Forging process of large medium-pressure transition flange for steam turbine

By adopting specific process routes and process parameters in the forging of large-scale medium-pressure transition flanges of steam turbines, the problem of inner hole forging cracks has been solved, the finished product qualification rate and material properties have been improved, and the high-temperature creep and corrosion of ultra-supercritical generator sets have been met. Require.

CN114130933BActive Publication Date: 2024-10-18WUXI HONGDA HEAVY IND
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202111359781.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-17
Publication Date
2024-10-18
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

The existing forging process is prone to inner hole forging cracks in the forging of large-scale medium-pressure transition flanges of steam turbines, resulting in a low pass rate of finished products and unable to meet the high-temperature creep and corrosion requirements of supercritical and ultra-supercritical power generation units.

Method used

Adopting a process route including blanking, forging, post-forging high-temperature isothermal tempering, conventional isothermal annealing, rough machining, quenching, tempering, sampling, sample processing, tensile testing and Charpy impact testing, through five fire process parameters Conduct grain refinement heat treatment with near-net-shape tooling molds to control forging composition and process parameters to ensure the stability and reliability of inner hole forging.

Benefits of technology

It improves the finished product qualification rate of large medium-pressure transition flanges of steam turbines, reduces material usage and manufacturing costs, improves high-temperature creep strength and impact toughness, and meets the mechanical performance requirements of ultra-supercritical boilers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114130933B_ABST
    Figure CN114130933B_ABST
Patent Text Reader

Abstract

The present invention provides a forging process for a large medium-pressure transition flange of a steam turbine, which ensures the stability and reliability of the inner hole forging and improves the qualified rate of finished products. The forging process for a large medium-pressure transition flange of a steam turbine is characterized in that it includes the following process routes: blanking - forging - high temperature isothermal tempering after forging - conventional isothermal annealing - rough machining - quenching - tempering - sampling - sample processing - tensile test and Charpy impact test - test report - technical analysis; the forging process includes the following steps: a. the first three fires are blanking, upsetting, 1200 wide anvil method center compaction, upsetting, punching and blanking; b. the fourth fire forms a preset forging size; c. the fifth fire uses a near-net-shaped tooling die for extrusion molding and performs a near-net-shaped extrusion riveting and upsetting process; the high temperature isothermal tempering after forging and the conventional isothermal annealing are subjected to grain refinement heat treatment at two different austenitizing temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of forging technology, in particular to a forging technology for a large medium-pressure transition flange of a steam turbine. Background Art

[0002] The requirements of supercritical and ultra-supercritical generating units for existing materials are mainly reflected in high temperature corrosion resistance and high temperature creep limit. F92 is a new type of ferrite heat-resistant steel developed by Japan Steel Corporation and recognized and approved by ASME in October 1999. It is based on F91 and adds a certain amount of tungsten and boron. Through W-Mo composite solid solution strengthening and B grain boundary strengthening, its high temperature creep limit is further improved, which not only saves material consumption and reduces manufacturing costs, but also because this material has a higher thermal conductivity and lower thermal expansion coefficient, which reduces the thermal fatigue loss of components and enables the unit to work more stably for a longer period of time. The manufacture of forgings made of materials such as F92, F91 and WB36 and their corresponding standard pipe fittings (pipe joints) has high technical content, complex processes, high equipment capacity requirements, and high requirements for supporting equipment.

[0003] With the increase of boiler steam temperature and pressure, it is required to use new creep-resistant steel suitable for high-temperature pressure structure to improve boiler efficiency. Japan's Nippon Steel Corporation further developed NF616 (T / P92) heat-resistant steel with higher strength grade based on SA-335P91. SA-182F92 (hereinafter referred to as F92) is a series of alloy forgings in 92-grade steel, mainly used for the spherical head of the last superheater header and the last reheater header in ultra-supercritical pressure boilers, inspection hole pipe joints, etc. F92 steel has a high content of alloy elements, a high tendency to harden in welded joints, and is prone to produce martensitic structure, which will produce cold cracks under the combined action of hydrogen and stress. The existing process is prone to internal hole forging cracks when forging large medium-pressure transition flanges of steam turbines, resulting in scrapping. Therefore, it is urgent to find a forging process that can improve the qualified rate of finished products. Summary of the invention

[0004] In view of the above problems, the present invention provides a forging process for a large medium-pressure transition flange of a steam turbine, which ensures the stability and reliability of the inner hole forging and improves the qualified rate of finished products.

[0005] The forging process of a large medium-pressure transition flange of a steam turbine is characterized in that it includes the following process routes:

[0006] Cutting - forging - high temperature isothermal tempering after forging - conventional isothermal annealing - rough machining - quenching - tempering - sampling - specimen processing - tensile test and Charpy impact test - test report - technical analysis;

[0007] The forging process includes the following steps:

[0008] a The first three fires are blanking, upsetting, 1200 wide anvil center compaction, upsetting, and punching.

