An agile gas throttle with gradient pore structure and preparation method thereof
By adopting an agile gas restrictor with a gradient pore structure in the space electric propulsion system, Fe-Ni-Cr-Mo alloy and nano-porous coating technology are used to solve the shortcomings of the metal porous core in gas micro-flow control. It achieves gas throttling effect with high precision, stability and safety, and is suitable for single piece or small batch customization.
Patent Information
- Application Number
- CN202111417123.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The existing metal porous throttling cores in space electric propulsion systems have problems such as large flow resistance dispersion, low precision, poor flow customization capabilities, poor stability, easy clogging and low production efficiency. It is difficult to achieve high precision and low gas micro-flow. Lightweight and miniaturized control.
An agile gas restrictor with a gradient pore structure is used. Fe-Ni-Cr-Mo alloy material is combined with 3D printing and nano-porous coating technology to prepare a gradient material structure composed of a dense layer and a porous layer to achieve gas flow control. Stable and precise control.
It improves the stability and accuracy of flow, reduces sample heterogeneity, improves production efficiency, ensures the safety and high performance of the propeller, and is suitable for single-piece or small batch customization.
Smart Images

Figure CN114165400B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to electric propulsion systems for space applications. In space propulsion systems, especially when Hall electric thrusters are working, a stable micro-flow gas propellant needs to be provided to the system. Its application goal is to effectively control the decompression and partial pressure of the micro-flow of gas during the electric propulsion process in a high-pressure source gas environment to achieve a stable flow control effect. Maintain the stability, directionality and constancy of the gas after the flow is blocked, and provide a stable micro-flow gas to the electric propulsion system. Background Art
[0002] The choke, partial pressure and micro-flow control of gas propellant in space electric propulsion system is realized by the thermal valve of storage and supply unit, which is called micro-throttle. It is the key device to realize the small gas pressure and stable gas micro-flow required by electric thruster from high-pressure gas environment.
[0003] In the process of achieving pressure control, the micro-throttle requires a throttling core, and the throttling core must be a porous structure to achieve the regulation, partial pressure, flow resistance and stability of the micro-flow of gas propellant. Therefore, the porous throttling core is a key component for regulating the gas propellant within a certain gas range. Its porous and mechanical properties are key performances to ensure the accuracy and life of the micro-throttle of the electric propulsion system.
[0004] At present, there are the following problems in the application of metal porous throttling core:
[0005] ① Large flow resistance and dispersion difference, low precision, and poor mechanical properties;
[0006] ②Poor traffic customization capability and stability;
[0007] ③ It is difficult to control the pore size and uniform distribution of materials when making porous materials. The vent holes are easily blocked during use, threatening the safety of the propeller;
[0008] ④ The flow consistency of the metal porous material core is poor, making it difficult to achieve effective control of the gas in an agile, lightweight and miniaturized manner.
[0009] In addition, the current flow consistency of metal porous cores is poor, and screening is required among a large number of samples to meet the sample requirements for flow control consistency. The selection ratio is almost 10%, that is, if 10 samples with good consistency are needed, 100 samples must be produced for selection. The production efficiency is low, the sample heterogeneity is poor, and the cost is high. These are all problems that urgently need to be solved when metal porous material cores are applied to micro gas throttles. Summary of the invention
[0010] In order to solve the problems of the prior art, the purpose of the present invention is to overcome the shortcomings of the existing technology and provide an agile gas throttle with a gradient pore structure and a preparation method thereof. The gradient pore structure micro gas throttle prepared by the present invention is suitable for flexible customization of single or small batch porous core samples, with high control accuracy, excellent mechanical properties, good flow stability, and protection of the safety of the propeller. The gradient pore structure micro gas throttle implemented by the present invention has high production efficiency and good sample heterogeneity, overcoming the shortcomings of poor flow consistency of the current metal porous core.
