hydroxyl moiety, and the molar ratio of the isocyanate moiety to the hydroxyl moiety of the reaction mixture is 0.90: 1 to 7: 1. In further embodiments, the reaction mixture can be used to form a polyurethane polymer foam, wherein the reaction mixture comprises an isocyanate compound having an isocyanate moiety and an isocyanate reactive composition as provided herein, wherein the polyol comprises a hydroxyl moiety, and the molar ratio of the isocyanate moiety to the hydroxyl moiety of the reaction mixture is 0.90: 1 to 7: 1. In further embodiments, the reaction mixture may further comprise a compound selected from the group consisting of water, a catalyst, a surfactant, a blowing agent, or a combination thereof.

[0014] The present disclosure provides a method for preparing a liquid transition metal chelate polyol blend, wherein the method includes providing a polyol; providing a chelating agent having a nitrogen-based chelating portion; and providing a transition metal compound having a transition metal ion. The method also includes mixing the polyol, the chelating agent, and the transition metal compound to form a liquid transition metal chelate polyol blend, wherein the polyol in the blend has 0.001 to 1.0 moles of nitrogen in the nitrogen-based chelating portion per 100g of the liquid transition metal chelate polyol blend. For each embodiment, the molar ratio of nitrogen in the nitrogen-based chelating portion of the liquid transition metal chelate polyol blend to the transition metal ion is 8.0:1.0 to 1.0:1.0 (nitrogen moles: transition metal ion moles).

[0015] The present disclosure also provides a method for preparing a reaction mixture for producing a polyurethane polymer, wherein the method includes providing an isocyanate reactive composition as provided herein; providing an isocyanate compound having an isocyanate moiety; and mixing the isocyanate reactive composition and the isocyanate compound to form a reaction mixture having a molar ratio of isocyanate moieties to hydroxyl moieties of 0.90: 1 to 7: 1. For various embodiments, mixing the isocyanate reactive composition and the isocyanate compound may further include mixing water, a catalyst, a surfactant, a flame retardant, a blowing agent, an additive, or a combination thereof with the reaction mixture to form a polyurethane polymer, including a polyurethane foam. DETAILED DESCRIPTION

[0016] The present disclosure provides a liquid transition metal chelated polyol blend that can be used in isocyanate reactive compositions and reaction mixtures containing isocyanate reactive compositions for forming polyurethane polymers. The polyurethane polymers and polyurethane foams of the present disclosure can have improved smoke performance with respect to the emission of hydrogen cyanide (HCN) and carbon monoxide (CO) during a pyrolysis event (e.g., a fire).

[0017] The liquid transition metal chelate polyol blend of the present disclosure comprises a polyol, a transition metal compound having a transition metal ion, and a chelating agent having a nitrogen-based chelating moiety, wherein there is 0.05 weight percent (wt.%) to 10.0 wt.% of the transition metal ion from the transition metal compound, the wt.% being based on the total weight of the liquid transition metal chelate polyol blend, and wherein the liquid transition metal chelate polyol blend has 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 grams (g) of the polyol in the liquid transition metal chelate polyol blend. In various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion of the liquid transition metal chelate polyol blend to transition metal ions is from 8.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), wherein for various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is preferably from 4.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), more preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is from 2.8:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), and most preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is from 2.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions). As used herein, the liquid transition metal chelate polyol blend is liquid at a pressure of 80 to 25,000 kilopascals and is liquid at a temperature above -10°C and below 80°C, preferably below 60°C, more preferably below 40°C, and most preferably below 25°C. As used herein, the liquid transition metal chelate polyol blend comprises a non-nominal amount of transition metal compound particles / solids such that the nominal amount of transition metal compound particles / solids is less than 0.10 weight percent (wt.%), preferably less than 0.01 wt.%, more preferably less than 0.001 wt.%, based on the weight of the liquid transition metal chelate polyol blend.

[0018] In various embodiments, the polyol in the transition metal chelate polyol blend is selected from the group consisting of polyester polyols, polyether polyols, polycarbonate polyols, polyether carbonate polyols, and combinations thereof. In some embodiments, the polyol is preferably a polyester polyol. In other embodiments, the polyol is preferably a polyether polyol.

[0019] The polyester polyol of the present disclosure can be a homopolymer, a random copolymer, a block copolymer, a multi-block copolymer, and an end-capped product that may contain an initiator residue in the case of a ring-opening polyester polyol. Polyester polyols can be aromatic, aliphatic or alicyclic, and can include their hydrogenated products. In various embodiments, polyester polyols are aromatic polyester polyols with aromatic moieties, and the aromatic moieties account for 5 weight percentages (wt.%) to 60wt.% of the total weight of aromatic polyester polyols. In various embodiments, polyester polyols are preferably aromatic polyester polyols with aromatic moieties, and the aromatic moieties account for 10wt.% to 40wt.% of the total weight of aromatic polyester polyols. In various embodiments, polyester polyols are more preferably aromatic polyester polyols with aromatic moieties, and the aromatic moieties account for 10wt.% to 20wt.% of the total weight of aromatic polyester polyols. As used herein, "aromatic moieties" are at least one cyclic conjugated molecule moiety in the form of a planar unsaturated carbon atom ring that is covalently attached to an isocyanate-reactive compound. The planar unsaturated ring of carbon atoms may have at least six (6) carbon atoms. For illustration, the isocyanate-reactive compound bis(2-hydroxyethyl)terephthalate has C 12 H 14 O6 molecular formula and a formula weight of 254.2 g / mol, and has an aromatic content corresponding to the C6H4 molecular formula and a corresponding formula weight of 76.1 g / mol, wherein the aromatic portion of bis(2-hydroxyethyl)terephthalate is 29.9 weight percent (wt.%).

[0020] The liquid polyester polyols may have a low to medium number average molecular weight ranging from 100 to 5,000, preferably 200 to 2,500, more preferably 300 to 1,000, and most preferably 350 to 750. The number average molecular weight may be measured using end group analysis or gel permeation chromatography (GPC) as known in the art. The liquid polyester polyols may also have a number average isocyanate reactive group functionality (e.g., hydroxyl) of 1.8 to 4, e.g., 2 to 3, per molecule, wherein each value is an average. A variety of chemical structures may constitute the liquid polyester polyols, wherein at least one requirement is the presence of at least two hydroxyl groups (i.e., diols), and the liquid polyester polyols are liquid at pressures of 80 to 25,000 kilopascals and are liquid at temperatures above -10°C and below 80°C,

[0021] For example, the monomers used to form the liquid polyester polyols may include polyols, such as diols, triols and / or higher alcohols, and polyacids, such as dibasic acids and / or triacids, such as carboxylic acids and / or polycarboxylic acid anhydrides or corresponding polycarboxylic acid esters of lower alcohols, cyclic esters or mixtures thereof, wherein these compounds react as known in the art to form a reaction product of the liquid polyester polyol. Exemplary polyols include, but are not limited to, ethylene glycol, propylene glycol-(1,2) and -(1,3), butanediol-(1,4) and -(2,3), hexanediol-(1,6), octanediol-(1,8), neopentyl glycol, cyclohexanedimethanol (1,4-bis-hydroxy-methylcyclohexane and other isomers), 2-methyl-1,3-propanediol, glycerol, trimethylolpropane, hexanetriol-(1,2,6), butanetriol-(1,2,4), trimethylolethane, pentaerythritol, quinitol, mannitol and sorbitol, methyl glycosides, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol, and polybutylene glycol. The polyols may also include polycarbonate polyols such as the reaction products of diols (e.g., propylene glycol-(1,3), butanediol-(1,4) and / or hexanediol-(1,6), diethylene glycol, triethylene glycol or tetraethylene glycol) with diaryl carbonates (e.g., diphenyl carbonate), dialiphatic carbonates (e.g., dimethyl carbonate) or phosgene, or from the reaction of epoxides and carbon dioxide.

[0022] Polyacid can be aliphatic, alicyclic, aromatic and / or heterocyclic, and it can be substituted by halogen atom for example, and / or can be undersaturated. Suitable polyacid, acid anhydride and the polycarboxylic acid ester of lower alcohol include but not limited to succinic acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, phthalic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, endomethylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimerization and trimerization fatty acid (such as oleic acid) optionally mixed with monomer fatty acid, dimethyl terephthalate and terephthalic acid-bis-ethylene glycol ester.