[0009] b. The fourth fire uses a 600-width upper flat anvil, a lower V-shaped anvil, and a mandrel to alternately pull the right step to the remaining size and the left step to the remaining size according to the designed shape. The pressing amount during the pulling process is ≤50mm, and the forging is fast. Finally, the middle large circle is rounded to the remaining deformation size to form the preset forging size;

[0010] c The fifth fire is to extrude and form with a near-net-shape tooling die, and perform a near-net-shape extrusion riveting and upsetting process. The near-net-shape tooling die includes an upper die and a lower die frame. The upper die includes a first leaking plate with a four-sided profiling and a center punch assembly. The lower die frame includes a second leaking plate with a four-sided convex profiling. After the middle large circle of the forging is supported on the lower die frame, the upper die is pressed down to complete the near-net shape of the forging die and the design drawing;

[0011] The post-forging high temperature isothermal tempering and conventional isothermal annealing are used for grain refinement heat treatment through two different austenitizing temperatures.

[0012] It is further characterized by:

[0013] The composition contents in the forging process are as follows: 0.10-0.13wt% C, ≤0.30wt% Si, 0.30-0.40wt% Mn, ≤0.015wt% P, ≤0.010wt% S, 8.65-9.40wt% Cr, 0.45-0.60wt% Mo, 0.10-0.15wt% Ni, 0.18-0.25wt% V, 0.06-0.07wt% t% Nb, 0.04-0.05wt% N, 1.55-1.95wt% W, 0.003-0.004wt% B, ≤0.10wt% Cu, ≤0.010wt% Sn, ≤0.007wt% Pb, ≤0.0015wt% Sb, ≤0.010wt% As, ≤0.010wt% Bi, ≤20PPm O, ≤1.7ppm H, the rest is Fe;

[0014] Its adjustment is beneficial to reduce high temperature ferrite forming elements, refine grains, improve impact toughness beneficial elements, reduce five small harmful elements, control H, O, N content within a certain range, meet the mechanical properties requirements and high temperature creep strength;

[0015] The process parameters of the five fires in the forging process are as follows: the first fire is 1220℃~900℃, for riser removal and surface compaction process;

[0016] The second fire is 1250℃~900℃, and the center compaction process is carried out with a 1200 wide anvil and a large reduction;

[0017] The third heat is 1250℃~900℃, and the upsetting and punching blank making process is carried out;

[0018] The fourth fire is 1220℃~850℃, and the mandrel and V-shaped anvil are stretched and preformed;

[0019] The fifth fire is 1150℃~850℃, implementing the near-net-shape extrusion riveting and upsetting process to control the grain size;

[0020] The process parameters of the high temperature isothermal tempering are as follows: preheat at 650°C for 2-3h, then keep at 785°C for 10-12h, then increase the power to 1070°C-1100°C±10°C, keep for 6-8h; then furnace cool or air cool; isothermal at 770°C, keep for 12-15h, and air cool;

[0021] The process parameters of the conventional isothermal annealing are as follows: first, keep warm at 650°C for 2-3h, then keep warm at 785°C for 10-12h, increase the power to 950-980°C±10°C, keep warm for 6-8h; then furnace cool or air cool; isothermal at 770°C, keep warm for 12-15h, and air cool.

[0022] After adopting the process of the present invention, the FM method pressing amount of the lower platform and the upper 800mm anvil is replaced by the pressing amount of the 1200mm wide anvil, so as to better implement the core compaction and organization improvement of the blank and reduce the generation of surface cracks; the workpiece blank is subjected to the near-net-forming extrusion riveting and upsetting process through the near-net-forming tooling die, so that the entire outer surface, the inner hole and the inside of the material are in a uniform compressive stress state, which is conducive to the full forging of internal defects generated in the blank making stage and ensures that the flaw detection meets the technical requirements; then, the grain refinement heat treatment is carried out through two isothermal annealing treatments at different austenitizing temperatures, which ensures the stability and reliability of the inner hole forging and improves the qualified rate of finished products. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a finished product size drawing of a specific embodiment of the present invention;

[0024] Figure 2 It is a dimension drawing of a forging after the fourth fire of a specific embodiment of the present invention;

[0025] Figure 3 It is a dimensional drawing of a forging after a near-net-shape extrusion riveting and upsetting process according to a specific embodiment of the present invention;

[0026] Figure 4 It is a schematic diagram of the process flow of the near-net-shape extrusion riveting and upsetting process of the present invention;

[0027] The names corresponding to the serial numbers in the figure are as follows:

[0028] An upper die 10 , a first leaking disc 11 , a center punch assembly 12 , a lower die frame 20 , a contoured second leaking disc 21 , and a forging 30 . DETAILED DESCRIPTION

[0029] Forging process of large medium pressure transition flange for steam turbine, specific embodiment, its finished product size see Figure 1 , the preset forging dimensions after forging are shown in Figure 3 , which includes the following process routes:

[0030] Cutting - forging - high temperature isothermal tempering after forging - conventional isothermal annealing - rough machining - quenching - tempering - sampling - specimen processing - tensile test and Charpy impact test - test report - technical analysis;

[0031] Specifically, the forging process includes the following steps:

[0032] a The first three fires are blanking, upsetting, 1200 wide anvil center compaction, upsetting, and punching.