[0011] In order to achieve the above object, the present invention adopts the following technical scheme:
[0012] An agile gas throttle with a gradient pore structure, wherein the main component of the throttle is a Fe-Ni-Cr-Mo alloy, and the throttle is a structure combining an outer dense layer and a middle air-permeable cylindrical part, wherein the outer dense layer is in the form of a tube wall, and the middle air-permeable cylindrical part is arranged in the cavity of the outer dense layer; Fe-Ni-Cr-Mo alloy powder is used as a raw material, and a 3D printing method is used to prepare an integrated middle air-permeable cylindrical part and an outer dense layer of the throttle, wherein the cylindrical side wall is a dense structure with a relative density of 100%, and the pores are The degree is zero; the middle air-permeable cylindrical part is a porous structure with a relative density of 5-92%, so that the throttle presents a gradient material structure from pores to dense in the radial direction; along the air flow direction, a nanoporous coating is also arranged, the nanoporous coating is arranged in the outer dense layer cavity, and is close to the end of the middle air-permeable cylindrical part, the nanoporous coating is combined with the middle air-permeable cylindrical part to form a composite material air-permeable core; the outer dense layer, the middle air-permeable cylindrical part and the nanoporous coating form an agile gas throttle with a gradient pore structure.
[0013] Preferably, the relative density of the porous structure of the central air-permeable cylindrical portion is 5-80%; further preferably, the relative density of the porous structure of the central air-permeable cylindrical portion is 5-50%.
[0014] Preferably, the pore size of the porous structure of the central air-permeable cylindrical portion is 5-53 μm.
[0015] Preferably, the composition of the Fe-Ni-Cr-Mo alloy is as follows in terms of mass percentage:
[0016]
[0017] Wherein, the main element is Fe.
[0018] Further preferably, the composition of the Fe-Ni-Cr-Mo alloy is as follows in terms of mass percentage:
[0019]
[0020] Wherein, the main element is Fe.
[0021] Preferably, the end of the middle air-permeable cylindrical part prepared by the 3D printing method is subjected to a coating heat treatment, and the coating heat treatment process is as follows:
[0022] The material of the coating is Fe-Cr-Ni-Mo-Al alloy or Fe-Ni-Cr-Mo alloy; the temperature of the coating heat treatment process is 900-1020°C, and the insulation time is 1-4h.
[0023] Preferably, when using the 3D printing method, the Fe-Ni-Cr-Mo alloy powder is a spherical particle powder with a mesh size of 200-400.
[0024] Further preferably, when using the 3D printing method, the Fe-Ni-Cr-Mo alloy powder adopts spherical particle powders with different particle size gradations of 200 mesh, 300 mesh and 400 mesh, and the spherical powders of 200 mesh, 300 mesh and 400 mesh are mixed in a mass ratio of 1:1:(1-2).
[0025] Preferably, the diameter of the central air-permeable cylindrical portion is 5 to 15 mm.
[0026] Preferably, the height of the central air-permeable cylindrical portion is at least 10 mm.
[0027] Preferably, in an air flow environment, when the initial gas pressure is 0.2-0.5 MPa, the gas flow rate after being throttled by the gas throttle is 0.1-2000 mg / s.
[0028] A method for preparing an agile gas throttle with a gradient pore structure of the present invention, using a 3D printing method combined with a coating heat treatment method, the steps of which are as follows:
[0029] (1) Preparation of the main structure of density gradient material:
[0030] Fe-Ni-Cr-Mo alloy spherical particle powders of different particle size distributions of 200-400 mesh are mixed in a set ratio as forming material powders, and a 3D printing method is used to prepare a middle air-permeable cylindrical part with pores on the X and Y axes, so that the porosity is 5-92%; there is no pore on the Z axis of the middle air-permeable cylindrical part, the density is 100%, and the diameter of the middle air-permeable cylindrical part is 5-15mm; a cylindrical side wall dense structure adapted to the middle air-permeable cylindrical part is prepared, the relative density is 100%, and the porosity is zero; the throttle presents a gradient material structure from pores to dense in the radial direction, and a density gradient material main structure is obtained;
[0031] (2) Preparation of composite material breathable core:
[0032] The main structure of the density gradient material prepared by 3D printing is heat treated by the coating heat treatment method, and a nanoporous coating of Fe-Cr-Ni-Mo-Al alloy or Fe-Ni-Cr-Mo alloy is used. The nanoporous coating is arranged on the end surface of the middle breathable cylindrical part along the air flow direction, and the temperature of the coating heat treatment process is controlled to be 900-1020℃, and the insulation time is 1-4h, so that the nanoporous coating is tightly combined with the end of the middle breathable cylindrical part to form a composite material breathable core, so that the outer dense layer, the middle breathable cylindrical part and the nanoporous coating form an agile gas throttle with a gradient pore structure.