[0023] The cyclic esters may be aliphatic and may be substituted, for example, by alkyl groups, and / or may be unsaturated. Suitable cyclic esters include, but are not limited to, ε-caprolactone, d,l-lactide, glycolide, δ-valerolactone, and pivolactone, and the like.

[0024] Liquid polyester polyol can be aromatic, aliphatic or alicyclic, and can include their hydrogenation products. Preferred examples of liquid polyester polyol include but are not limited to polycaprolactone polyol, polypropiolactone polyol, polyglycolide polyol, polypivalolactone polyol, polyvalerolactone polyol, polyethylene adipate polyol, polypropylene adipate polyol, polybutylene adipate polyol, polyhexamethylene adipate polyol, polyneopentyl adipate polyol, polycyclohexane dimethylene adipate polyol, polyethylene succinate polyol, polypropylene succinate polyol, polybutylene succinate polyol, polyhexamethylene succinate polyol, polysuccinate neopentyl polyol, polycyclohexane dimethyl succinate polyol, polyethylene azelate polyol, polypropylene azelate polyol, polybutylene Azelate polyol, polyhexamethylene azelate polyol, polyneopentyl azelate polyol, polycyclohexanedimethylene azelate polyol, polyethylene sebacate polyol, polypropylene sebacate polyol, polybutene sebacate polyol, polyhexamethylene sebacate polyol, polyneopentyl sebacate polyol, polycyclohexane dimethylene sebacate polyol, diethylene glycol / terephthalic acid polyol, polyethylene glycol / terephthalic acid polyol, diethylene glycol / phthalic acid or phthalic anhydride polyol, polyethylene glycol / phthalic acid or phthalic anhydride polyol, diethylene glycol / isophthalic acid polyol, polyethylene glycol / isophthalic acid polyol and copolyester polyols thereof.

[0025] More preferred examples of liquid polyester polyols include polycaprolactone polyols, polyethylene adipate polyols, polypropylene adipate polyols, polybutylene adipate polyols, polyhexamethylene adipate polyols, polycyclohexanedimethylene adipate polyols, polyethylene succinate polyols, polybutylene succinate polyols, diethylene glycol / terephthalic acid polyols, polyethylene glycol / terephthalic acid polyols, diethylene glycol / phthalic acid or phthalic anhydride polyols, polyethylene glycol / phthalic acid or phthalic anhydride polyols, diethylene glycol / isophthalic acid polyols, polyethylene glycol / isophthalic acid polyols, and copolyesters of diethylene glycol and / or polyethylene glycol terephthalate, isophthalate and / or phthalate (when an average hydroxyl functionality greater than 2.0 is desired, glycerol and / or trimethylolpropane are optionally used). The most preferred examples of liquid polyester polyols include diethylene glycol / terephthalic acid polyols, polyethylene glycol / terephthalic acid polyols, diethylene glycol / phthalic acid or phthalic anhydride polyols, polyethylene glycol / phthalic acid or phthalic anhydride polyols, diethylene glycol / isophthalic acid polyols, polyethylene glycol / isophthalic acid polyols, and copolyesters of diethylene glycol and / or polyethylene glycol terephthalate, isophthalate and / or phthalate (when an average hydroxyl functionality greater than 2.0 is desired, glycerol and / or trimethylolpropane are optionally used). For various embodiments, the polyester polyols may also be uncapped or capped with ethylene oxide (EO) and / or propylene oxide (PO) as known in the art to provide a hydrophilic or hydrophobic structure. Examples of other liquid polyester polyols include modified aromatic polyester polyols, such as those provided under the trade name STEPANPOL PS-2352 (acid value 0.6-1.0 mg KOH / g, hydroxyl value 230-250 mg KOH / g, hydroxyl functionality 2.0, Stepan Company). The liquid polyester may also contain a certain proportion of carboxyl end groups. Liquid polyester polyols formed from lactones such as ε-caprolactone or hydroxycarboxylic acids such as 6-hydroxycaproic acid may also be used.

[0026] Liquid polyether polyols may include those having at least 2, such as 2 or 3, hydroxyl groups per molecule and may be prepared, for example, by polymerizing epoxides / cyclic ethers such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide or epichlorohydrin by themselves in the presence of BF3 or by chemically adding these epoxides, optionally in the form of a mixture (such as a mixture of ethylene oxide and propylene oxide) or in sequence, to starting components having reactive hydrogen atoms such as water, ammonia, ethanol or amines. Examples of suitable starting components include ethylene glycol, propylene glycol-(1,3) or -(1,2), glycerol, trimethylolpropane, 4,4'-dihydroxy-diphenylpropane, Novolac, aniline, ethanolamine or ethylenediamine. Sucrose-based polyether polyols may also be used. In many cases it is preferred to use polyethers containing a predominant amount of primary OH groups (up to 100% of the OH groups present in the polyether). The nominal functionality of the polyether polyol or copolyether polyol should be at least 2.0. The nominal functionality is preferably 2.5 to 8, more preferably 2.5 to 7 or 2.5 to 6. The hydroxyl equivalent of the polyether polyol or copolyether polyol is at least 85, preferably at least 100, more preferably 150 to 3,200, 250 to 3,000 in some embodiments, and 300 to 2,500 in specific embodiments. The polyol can also be formed by a blend, wherein the blend includes a blend of a diol and a triol. The number average molecular weight (Mn) of the diol can be 200 to 8,000 g / mol and the average molecular weight (Mn) of the triol is 250 to 6,500 g / mol. Other examples of suitable polyether polyols include those polymers or copolymers having a hydroxyl equivalent of at least 75 formed with propylene oxide. The propylene oxide may be 1,3-propylene oxide, but is more typically 1,2-propylene oxide. If it is a copolymer, the comonomer is another copolymerizable alkylene oxide, such as ethylene oxide, 2,3-butylene oxide, tetrahydrofuran, 1,2-hexylene oxide, etc. The copolymer may contain 25% by weight or more, 50% by weight or more, and preferably 75% by weight or more of polymerized propylene oxide, based on the total weight of the polymerized alkylene oxide. The copolymer preferably contains no more than 75% by weight, especially no more than 50% by weight, of polymerized ethylene oxide.

[0027] In various embodiments, the hydroxyl value of the polyol can be 10 mg KOH / g to 700 mg KOH / g. In still other embodiments, the hydroxyl value of the polyol is 20 mg KOH / g to 500 mg KOH / g, or 30 mg KOH / g to 350 mg KOH / g. As used herein, the hydroxyl value is the number of milligrams of potassium hydroxide, which is equivalent to the hydroxyl content in one gram of polyol or other hydroxy compound. The number average isocyanate reactive group functionality of the polyol can also be 1.8 to 6, such as 2 to 4 or 2.2 to 3.0.

[0028] For various embodiments, the polyether polyols and / or polyester polyols may also be uncapped or capped with ethylene oxide (EO) and / or propylene oxide (PO) as known in the art to provide a hydrophilic or hydrophobic structure.

[0029] For various embodiments, the liquid transition metal chelate polyol blend comprises 0.05 weight percent (wt.%) to 10.0 wt.% transition metal ions from transition metal compounds based on the total weight of the liquid transition metal chelate polyol blend. The liquid transition metal chelate polyol blend may also comprise 0.15 wt.% to 6.0 wt.% transition metal ions from transition metal compounds, or 0.5 wt.% to 3.0 wt.% transition metal ions from transition metal compounds, the wt.% being based on the total weight of the liquid transition metal chelate polyol blend.