[0033] b The fourth fire uses a 600-width upper flat anvil, a lower V-shaped anvil, and a Φ530 mandrel to alternately pull the right step to 1000 and the left step to Φ1320 according to the designed shape. The pressing amount during the pulling process is ≤50mm, and the forging is fast. Finally, the middle large circle is rounded to Φ1500 to form the preset forging size (see Figure 2 );

[0034] c The fifth fire is extruded with a near net shape tooling die and a near net shape extrusion riveting process is performed. The near shape tooling die (see Figure 4 ) includes an upper die 10 and a lower die frame 20. The upper die 10 includes a first leaking plate 11 with a circumferential profiling and a center punch assembly 12. The lower die frame 20 includes a second leaking plate 21 with a circumferential convex profiling. After the middle large circle of the forging 30 is supported on the lower die frame 20, the upper die 10 is pressed downward to complete the forging die and the near-net shape of the design drawing (see Figure 3 );

[0035] High temperature isothermal tempering and conventional isothermal annealing after forging are used for grain refinement heat treatment at two different austenitizing temperatures.

[0036] The forging component contents in the forging process, except for Fe, are shown in Table 1:

[0037] Table 1

[0038]

[0039] Its adjustment is beneficial to reduce high temperature ferrite forming elements, refine grains, improve impact toughness beneficial elements, reduce harmful elements, control H, O, N content within a certain range, and meet mechanical property requirements and high temperature creep strength;

[0040] The process parameters of the five fires in the forging process are as follows: the first fire is 1220℃~900℃, and the riser removal and surface compaction process are carried out; the second fire is 1250℃~900℃, and the center compaction process with a large reduction amount of a 1200 wide anvil is implemented; the third fire is 1250℃~900℃, and the upsetting and punching process is implemented; the fourth fire is 1220℃~850℃, and the mandrel and V-shaped anvil are drawn and preformed; the fifth fire is 1150℃~850℃, and the near-net-shape extrusion riveting process is implemented to control the grain size;

[0041] The process parameters of high temperature isothermal tempering are as follows: preheat at 650℃ for 2-3h, then keep at 785℃ for 10-12h, then increase the power to 1070℃-1100℃±10℃, keep for 6-8h; then furnace cool or air cool; then isothermally keep at 770℃ for 12-15h, air cool;

[0042] The process parameters of conventional isothermal annealing are as follows: first keep at 650℃ for 2-3h, then keep at 785℃ for 10-12h, increase the power to 950-980℃±10℃, keep for 6-8h; then furnace cool or air cool; then isothermally keep at 770℃ for 12-15h, and air cool.

[0043] The forgings made by the forging process have the following mechanical properties: 40MPa; grain size: the overall grain size reaches above level 3, and the grain size difference is not greater than level 2; ultrasonic and magnetic particle inspection: the qualified rate reaches 100%; gross to net weight ratio: the weight of F92 medium-pressure transition flange forgings is reduced from 18747Kg to 15447Kg, achieving a material saving of 20% to 30% and a reduction of machining hours by 50%.

[0044] Its adjustment is beneficial to reduce high-temperature ferrite forming elements, refine grains, improve impact toughness beneficial elements, reduce five small harmful elements, control H, O, N content within a certain range, meet mechanical performance requirements and high-temperature creep strength; in the early stage of billet making, the FM method is improved to implement 1200mm wide anvil compaction, and the reduction amount is reduced from 20% to 15%, which effectively improves the surface stress state of the billet and prevents the billet from cracking, cracking and other surface defects; design a special tool and die, the die consists of a lower die frame, an upper die and a punch, and the tool and die are rationally optimized and designed through finite element calculation and numerical simulation analysis to reduce the weight of the die, ensure that the last fire extrusion riveting and upsetting forming can make the forgings in a uniform extrusion stress state, thereby effectively improving the last fire forging stress state to be a compressive stress state; its grain refinement heat treatment, take measures to increase the heating speed of the workpiece; adopt different higher austenitizing temperatures and different cooling methods, and perform isothermal annealing treatments at two different austenitizing temperatures; find the best heat treatment process parameters to obtain the grain size that meets the customer's technical requirements.