[0033] Preferably, in the step (1), when performing 3D printing, the process parameters are scanning spacing: 0.11-0.12 mm, laser power: 201-130 w, scanning speed: 900-1050 m / s, and layer thickness 15-20 microns;
[0034] Preferably, in the step (2), when the coating heat treatment process is performed, the temperature is controlled to be 950-980° C. and the insulation time is 2-4 hours.
[0035] Compared with the prior art, the present invention has the following obvious outstanding substantial features and significant advantages:
[0036] 1. The throttle of the present invention has a scale change of pore structure in the axial direction from the micron level of 5-53 microns in the middle air-permeable cylindrical part to the nanometer level of 2-50 nanometers in the outer dense layer. The pores in the axial direction of the micro gas throttle have gradient functional structural characteristics, so that it can achieve a good throttling effect;
[0037] 2. The present invention focuses on the problems existing in the application of metal porous material throttling core in micro gas throttling device, and relates to a metal porous gas throttling device with high-precision porosity and void distribution, which realizes high agility, light weight and safety in application;
[0038] 3. The present invention can meet the requirements of high performance, high reliability and long life in the harsh working environment of high and low temperature alternation and vibration impact in the Hall electric propulsion system. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic diagram of the configuration of a metal porous throttle according to a preferred embodiment of the present invention.
[0040] Figure 2 It is a schematic diagram of the main structure of a gradient porous micro gas throttle according to a preferred embodiment of the present invention.
[0041] Figure 3.It is a structural schematic diagram of a gradient porous micro gas throttle with a nano-film structure according to a preferred embodiment of the present invention.
[0042] Figure 4 This is a structural diagram of a gradient pore structure micro gas throttle according to an embodiment of the present invention.
[0043] Figure 5 This is a structural diagram of a gradient pore structure micro gas throttle according to Example 2 of the present invention. DETAILED DESCRIPTION
[0044] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:
[0045] Embodiment 1:
[0046] In this embodiment, see Figure 1-Figure 3 , an agile gas throttle with a gradient pore structure, the throttle is composed of Fe-Ni-Cr-Mo alloy, and the structure is a combination of an outer dense layer and a middle air-permeable cylindrical part, the outer dense layer forms a tube wall, and the middle air-permeable cylindrical part is arranged in the outer dense layer cavity; Fe-Ni-Cr-Mo alloy powder is used as raw material, and a 3D printing method is used to prepare an integrated middle air-permeable cylindrical part and an outer dense layer of the throttle, wherein the cylindrical side wall is a dense structure with a relative density of 100%, The porosity is zero; the middle air-permeable cylindrical part is a porous structure with a relative density of 80%, so that the throttle presents a gradient material structure from porous to dense in the radial direction; along the air flow direction, a nanoporous coating is also arranged, the nanoporous coating is arranged in the cavity of the outer dense layer, and is tightly attached to the end of the middle air-permeable cylindrical part, the nanoporous coating is combined with the middle air-permeable cylindrical part to form a composite material air-permeable core; the outer dense layer, the middle air-permeable cylindrical part and the nanoporous coating form an agile gas throttle with a gradient pore structure.
[0047] In this embodiment, spherical particle powders of 200 mesh, 300 mesh and 400 mesh are mixed in a mass ratio of 1:1:1, and the composition of the spherical particle powder is 65.73wt% of the main element, 2.27wt% of Mo, 18wt% of Cr, 13wt% of Ni, 1wt% of Mn, and the main element is Fe. Spherical particle powder is used as 3D printing material for 3D printing. The outer diameter of the prepared throttle is 10mm, the inner diameter of the outer dense layer is 6mm, and the length of the middle air-permeable cylindrical part is 11mm. The printing process parameters are scanning spacing: 0.11mm, laser power: 120w, scanning speed: 900m / s, and layer thickness 15 microns. A cylinder with voids on the X and Y axes and a porosity of 20%, that is, the prepared middle air-permeable cylindrical part is a porous structure with a density of 80%; there is no pore on the Z axis and the density is 100%. The throttle is made to present a gradient material structure from pores to denseness in the radial direction, so as to obtain a main structure part of a dense gradient material.