[0030] For embodiments, the transition metal compound is selected from the group consisting of transition metal carboxylates, transition metal salts, transition metal coordination compounds and combinations thereof, and the transition metal ion is selected from the transition metals and combinations thereof of the 4th, 5th, 6th, 7th, 8th, 9th, 10th, 11th, 12th groups and the 4th and 5th periods of the periodic table (IUPAC Periodic Table of Elements, November 28, 2016). Preferably, the transition metal compound is a transition metal carboxylate. Preferably, the transition metal ion is selected from the group consisting of: transition metal ions of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, cadmium, mercury, palladium, titanium, vanadium and combinations thereof. More preferably, the transition metal ion is selected from the group consisting of: transition metal ions of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium and combinations thereof. Most preferably, the transition metal ion is selected from the group consisting of: transition metal ions of copper, zinc, iron, manganese, cobalt, nickel and combinations thereof. Examples of transition metal compounds include copper (II) 2-ethylhexanoate, copper (II) acetate, copper (II) acetate monohydrate (Cu(OAc)2H2O), copper (I) acetate, copper butyrate, di-μ-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine) copper (II)] chloride, zinc stannate, zinc hydroxystannate, zinc (II) acetate, cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, manganese (II) 2-ethylhexanoate, and combinations thereof. Preferably, the transition metal compound is selected from the group consisting of copper (II) 2-ethylhexanoate (CuEH), copper (II) acetate, copper (II) acetate monohydrate (Cu(OAc)2H2O), copper (II) propionate, copper (II) isobutyrate (Cu(i-Bu)2), cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, and combinations thereof.

[0031] For embodiments, the chelating agent having a nitrogen-based chelating moiety is selected from the group consisting of a diamine chelating moiety, a triamine chelating moiety, a tetraamine chelating moiety, and combinations thereof. For some embodiments, the chelating agent having a nitrogen-based chelating moiety is selected from a tertiary polyamino compound having at least two tertiary nitrogens connected by carbon atoms. The chelating agent preferably may conform to Formula I

[0032]

[0033] wherein R1, R2, R3, R4 and R5 are each independently C1 to C8 alkyl, alkoxylate / polyalkoxylate (i.e. -(CH2CHRO) n -H, wherein R is H or C1 to C3 alkyl and n is an integer from 1 to 10) and equivalents thereof, x and x' are each independently an integer of 2 or 3, and y is an integer of 0, 1 or 2. More preferably, for Formula I, R1, R2, R3, R4 and R5 are each independently a C1 to C3 alkyl, an alkoxylate / polyalkoxylate as provided above, wherein the alkyl is C1 to C2, x and x' are each independently an integer of 2 or 3, and y is an integer of 0 or 1. Most preferably, for Formula I, R1, R2, R3, R4 and R5 are each independently a C1 to C3 alkyl, an alkoxylate / polyalkoxylate as provided above, wherein the alkyl is C1, x and x' are integers of 2, and y is an integer of 0 or 1.

[0034] For example, the chelating agent having a nitrogen-based chelating moiety may further have an isocyanate-reactive moiety. Preferred chelating agents having a nitrogen-based chelating moiety are diamines, triamines and tetraamines, wherein the amine moiety is a tertiary amine.

[0035] Examples of chelating agents having a diamine chelating moiety for the nitrogen-based chelating moiety include 2,2'-bipyridine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, triethylenediamine (1,4-diazabicyclo[2.2.2]octane), N,N'-dimethylaminoethyl-N-methylethanolamine, N,N'-dimethylaminoethylmorpholine, N,N,N',N'-tetramethyl-1,3-butanediamine, N,N'-dimethylpiperazine, methyl Hydroxyethylpiperazine, N,N,N',N'-tetra-(2-hydroxypropyl)ethylenediamine, 2-[[2-(dimethylamino)ethyl]methylamino]ethanol, N,N,N'-trimethyl-N'-hydroxyethyl-bis(aminoethyl)ether; N,N-bis(3-dimethylamino-propyl)-N-isopropanolamine; bis-(dimethylaminopropyl)amino-2-propanol; N,N,N'-trimethylaminopropylethanolamine, 1,2-ethylenediamine polymers with methyloxirane, and combinations thereof. Examples of chelating agents having triamine chelating moieties for nitrogen-based chelating moieties include VORANOL 1,2-ethylenediamine polymers with methyloxirane. TM RA 640 (available from Dow), N,N,N',N',N"-pentamethyldiethylenetriamine, N,N,N',N',N"-pentamethyldipropylenetriamine, 1-[bis[3-(dimethylamino)propyl]amino-2-propanol], N,N'-dimethylaminoethyl(N-methylpiperazine), and combinations thereof. Examples of chelating agents having a tetraamine chelating moiety for the nitrogen-based chelating moiety include 1,1,4,7,10,10-hexamethyltriethylenetetramine, tris[2-(dimethylamino)ethyl]amine, tris[2-(isopropylamino)ethyl]amine, and combinations thereof. Preferably, the chelating agent having a nitrogen-based chelating moiety is selected from the group consisting of 2,2'-bipyridine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N',N"-pentamethyldiethylenetriamine, 2-[[2-(dimethylamino)ethyl]methylamino]ethanol, 1-[bis[3-(dimethylamino)propyl]amino-2-propanol], 1,2-ethylenediamine polymers with methyl oxirane (e.g., VORANOL TM RA 640) and combinations thereof.

[0036] In various embodiments, the chelating agent having a nitrogen-based chelating moiety is soluble in the polyol of the transition metal chelate polyol blend, wherein the liquid transition metal chelate polyol blend has 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, preferably 0.003 to 0.60 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, more preferably 0.006 to 0.40 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend, and most preferably 0.01 to 0.20 mole of nitrogen in the nitrogen-based chelating moiety per 100 g of polyol in the liquid transition metal chelate polyol blend.

[0037] The molar ratio of nitrogen in the nitrogen-based chelating portion of the liquid transition metal chelate polyol blend to the transition metal ion is 8:0:1:0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), wherein for various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is preferably 4.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), more preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.8:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), and most preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions).

[0038] In various embodiments, the liquid transition metal chelate polyol blends of the present disclosure have little effect on the reaction of isocyanates and isocyanate-reactive compositions. For PIR systems, the liquid transition metal chelate polyol blends preferably do not reduce the isocyanurate content in the polyurethane foam by 50% or more compared to the same polyurethane foam formulation without the transition metal compound. More preferably, the transition metal compound does not reduce the isocyanurate content in the polyurethane foam by 40% or more compared to the same polyurethane foam formulation without the transition metal compound. More preferably, the transition metal compound does not reduce the isocyanurate content in the polyurethane foam by 30% or more compared to the same polyurethane foam formulation without the transition metal compound. Most preferably, the transition metal compound does not reduce the isocyanurate content in the polyurethane foam by 25% or more compared to the same polyurethane foam formulation without the transition metal compound.

[0039] The present disclosure provides a method for preparing a liquid transition metal chelate polyol blend, wherein the method includes providing a polyol; providing a chelating agent having a nitrogen-based chelating moiety; and providing a transition metal compound having a transition metal ion. The method also includes mixing the polyol, the chelating agent, and the transition metal compound to form a liquid transition metal chelate polyol blend, wherein the blend has 0.001 to 1.0 moles of nitrogen in the nitrogen-based chelating moiety per 100 g of the polyol in the liquid transition metal chelate polyol blend. For various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion of the liquid transition metal chelate polyol blend to the transition metal ion is 8:0:1:0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), wherein for various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is preferably 4.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), more preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.8:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), and most preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to the transition metal ion is 2.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions). For various embodiments, mixing can occur at atmospheric pressure (eg, 101.23 KPa) and a temperature below 100°C, preferably below 80°C, more preferably below 60°C, and most preferably below 40°C to form a liquid transition metal chelate polyol blend.

[0040] The present disclosure also provides an isocyanate reactive composition, which includes a liquid transition metal chelate polyol blend as provided herein, optionally a catalyst and a flame retardant, wherein the isocyanate reactive composition can be used to form a polyurethane polymer. Embodiments of the present disclosure also include an isocyanate reactive composition with a liquid transition metal chelate polyol blend as provided herein, and also include a polyol (separated from the polyol in the liquid transition metal chelate polyol blend), a phosphorus flame retardant, a catalyst, a blowing agent, water, a surfactant or a combination thereof, wherein the isocyanate reactive composition can be used to form a polyurethane foam. For example, an isocyanate reactive composition as provided herein may include a blowing agent and a surfactant for forming a polyurethane polymer foam. The catalyst, water, surfactant, flame retardant and blowing agent each having an amount (e.g., wt.% value) and each example thereof that can be used in an isocyanate reactive composition are provided herein in the context of a reaction mixture for forming a polyurethane polymer of the present disclosure discussed below.