[0045] Its working principle is as follows: rationalize the element range of grain refinement, control harmful elements, control the contents of O and H within 20ppm and 1.7ppm, and complete composition optimization; replace the FM method reduction of the lower platform and the upper 800mm anvil with the reduction of the 1200mm wide anvil, better implement the core compaction and organization improvement of the billet, and reduce the generation of surface cracks; use the near-net-forming tooling die to perform near-net-forming extrusion riveting and upsetting process on the workpiece billet, so that the entire outer surface, inner hole and the inside of the material are in a uniform compressive stress state, which is conducive to the full forging of internal defects generated in the billet making stage, and ensure that the flaw detection meets the technical requirements; then, the grain refinement heat treatment is carried out through two isothermal annealing treatments at different austenitizing temperatures, which ensures the stability and reliability of the inner hole forging and improves the qualified rate of finished products.

[0046] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0047] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. The forging process of large medium-pressure transition flange for steam turbine is characterized by: It includes the following process routes: Cutting - forging - high temperature isothermal tempering after forging - conventional isothermal annealing - rough machining - quenching - tempering - sampling - specimen processing - tensile test and Charpy impact test - test report - technical analysis; The forging process includes the following steps: a The first three fires are blanking, upsetting, 1200 wide anvil center compaction, upsetting, and punching; b. The fourth fire uses a 600-width upper flat anvil, a lower V-shaped anvil, and a mandrel to alternately pull the right step to the remaining size and the left step to the remaining size according to the designed shape. The pressing amount during the pulling process is ≤50mm, and the forging is fast. Finally, the middle large circle is rounded to the remaining deformation size to form the preset forging size; c The fifth fire is to extrude and form with a near-net-shape tooling die, and perform a near-net-shape extrusion riveting and upsetting process. The near-net-shape tooling die includes an upper die and a lower die frame. The upper die includes a first leaking plate with a four-sided profiling and a center punch assembly. The lower die frame includes a second leaking plate with a four-sided convex profiling. After the middle large circle of the forging is supported on the lower die frame, the upper die is pressed down to complete the near-net shape of the forging die and the design drawing; The post-forging high temperature isothermal tempering and conventional isothermal annealing are performed through two different austenitizing temperatures to perform grain refinement heat treatment; The composition contents in the forging process are as follows: 0.10-0.13wt% C, ≤0.30wt% Si, 0.30-0.40wt% Mn, ≤0.015wt% P, ≤0.010wt% S, 8.65-9.40wt% Cr, 0.45-0.60wt% Mo, 0.10-0.15wt% Ni, 0.18-0.25wt% V, 0.06-0.07wt% t% Nb, 0.04-0.05wt% N, 1.55-1.95wt% W, 0.003-0.004wt% B, ≤0.10wt% Cu, ≤0.010wt% Sn, ≤0.007wt% Pb, ≤0.0015wt% Sb, ≤0.010wt% As, ≤0.010wt% Bi, ≤20PPm O, ≤1.7ppm H, the rest is Fe; Its adjustment is beneficial to reduce high temperature ferrite forming elements, refine grains, improve impact toughness beneficial elements, reduce harmful elements, control H, O, N content, meet mechanical property requirements and high temperature creep strength; The first fire in the forging process is 1220℃~900℃, which is used to remove the riser and compact the surface; The second fire in the forging process is 1250℃~900℃, and the center compaction process with a 1200 wide anvil and large reduction is implemented; The third heat in the forging process is 1250℃~900℃, and the upsetting and punching blank making process is carried out; The fourth fire in the forging process is 1220℃~850℃, and the mandrel and V-shaped anvil are stretched and preformed; The fifth heat in the forging process is 1150℃~850℃, and the near-net-shape extrusion riveting and upsetting process is implemented to control the grain size; The process parameters of the high temperature isothermal tempering are as follows: preheat at 650°C for 2-3h, then keep at 785°C for 10-12h, then increase the power to 1070°C-1100°C±10°C, keep for 6-8h; then furnace cool or air cool; isothermal at 770°C, keep for 12-15h, and air cool; The process parameters of the conventional isothermal annealing are as follows: first, keep warm at 650°C for 2-3h, then keep warm at 785°C for 10-12h, increase the power to 950-980°C±10°C, keep warm for 6-8h; then furnace cool or air cool; isothermal at 770°C, keep warm for 12-15h, and air cool.

Citation Information

Patent Citations

  • Forging method for thin-walled step short sleeve type main shaft flange of water turbine

    CN102527897A

  • Planet carrier flange forge piece forging process

    CN103212948A

  • Hollow forging piece profiling forging method of overlong-asymmetric-pipe-mouth-contained reactor coolant piping

    CN105033132A

  • Method for manufacturing spindle of large monoblock forged water turbine

    CN106040952A

  • Manufacturing process for manufacturing large ship-used shafting forge pieces

    CN108453202A