[0041] For various embodiments, the isocyanate reactive composition may also include a polyol separated from the polyol in the liquid transition metal chelate polyol blend, wherein the isocyanate reactive composition includes 0.1 to 100 weight percent (wt.%) of the liquid transition metal chelate polyol blend and up to 99.9% of the polyol separated from the polyol of the liquid transition metal chelate polyol blend to form an isocyanate reactive composition for a polyurethane polymer, the wt.% being based on the total weight of the isocyanate reactive composition. For various embodiments, the polyol used with the liquid transition metal chelate polyol blend to help form the isocyanate reactive composition can be selected from the group consisting of polyester polyols, polyether polyols, polycarbonate polyols, polyether carbonate polyols, and combinations thereof.

[0042] The number average molecular weight of the polyol separated from the polyol in the liquid transition metal chelate polyol blend can be 100g / mol to 10,000g / mol. Other number average molecular weight values ​​are also possible. For example, the number average molecular weight of the polyol can be a low value of 100, 200, 300, 350 or 400g / mol to a high value of 500, 750, 1,000, 2,000 or 10,000g / mol. The number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography and other methods as known in the art. The polyol used together with the liquid transition metal chelate polyol blend to help form the isocyanate reactive composition can also include an aromatic portion. As used herein, "aromatic portion" is at least one cyclic conjugated molecular portion in the form of a planar unsaturated carbon atom ring covalently attached to a polyol compound. The planar unsaturated ring of carbon atoms can have at least six (6) carbon atoms.

[0043] For embodiments, the isocyanate reactive composition may also include 0.1wt.% to 7.0wt.% phosphorus from a flame retardant compound, wherein the wt.% of phosphorus is based on the gross weight of the isocyanate reactive composition. Preferably, the isocyanate reactive composition includes 0.5wt.% to 5.0wt.% phosphorus from a flame retardant compound (wt.% of phosphorus is based on the gross weight of the isocyanate reactive composition). More preferably, the isocyanate reactive composition includes 1.0wt.% to 3.0wt.% phosphorus from a flame retardant compound (wt.% of phosphorus is based on the gross weight of the isocyanate reactive composition). The isocyanate reactive composition may also include 0.05wt.% to 10.0wt.% transition metal, wherein the transition metal is from a transition metal compound with a transition metal ion as provided herein, and the wt.% of the transition metal is based on the gross weight of the liquid transition metal chelated polyol blend. Preferably, the isocyanate reactive composition may further comprise 0.15 wt.% to 6.0 wt.% of a transition metal from a transition metal compound with a transition metal ion as provided herein (wt.% of the transition metal is based on the total weight of the liquid transition metal chelate polyol blend), and most preferably 0.5 wt.% to 3.0 wt.% of a transition metal from a transition metal compound with a transition metal ion as provided herein (wt.% of the transition metal is based on the total weight of the liquid transition metal chelate polyol blend). For a given weight percentage value, the molar ratio of the transition metal ion to phosphorus of the isocyanate reactive composition (moles of transition metal ions: moles of phosphorus) is 0.05:1 to 5:1. Preferably, the molar ratio of transition metal ions to phosphorus (moles of transition metals: moles of phosphorus) is 0.1:1 to 2:1. More preferably, the molar ratio of transition metal ions to phosphorus (moles of transition metals: moles of phosphorus) is 0.5:1 to 1:1.

[0044] For the embodiments provided herein, the isocyanate reactive composition may have a flame retardant compound selected from the group consisting of the following, preferably a halogen-free flame retardant compound: phosphate, phosphonate, phosphinate, phosphite and a combination thereof. Examples of phosphates include trialkyl phosphates, triaryl phosphates, phosphates and resorcinol bis (diphenyl phosphate). As used herein, trialkyl phosphates have at least one alkyl group with 2 to 12 carbon atoms. The other two alkyl groups of the trialkyl phosphate can be independently the same as or different from the first alkyl group, containing 1 to 8 carbon atoms, including straight or branched alkyl groups, cyclic alkyl groups, alkoxyethyl groups, hydroxyalkyl groups, hydroxyalkoxyalkyl groups and straight or branched alkylene groups. The example of other two alkyls of trialkyl phosphate includes for example methyl, ethyl, propyl, butyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, butoxyethyl, isopentyl, neopentyl, isohexyl, isoheptyl, cyclohexyl, propylene, 2-methylpropylene, neopentene, hydroxymethyl, hydroxyethyl, hydroxypropyl or hydroxybutyl. The blend of different trialkyl phosphates can also be used. The three alkyls of trialkyl phosphate can be the same. The alkyl can be a halogenated alkyl, and preferably the alkyl is a halogen-free alkyl. Trialkyl phosphate can be tris (2-chloro-1-methylethyl) phosphate (TCPP), tris [2-chloro-1-(chloromethyl) ethyl] phosphate (TDCP), tris (p-tert-butylphenyl) phosphate (TBPP) and tris (2-chloroethyl) phosphate (TCEP). Trialkyl phosphate is ideally triethyl phosphate (TEP).

[0045] Examples of phosphonates include diethyl (hydroxymethyl) phosphonate, dimethyl methyl phosphonate, and diethyl ethyl phosphonate. Examples of phosphinates include metal salts of organic phosphinates, such as aluminum methylethylphosphinate, aluminum diethylphosphinate, zinc methylethylphosphinate, and zinc diethylphosphinate. Examples of additional halogen-free flame retardant compounds include resorcinol diphosphoric acid, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, ammonium polyphosphate, and combinations thereof.

[0046] The present disclosure also provides a reaction mixture for forming a polyurethane polymer. The reaction mixture comprises an isocyanate compound with an isocyanate moiety as provided herein and an isocyanate-reactive composition with a hydroxyl moiety (e.g., from a polyester polyol), wherein the molar ratio of the isocyanate moiety to the hydroxyl moiety of the reaction mixture is 0.90:1 to 7:1. For rigid polyurethane (PUR) and polyisocyanurate (PIR), preferably, the molar ratio of the isocyanate moiety to the hydroxyl moiety is 1.2:1 to 7:1, more preferably, the molar ratio of the isocyanate moiety to the hydroxyl moiety is 1.5:1 to 5:1, and most preferably, the molar ratio of the isocyanate moiety to the hydroxyl moiety is 2:1 to 4:1. For flexible polyurethane foams, preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 0.90:1 to 1.20:1, more preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 0.95:1 to 1.15:1, and most preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 1:1 to 1.10: 1. For two-component polyurethane adhesives, sealants, coatings and elastomers, preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 0.95:1 to 1.35:1, more preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 0.98:1 to 1.10:1, and most preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is 1:1 to 1.05:1.

[0047] For each embodiment, the number average molecular weight of the isocyanate compound is 150g / mol to 750g / mol. Other number average molecular weight values ​​are also possible. For example, the number average molecular weight of the isocyanate reactive compound can be from a low value of 150, 200, 250 or 300g / mol to a high value of 350, 400, 450, 500 or 750g / mol. In certain embodiments, when the isocyanate compound is an isocyanate reactive compound and a polyisocyanate compound or a polymerized isocyanate compound in excess of moles, the isocyanate prepolymer produced by the reaction under the condition of not causing gelling or curing, the isocyanate prepolymer can have a higher number average molecular weight greater than 750g / mol, and can be calculated by the number average molecular weight and relative mass of each component used to prepare the prepolymer. The number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography and other methods as known in the art. As known in the art, the isocyanate compound can be monomeric and / or polymeric. In addition, the isocyanate equivalent weight of the isocyanate compound can be 80 to 1750. In certain embodiments, the viscosity of the isocyanate is 5 to 50,000 mPa s at 25°C when measured using a Brookfield DVE viscometer. Other viscosity values ​​are also possible. For example, the viscosity value of the isocyanate reactive compound can be a low value of 5, 10, 30, 60 or 150 mPa s to an upper limit of 500, 2500, 10,000 or 50,000 mPa s, each of which is measured at 25°C using a Brookfield DVE viscometer.

[0048] As used herein, polymeric isocyanate compounds contain two or more -NCO groups per molecule and are also considered to be isocyanate compounds. For various embodiments, the polymeric isocyanate compound is selected from aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, polyisocyanates, isocyanate prepolymers and combinations thereof. For various embodiments, the number average molecular weight of the isocyanate compound is 150 g / mol to 750 g / mol. In addition, the isocyanate equivalent of the polymeric isocyanate compound can be 80 to 150, preferably 100 to 145 and more preferably 110 to 140, with a so-called MDI product as a mixture of isomers of diphenylmethane diisocyanate (MDI) in monomeric MDI or a so-called polymeric MDI product as a mixture of polymethylene polyphenylene polyisocyanates in monomeric MDI.

[0049] Examples of the polymeric isocyanate compounds of the present disclosure may include, but are not limited to, methylene diphenyl diisocyanate (MDI), polymethylene polyphenyl isocyanate containing MDI, polymeric MDI (PMDI), 1,6-hexamethylene diisocyanate (HDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene diisocyanate, hydrogenated MDI (HDI), and the like. 12Suitable isocyanates include methoxyphenyl-2,4-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4',4"-triphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, hydrogenated polymethylene polyphenyl polyisocyanate, toluene-2,4,6-triisocyanate and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, methylene biscyclohexyl isocyanate (HMDI), isophorone diisocyanate (IPDI), and combinations thereof. Suitable isocyanates may also include other aromatic and / or aliphatic polyfunctional isocyanates. Aromatic diisocyanates Esters include those containing phenyl, tolyl, xylyl, naphthyl or diphenyl moieties or combinations thereof, such as trimethylolpropane adducts of xylylene diisocyanate, trimethylolpropane adducts of toluene diisocyanate, 4,4'-diphenyldimethane diisocyanate (MDI), xylylene diisocyanate (XDI), 4,4'-diphenyldimethylmethane diisocyanate, dialkyl diphenylmethane diisocyanate and tetraalkyl diphenylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate and combinations thereof. Suitable aliphatic polymeric isocyanate compounds include trimers of hexamethylene diisocyanate, trimers of isophorone diisocyanate, Biuret of hexamethylene diisocyanate, hydrogenated polymerized methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, hydrogenated MDI, tetramethylxylene diisocyanate (TMXDI), 1-methyl-2,4-diisocyanatocyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane, tetramethoxybutane 1,4-diisocyanate, butane 1,4-diisocyanate, hexane 1,6-diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane 1,4-diisocyanate, and combinations thereof. Examples of other polymeric isocyanate compounds include additional aliphatic, alicyclic, polycyclic or aromatic compounds such as hydrogenated diisocyanate. Toluene diisocyanate (HXDI), p-phenylene diisocyanate (PPDI), 3,3'-dimethyldiphenyl-4,4'-diisocyanate (DDDI), 2,2,4-trimethylhexamethylene diisocyanate (TMDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12MDI) and norbornane diisocyanate (NDI). In addition to the isocyanates mentioned above, partially modified polyisocyanates can be used, including uretdione, isocyanurate, carbodiimide, uretonimine, allophanate or biuret structure and combinations thereof, etc. As provided herein, the polyol can be pre-reacted with an organic polyisocyanate to form a prepolymer or quasi-prepolymer containing an isocyanate group.The isocyanate content of the prepolymer or quasi-prepolymer may be, for example, 1 to 20 weight percent. In some embodiments, the isocyanate content may be at least 2.5% or at least 4%, and at most 15%, at most 12%, or at most 10%.

[0050] In addition to providing a reaction mixture, the present disclosure also provides a method for preparing a reaction mixture for producing polyurethane polymers. As discussed herein, the reaction mixture for forming a polyurethane polymer comprises an isocyanate compound with an isocyanate moiety and an isocyanate-reactive composition as discussed herein, wherein the polyol comprises a hydroxyl moiety, and the molar ratio of the isocyanate moiety to the hydroxyl moiety of the reaction mixture is 0.90: 1 to 7: 1 (and other values ​​as discussed herein). The method for preparing a reaction mixture for producing a polyurethane polymer includes providing an isocyanate-reactive composition as provided herein; providing an isocyanate compound with an isocyanate moiety as provided herein; and mixing the isocyanate-reactive composition and the isocyanate compound to form a reaction mixture having a molar ratio of the isocyanate moiety to the hydroxyl moiety of 0.90: 1 to 7: 1 (and other values ​​as discussed herein). Mixing the isocyanate-reactive composition and the isocyanate compound can also include mixing water, a catalyst, a surfactant, a blowing agent, a phosphorus-containing flame retardant compound, and a combination thereof with the reaction mixture to form a polyurethane polymer, including a subset of polyurethane polymer foams. The result of the method can be a polyurethane polymer or a polyurethane polymer foam formed from the reaction mixture as provided herein.

[0051] For each embodiment provided herein, the catalyst can be present in the reaction mixture in an amount of 0.01 to 1.5 wt.%, based on the total weight of the reaction mixture. The catalyst can be selected from the group consisting of: an organic tertiary amine, a tertiary phosphine, potassium acetate, a carbamate-based catalyst, and a combination. The catalyst can also include an organotin compound, as known in the art.

[0052] The catalyst may be a foaming catalyst, a gelling catalyst, a trimerization catalyst, or a combination thereof. As used herein, a foaming catalyst and a gelling catalyst may be distinguished by a tendency to favor a urea (foaming) reaction in the case of a foaming catalyst or a urethane (gelling) reaction in the case of a gelling catalyst. A trimerization catalyst may be used to promote an isocyanurate reaction in a composition. Both foaming catalysts and gelling catalysts are used to prepare rigid and flexible polyurethane foams. Polyurethanes that are not foams or microporous (e.g., many coatings, adhesives, sealants, and elastomers) utilize gelling catalysts.

[0053] Examples of blowing catalysts (e.g., catalysts that may tend to favor the blowing reaction) include, but are not limited to, short chain tertiary amines or oxygen-containing tertiary amines. Amine-based catalysts may not be sterically hindered. For example, blowing catalysts include bis-(2-dimethylaminoethyl) ether; pentamethyldiethylene-triamine, triethylamine, tributylamine, N,N-dimethylaminopropylamine, dimethylethanolamine, N,N,N',N'-tetramethylethylenediamine, and combinations thereof, and the like. An example of a commercially available blowing catalyst is POLYCAT® available from Evonik. TM 5, and other commercially available blowing catalysts.

[0054] Examples of gelling catalysts (e.g., catalysts that may tend to favor the gelling reaction) include, but are not limited to, organometallic compounds, cyclic tertiary amines and / or long chain amines (e.g., containing several nitrogen atoms), and combinations thereof. Organometallic compounds include organotin compounds, such as tin (II) salts of organic carboxylic acids, such as tin (II) diacetate, tin (II) dioctoate, tin (II) diethylhexanoate, and tin (II) dilaurate, and dialkyltin (IV) salts of organic carboxylic acids, such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate. Bismuth salts of organic carboxylic acids may also be used as gelling catalysts, such as bismuth octoate. Cyclic tertiary amines and / or long chain amines include dimethylbenzylamine, triethylenediamine, and combinations thereof. An example of a commercially available gelling catalyst is POLYCAT® purchased from Evonik. TM 8 and T-12, and other commercially available gelling catalysts.

[0055] Examples of trimerization catalysts include N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA); N,N′,N″-tris(3-dimethylaminopropyl)hexahydro-S-triazine; N,N-dimethylcyclohexylamine; 1,3,5-tris(N,N-dimethylaminopropyl)-s-hexahydrotriazine; [2,4,6-tris(dimethylaminomethyl)phenol]; potassium acetate, potassium octoate; tetraalkylammonium hydroxides such as tetramethylammonium hydroxide; alkali metal hydroxides such as sodium hydroxide; alkali metal alkoxides such as sodium methoxide, potassium isopropoxide; and alkali metal salts of long-chain fatty acids having 10 to 20 carbon atoms, and combinations thereof, and the like. Some commercially available trimerization catalysts include all available from Evonik TMR-2, TMR-7, K 2097; K15, POLYCAT TM 41 and POLYCAT TM 46, and other commercially available trimerization catalysts.

[0056] For each of the embodiments provided herein, water can be present in the reaction mixture in an amount of 0.1 to 1.5 wt. %, based on the total weight of the reaction mixture.

[0057] For each embodiment, the surfactant may be present in the reaction mixture in an amount of 0.1 to 10 wt.% based on the total weight of the reaction mixture. Examples of suitable surfactants include silicone-based surfactants and organic-based surfactants. Some representative materials are typically polysiloxane polyoxyalkylene block copolymers, such as those disclosed in U.S. Patents Nos. 2,834,748, 2,917,480; and 2,846,458, the disclosures of which are incorporated herein by reference. Also included are organic surfactants containing polyoxyethylene-polyoxybutylene block copolymers, such as described in U.S. Patent No. 5,600,019, the disclosures of which are incorporated herein by reference as a whole. Other surfactants include polyethylene glycol ethers of long-chain alcohols, long-chain allylic acid sulfates, alkyl sulfonates, tertiary amines or alkanolamine salts of alkylaryl sulfonic acids, and combinations thereof.

[0058] For each embodiment, the blowing agent can be present in the reaction mixture for forming the polyurethane polymer foam in an amount of 1.0 to 15 wt.% based on the total weight of the reaction mixture. In addition to other blowing agents provided herein, as known in the art, the blowing agent can be selected from the group consisting of: water, volatile organic substances, dissolved inert gases and combinations thereof. Examples of blowing agents include hydrocarbons such as butane, isobutane, 2,3-dimethylbutane, n-pentane and isopentane isomers, hexane isomers, heptane isomers and cycloalkanes, including cyclopentane, cyclohexane, cycloheptane; hydrofluorocarbons such as HCFC-142b (1-chloro-1,1-difluoroethane), HCFC-141b (1,1-dichloro-1-fluoroethane), HCFC-22 (chlorodifluoromethane), HFC-245fa (1,1,1,3,3-pentafluoropropane), HFC-365mfc (1,1,1,3,3-pentafluorobutane), HFC HFC-227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-134a (1,1,1,2-tetrafluoroethane), HFC-125 (1,1,1,2,2-pentafluoroethane), HFC-143 (1,1,2-trifluoroethane), HFC 143A (1,1,1-trifluoroethane), HFC-152 (1,1-difluoroethane), HFC-227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-236ca (1,1,2,2,3,3-hexafluoropropane), HFC 236fa (1,1,1,3,3,3-hexafluoroethane), HFC245ca (1,1,2,2,3-pentafluoropentane), HFC 356mff (1,1,1,4,4,4-hexafluorobutane), HFC 365mfc (1,1,1,3,3-pentafluorobutane); hydrofluoroolefins, such as cis-1,1,1,4,4,4-hexafluoro-2-butene, 1,3,3,3-tetrafluoropropylene, trans-1-chloro-3,3,3-trifluoropropylene; chemical blowing agents, such as formic acid and water. The blowing agent can also be other volatile organic substances, such as ethyl acetate; methanol; ethanol; halogen-substituted alkanes, such as dichloromethane, chloroform, vinylidene chloride, vinylidene chloride, monochlorotrichloromethane, monochlorodifluoromethane or dichlorodifluoromethane; butane; hexane; heptane; ether and gases, such as nitrogen; air; and carbon dioxide.

[0059] In addition to water, catalysts, blowing agents, surfactants and combinations thereof, the reaction mixture may also include fillers and other additives. The total amount of such other additives may be from 0.01 wt.% to 30.0 wt.%. The use of other additives for polyurethane polymer compositions is also known and can be used with the present disclosure.

[0060] As discussed herein, the liquid transition metal chelate polyol blend has a molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions of 8:0:1:0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), wherein for various embodiments, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is preferably 4.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), more preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is 2.8:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions), and most preferably, the molar ratio of nitrogen in the nitrogen-based chelating portion to transition metal ions is 2.0:1.0 to 1.0:1.0 (moles of nitrogen:moles of transition metal ions). While other molar ratios of nitrogen to transition metal ion in the nitrogen-based chelating moiety may be used, it is desirable to maximize the amount of transition metal ion (e.g., copper) that can be delivered to the reaction mixture relative to nitrogen so that the reaction rates of the isocyanate and isocyanate-reactive moieties in the isocyanate-reactive composition or reaction mixture used to produce the polyurethane polymer and / or polyurethane polymer foam of the present disclosure are not unduly affected by the higher catalytic amine chelating agent content resulting from the higher nitrogen to transition metal ion molar ratio, such that the foaming, gelling and / or trimerization reactions are unbalanced during the foaming process, thereby resulting in a foam having significantly reduced foam properties, such as insulating properties, increased density and / or other defective foam attributes, while the reaction kinetic parameters such as cream time, gel time and open time are suitable for the processing parameters of the foaming process and related equipment.

[0061] For embodiments of the present invention, the reaction kinetics parameters of polyurethane foam are determined using a wooden tongue pressure plate for the reaction mixture provided herein. A total of 80 grams (g) of the reaction mixture with an isocyanate compound and an isocyanate-reactive composition is poured into a 500mL beaker. Cream time is defined as the time from the preparation of the reaction mixture to the identifiable start of the foaming mixture, such as the visual change (color change and / or start to rise) of the reactant. Gel time (or string time) is defined as the time from the preparation of the reaction mixture to the time when the fluid state is changed into a solid state. It is determined by repeatedly immersing the wooden tongue pressure plate in and pulling out the reaction mixture. When the wooden tongue pressure plate is pulled out from the reaction mixture, the gel time is reached as soon as a string is formed. Table dry time is defined as the time from the preparation of the foam reaction mixture to the non-sticky surface of the foam. It is determined by depositing a wooden tongue pressure plate on the foam surface. If the wooden tongue pressure plate is lifted, the foam surface will not be delaminated or broken, in other words, when the foam surface is no longer sticky, the table dry time is reached.

[0062] For each embodiment, the combination of the liquid transition metal chelate polyol blend and the optional catalyst provides reaction kinetic parameters for the polyurethane foam formulation containing the isocyanate compound and the isocyanate reactive composition, which is similar to the typical polyurethane foam formulation of the same type without the liquid transition metal chelate polyol blend. Compared with the cream time of the typical polyurethane foam of the same type without the liquid transition metal chelate polyol blend, the cream time of the foam system containing the liquid transition metal chelate polyol blend is preferably within 10 seconds, more preferably within 5 seconds, and most preferably within 2 seconds. Compared with the gel time of the typical polyurethane foam of the same type without the liquid transition metal chelate polyol blend, the gel time of the foam system containing the liquid transition metal chelate polyol blend is preferably within 20 seconds, more preferably within 10 seconds, and most preferably within 8 seconds. Compared with the surface dry time of the typical polyurethane foam of the same type without the liquid transition metal chelate polyol blend, the surface dry time of the foam system containing the liquid transition metal chelate polyol blend is preferably within 20 seconds, more preferably within 10 seconds, and most preferably within 8 seconds.

[0063] For typical PIR foam systems with or without liquid transition metal chelate polyol blends, the cream time is preferably in the range of 1 to 20 seconds, more preferably in the range of 3 to 15 seconds, even more preferably in the range of 5 to 12 seconds, and most preferably in the range of 6 to 10 seconds. For typical PIR foam systems with or without liquid transition metal chelate polyol blends, the gel time is preferably in the range of 15 to 60 seconds, more preferably in the range of 18 to 50 seconds, even more preferably in the range of 20 to 40 seconds, and most preferably in the range of 25 to 35 seconds. For typical PIR foam systems with or without liquid transition metal chelate polyol blends, the tack free time is preferably in the range of 30 to 120 seconds, more preferably in the range of 40 to 90 seconds, even more preferably in the range of 50 to 80 seconds, and most preferably in the range of 55 to 70 seconds.

[0064] For each embodiment, the reaction mixture can be used to form a polyurethane polymer or a polyurethane polymer foam. The method for preparing a reaction mixture for producing a polyurethane polymer or a polyurethane polymer foam can be achieved by any process technology known in the art. Generally, the polyurethane polymer foam of the present disclosure can be produced by a discontinuous or continuous process, including processes commonly referred to as discontinuous plate methods (DCP) and continuous lamination, wherein the foaming reaction and subsequent curing are carried out in a mold or on a conveyor. The method for forming a polyurethane polymer or a polyurethane polymer foam as provided herein can be carried out at a temperature of 15°C to 80°C and a mixing pressure of 80kPa to 25,000kPa. Mixing the components of the polyurethane foam can be carried out using a known mixing device. The density of the resulting polyurethane polymer foam can be 10kg / m 3 or higher, preferably 15kg / m 3 or higher, more preferably 25kg / m 3 or higher, most preferably 35kg / m 3 or higher, and at the same time usually 200kg / m 3 or less, preferably 100 kg / m 3 or less, more preferably 70kg / m 3 or less, and most preferably 50 kg / m 3 or smaller.

[0065] For various embodiments, the polyurethane polymer foam of the present disclosure provides low smoke generation and high thermal stability as determined according to ASTM E662 "Test Method for Specific Optical Density of Smoke Generated by Solid Materials". Lower maximum specific optical density (Max Ds) values ​​mean lower smoke generation. Lower mass loss % values ​​mean higher thermal stability. Max Ds may be 400 or less, preferably 200 or less, more preferably 100 or less, and also most preferably 50 or less. Mass loss % may be 50% or less, preferably 45% or less, more preferably 40% or less, and also most preferably 30% or less.

[0066] The polyurethane polymer foam of the present disclosure may have low thermal conductivity in applications such as for building insulation. The thermal conductivity of rigid foams is represented by the K factor. The K factor is a measure of insulation performance. The K factor of the prepared foam may be 30.0 mW / m·K or less, preferably 27.0 mW / m·K or less, more preferably 24.0 mW / m·K or less, and most preferably 22.0 mW / m·K or less. Thermal conductivity (K factor) is measured using ASTM C-518-17 at an average temperature of 75°F.

[0067] The applications of the polyurethane polymer foam produced by the present disclosure are those known in the industry. For example, polyurethane polymer foam can be used for the thermal insulation used in building walls and roofs, garage doors, transport trucks and rail cars, and cold storage facilities. The polyurethane polymer foam disclosed herein can have a combination of properties desired for these applications. For example, the polyurethane polymer foam disclosed herein can advantageously provide desired low thermal conductivity, smoke density, thermal stability, and improved combustion characteristics while reducing HCN and CO emissions.

[0068] The liquid transition metal chelate polyol blends and polyurethane polymers disclosed herein can also be used as, for example, coatings, elastomers, sealants, binders, adhesives or flexible foams. For use as coatings, elastomers, sealants, binders or adhesives, the reactants are preferably formulated into a two-component system (2K), one component containing a polyisocyanate (more preferably an isocyanate-terminated prepolymer or quasi-prepolymer), and the other component is an isocyanate-reactive composition containing at least one liquid transition metal chelate polyol blend, which imparts antifungal, antimicrobial, deodorizing, hardness, friction resistance, improved combustion performance and / or similar properties to the cured polyurethane product. For use as coatings, elastomers, sealants, binders or adhesives, the liquid transition metal chelate polyol blend with other optional polyols can be pre-reacted with an organic polyisocyanate to form a prepolymer or quasi-prepolymer containing isocyanate groups and used as a one-component (1K) curing system.

[0069] Some embodiments of the present disclosure will now be described in detail in the following examples.

[0070] Examples

[0071] Some embodiments of the present disclosure will now be described in detail in the following examples, wherein all parts and percentages are by weight unless otherwise specified. In the examples, the following materials and tests were used.

[0072] Material

[0073] Materials used in Examples and / or Comparative Examples include the following.

[0074] Polyol A is a polyester polyol (aromatic polyester polyol from terephthalic acid, polyethylene glycol 200 and diethylene glycol) having a hydroxyl value of 220 mg KOH / g and a functionality of 2, and a total content of aromatic parts of 14.8 wt.%.

[0075] Polyol B is a polyester polyol (aromatic polyester polyol from terephthalic acid, polyethylene glycol 200, glycerol and diethylene glycol) having a hydroxyl value of 315 mg KOH / g and a functionality of 2.4 with a total aromatic content of 17.4 wt.%.

[0076] Polyethylene glycol 200 (PEG 200) is available from TCI, USA.

[0077] 2,2'-Bipyridine (BIPY) is available from Sigma-Aldrich.

[0078] 2-[[2-(Dimethylamino)ethyl]methylamino]ethanol (TMDAOH) can be obtained from TCI, USA.

[0079] 1-[Bis[3-(dimethylamino)propyl]amino-2-propanol] is available from Sigma-Aldrich.

[0080] VORANOL TM RA 640 polyol is an amine initiated polyol having a hydroxyl value of 654 mg KOH / g and a viscosity of 21,500 cSt at 25°C, available from Dow.

[0081] N,N,N',N'-Tetramethylethylenediamine (TMEDA) can be obtained from TCI, USA.

[0082] Triethyl phosphate (TEP) is a flame retardant from LANXESS.

[0083] 5 is N,N,N',N',N"-pentamethyldiethylenetriamine (PMDTA) catalyst from Evonik Industries AG.

[0084] 46 is a catalyst from Evonik Industries AG.

[0085] Silicone surfactants are silicone rigid foam surfactants from Evonik Industries AG.

[0086] The water is deionized water having a specific resistivity of 10 MΩ×cm (million ohms) at 25°C.

[0087] Cyclopentane (c-Pentane) is a blowing agent from Sigma-Aldrich.

[0088] PAPI TM 580N is a polymethylene polyphenyl isocyanate from Dow Inc. containing methylene diphenyl diisocyanate (MDI) and having 30.8% isocyanate.

[0089] Copper(II) hydroxide (Cu(OH)2), technical grade, available from Sigma-Aldrich.

[0090] Copper(I) oxide (Cu2O), technical grade, available from Sigma-Aldrich.

[0091] Copper(II) 2-ethylhexanoate (CuEH) is available from Sigma-Aldrich.

[0092] Copper(II) acetate monohydrate (Cu(OAc)2H2O) can be obtained from Acros Organics.

[0093] Copper (II) isobutyrate (Cu(I-But)2) is available from Strem Chemical.

[0094] Cobalt(II) acetate tetrahydrate (Co(OAc)2 4H2O) was obtained from Across Organics.

[0095] Nickel(II) acetate tetrahydrate (Ni(OAc)2 4H2O) was obtained from Across Organics.

[0096] Silver(I) acetate (Ag(OAc)) is available from Fisher Scientific.

[0097] Preparation of Liquid Transition Metal Chelated Polyol Blends

[0098] By using a FlackTek SpeedMixer in a 250mL plastic container TM DAC600 FVZ mixed the polyol, transition metal compound and chelating agent in the amounts shown in Table 1 at 3000 rpm for 45 seconds to prepare each liquid transition metal chelate polyol blend (LPB) in Table 1. Next, the container was placed in a convection oven preheated to 80°C for 1 hour (h). After 1 h, the FlackTek SpeedMixer was used again. TM The LPB was mixed at 3000 rpm for 45 seconds.

[0099] In order to form a transition metal-containing LPB, an organic transition metal salt is used as a transition metal compound and a derivative of an amine-based chelating agent is used as a chelating agent, wherein the molar ratio (N / M) of nitrogen (N) from the amine-based chelating agent to the transition metal (M) from the organic transition metal salt is greater than 1.1, as shown in Table 1.

[0100] Table 1 - Composition of Liquid Transition Metal Chelate Polyol Blend (LPB) Inventive (EX) and Comparative (C EX) Compositions

[0101]

[0102] Preparation of polyurethane foams using liquid transition metal chelated polyol blends

[0103] The following components were used in the reaction mixture (Table 2) to form polyurethane foams for the inventive examples (EX) and comparative examples (C Ex). The amount of each component is given in parts by weight (PBW), based on the total weight of the reaction mixture used to form the polyurethane foam.

[0104] Table 2 - Reaction mixtures of polyurethane foams using LPB

[0105]

[0106] Wt. %* - Weight percentages are based on the total weight of the reaction mixture.

[0107] Prepare polyurethane foam as follows. Prepare the reaction mixture of 80 grams (g) of each EX and C EX provided in Table 2 in a 500mL beaker. The components of the isocyanate reactive composition provided in Table 2 were mixed with a rotary mixer at 3000rpm for 10 seconds (s). Next, the isocyanate reactive composition and isocyanate were mixed again in a beaker at 3000rpm for 5 seconds at room temperature (23°C, 50% relative humidity). After 24 hours (h), remove the foam part that has risen above the top plane of the beaker, and then cut off the center core of 2.54cm x 2.54cm x 2.54cm. Cream time is defined as the time from the preparation of the reaction mixture to the identifiable start of the foaming mixture, such as the visual change of the reactant (color change and / or start to rise). Gel time (or string time) is defined as the time from the preparation of the reaction mixture to the time when the fluid state is changed to the solid state. It is determined by repeatedly immersing and pulling out the wooden tongue pressure plate in the reaction mixture. The gel time is reached as soon as a string is formed when the wooden tongue pressure plate is pulled out of the reaction mixture. The tack free time is defined as the time from the preparation of the foam reaction mixture until the foam surface is no longer tacky. It is determined by depositing the wooden tongue pressure plate on the foam surface. The tack free time is reached if lifting the wooden tongue pressure plate does not cause delamination or cracking of the foam surface, in other words, when the foam surface is no longer tacky.

[0108] Flue gas composition analysis

[0109] Pyrolysis tests were performed using a Frontier Labs 2020D pyrolyzer mounted on an Agilent 6890GC with a flame ionization detector (FID). Approximately 200-250 μg of sample was weighed into a Frontier labs silica gel lined stainless steel cup. Pyrolysis was performed in single shot mode by placing the sample cup in an oven and analyzing it for 2 min under air conditions at 600 ° C and then for another 2 min under helium conditions. A micro cryogenic trap (MCT) was used to capture volatile products emitted from the sample at the top of the separation column. A 10mx 0.32mm ID x 5μm PoraBond Q column from Agilent was used to achieve separation with HP-1 (10m x 0.53mm x 2.65μm) as a guard column. The back injection port pressure was used for backflush purposes (0.5mx 0.53mm guard column, using the back injection port as its top pressure tee in the PoraBond Q and HP-1 columns). HCN was detected on the backside FID detector. HCN concentration comparisons were made using HCN peak areas normalized to sample weight.

[0110] GC conditions: front inlet: 300°C; 1:1 split injector; ramp pressure: 4.9 psi for 1.5 min, then increased to 3.1 psi at 50 psi / min; back inlet: 4 psi; GC oven: 40°C for 3 min, increased to 240°C at 30°C / min; FID: 250°C, H2 flow rate: 40 mL / min, air flow rate: 450 mL / min, tail gas (N2): 30 mL / min, 50 Hz.

[0111] Relative isocyanurate content measurement

[0112] Attenuated total reflection Fourier transform infrared spectroscopy (ATR-FTIR) measurements were performed on a Nicolet iS50 FT-IR instrument with a SMART iTX single reflection diamond ATR. -1 Spectral range: 4 cm -1 Sixteen scans were collected at a resolution of 1000 nm. A rectangular cross section (10 mm x 60 mm) was cut from the center of the molded polyurethane-based foam sample. The cross section was tested three times and the three measurements of the characteristic peaks were averaged. The relative isocyanurate content was defined as the height of the characteristic peak of the isocyanurate group (about 1409 cm -1 ) and the phenyl characteristic peak height (about 1595cm -1) is a ratio normalized by the peak height ratio of a comparative control example not containing a transition metal.

[0113] result

[0114] As shown in Table 2, the use of foams containing copper-containing liquid transition metal chelate polyol blends can significantly reduce the generation of HCN. These examples show similar reactivity to CEX A.

Claims

1. A liquid transition metal chelated polyol blend comprising: A polyol, wherein the polyol is an aromatic polyester polyol having an aromatic portion, the aromatic portion constituting 5 wt.% to 60 wt.% of the total weight of the aromatic polyester polyol; 0.05 wt.% to 10.0 wt.% of transition metal ions from a transition metal compound, the wt.% being based on the total weight of the liquid transition metal chelate polyol blend; wherein the transition metal compound is selected from the group consisting of: copper (II) 2-ethylhexanoate, copper (II) acetate, copper (II) acetate monohydrate (Cu(OAc) 2 ·H 2 O), copper (II) propionate, copper (II) isobutyrate, cobalt (II) acetate, nickel (II) acetate, and combinations thereof; a chelating agent having a nitrogen-based chelating moiety, wherein the liquid transition metal chelate polyol blend has from 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 grams (g) of the polyol in the liquid transition metal chelate polyol blend, and the molar ratio of nitrogen in the nitrogen-based chelating moiety to the transition metal ion is from 8.0:1.0 to 1.0:1.0; and The liquid transition metal chelate polyol blend comprises less than 0.10 wt.% of transition metal compound particles based on the weight of the liquid transition metal chelate polyol blend, is liquid at a pressure of 80 to 25,000 kPa and is liquid at a temperature above -10°C and below 80°C.

2. The liquid transition metal chelate polyol blend of claim 1, wherein the nitrogen-based chelating moiety is selected from the group consisting of a diamine chelating moiety, a triamine chelating moiety, a tetraamine chelating moiety, and combinations thereof.

3. The liquid transition metal chelate polyol blend of claim 1, wherein the chelating agent having a nitrogen-based chelating moiety is selected from the group consisting of 2,2'-bipyridine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N',N"-pentamethyldiethylenetriamine, 2-[[2-(dimethylamino)ethyl]methylamino]ethanol, 1-[bis[3-(dimethylamino)propyl]amino-2-propanol], 1,2-ethylenediamine polymers with methyloxirane, and combinations thereof.

4. An isocyanate-reactive composition comprising: The liquid transition metal chelate polyol blend according to any one of claims 1 to 3; and A polyol separated from the polyol of the liquid transition metal chelate polyol blend, wherein the isocyanate-reactive composition comprises 0.1 to 100 wt. % of the liquid transition metal chelate polyol blend and up to 99.9 wt. % of the polyol separated from the polyol of the liquid transition metal chelate polyol blend to form the isocyanate-reactive composition, the wt. % being based on the total weight of the isocyanate-reactive composition.

5. The isocyanate-reactive composition of claim 4, further comprising 0.1 wt.% to 7.0 wt.% of phosphorus from a flame retardant compound selected from the group consisting of phosphates, phosphonates, phosphinates, phosphites, and combinations thereof, the wt.% being based on the total weight of the isocyanate-reactive composition; or Also comprising a catalyst, a blowing agent and a surfactant for forming a polyurethane polymer foam; or Optionally, water is also included for forming the polyurethane polymer foam.

6. A reaction mixture for forming a polyurethane polymer, comprising: an isocyanate compound having an isocyanate moiety; and The isocyanate-reactive composition of any one of claims 4-5, wherein the polyol comprises hydroxyl moieties and the molar ratio of the isocyanate moieties to the hydroxyl moieties of the reaction mixture is from 0.90:1 to 7:

1.

7. The reaction mixture of claim 6, wherein the polyurethane polymer is a polyurethane foam.

8. A method for preparing the liquid transition metal chelate polyol blend according to claim 1, wherein the method include: Providing a polyol, wherein the polyol is an aromatic polyester polyol having an aromatic portion, the aromatic portion constituting 5 wt.% to 60 wt.% of the total weight of the aromatic polyester polyol; providing a chelating agent having a nitrogen-based chelating moiety; A transition metal compound having a transition metal ion is provided; wherein the transition metal compound is selected from the group consisting of: copper (II) 2-ethylhexanoate, copper (II) acetate, copper (II) acetate monohydrate (Cu(OAc) 2 ·H 2 O), copper (II) propionate, copper (II) isobutyrate, cobalt (II) acetate, nickel (II) acetate, and combinations thereof; mixing the polyol, the chelating agent, and the transition metal compound to form the liquid transition metal chelate polyol blend having 0.001 to 1.0 mole of nitrogen in the nitrogen-based chelating moiety per 100 grams of the polyol in the liquid transition metal chelate polyol blend, and a molar ratio of nitrogen in the nitrogen-based chelating moiety to the transition metal ion of 8.0:1.0 to 1.0:1.0; The liquid transition metal chelate polyol blend further comprises 0.05 wt. % to 10.0 wt. % of transition metal ions from a transition metal compound, the wt. % being based on the total weight of the liquid transition metal chelate polyol blend.

9. A method for preparing a reaction mixture for producing a polyurethane polymer, the method comprising: include: Providing an isocyanate reactive composition according to any one of claims 4-5, wherein the polyol comprises a hydroxyl moiety; providing an isocyanate compound having an isocyanate moiety; and The isocyanate-reactive composition and the isocyanate compound are mixed to form the reaction mixture having a molar ratio of the isocyanate moieties to the hydroxyl moieties of 0.90:1 to 7:1.