[0048] Then, the coating heat treatment method was used to heat treat the main structural parts of the density gradient material prepared by 3D printing. A nanoporous coating of Fe-Ni-Cr-Mo alloy was used, and the nanoporous coating was arranged on the end surface of the middle breathable cylindrical part along the airflow direction. The temperature of the coating heat treatment process was controlled to 950°C, and the insulation time was 2h, so that the nanoporous coating was tightly combined with the end of the middle breathable cylindrical part to form a composite material breathable core, so that the outer dense layer, the middle breathable cylindrical part and the nanoporous coating formed an agile gas throttle with a gradient pore structure.
[0049] Experimental test analysis:
[0050] The throttle prepared in this embodiment was tested. The tested atmosphere was xenon gas. The inlet pressure was 0.2 MPa. After the flow was blocked, the gas flow rate was 300 mg / s. Figure 4 . Figure 4 Schematic diagram of the structure of the gradient pore structure micro gas throttle of this embodiment. The diameter of the throttle is 10 mm, the inner diameter of the outer dense layer is 6 mm, and the length of the middle air-permeable cylindrical part is 11 mm.
[0051] Embodiment 2:
[0052] This embodiment is basically the same as the first embodiment, except that:
[0053] In this embodiment, spherical particle powders of 200 mesh, 300 mesh and 400 mesh are mixed in a mass ratio of 1:1:2. The composition of the spherical particle powder is 65.73wt% of the main element, 2.27wt% of Mo, 18wt% of Cr, 13wt% of Ni, 1wt% of Mn, and the main element is Fe. Spherical particle powder is used as 3D printing material for 3D printing. The outer diameter of the prepared throttle is 8mm, the inner diameter of the outer dense layer is 5mm, and the length of the middle air-permeable cylindrical part is 11mm. The printing process parameters are scanning spacing: 0.12mm, laser power: 130w, scanning speed: 1050m / s, and layer thickness 20 microns. A cylinder with voids on the X and Y axes and a porosity of 8%, that is, the prepared middle air-permeable cylindrical part is a porous structure with a density of 92%; there is no pore on the Z axis and the density is 100%. The throttle is made to present a gradient material structure from pores to denseness in the radial direction, so as to obtain a main structure part of a dense gradient material.
[0054] Then, the coating heat treatment method was adopted to heat treat the main structure of the density gradient material prepared by 3D printing. A nanoporous coating of Fe-Ni-Cr-Mo alloy was used, and the nanoporous coating was arranged on the end surface of the middle breathable cylindrical part along the airflow direction. The temperature of the coating heat treatment process was controlled to 980°C, and the insulation time was 2h, so that the nanoporous coating was tightly combined with the end of the middle breathable cylindrical part to form a composite material breathable core, so that the outer dense layer, the middle breathable cylindrical part and the nanoporous coating formed an agile gas throttle with a gradient pore structure.
[0055] Experimental test analysis:
[0056] The throttle prepared in this embodiment was tested. The tested atmosphere was xenon gas, the inlet pressure was 0.2 MPa, and after the flow was blocked, the gas flow rate was 12 mg / s. Figure 5 . Figure 5 This is a schematic diagram of the structure of the gradient pore structure micro gas throttle of this embodiment. The diameter of the throttle is 8 mm, the inner diameter of the outer dense layer is 6 mm, and the length of the middle air-permeable cylindrical part is 11 mm.
[0057] Embodiment three:
[0058] This embodiment is basically the same as the above embodiment, with the following features:
[0059] In this embodiment, the composition of the agile gas throttle with gradient pore structure in the above embodiment is Fe-Ni-Cr-Mo alloy. The structure is a cylindrical shape with dense outer layer and air permeable middle. Figure 1, using Fe-Ni-Cr-Mo alloy powder, after 3D printing, a cylindrical gas throttle with a throttle diameter of 7 to 15 mm can also be prepared, wherein the cylindrical side wall is a dense structure with a relative density of 100% and a porosity of zero; the cylindrical middle part is a porous structure with a relative density of 5-50%, wherein the pore structure is 5-53 microns, that is, the throttle presents a gradient functional structure from pores to dense in the radial direction, and its structure is shown in FIG. Figure 2 For the printed throttle, the micro gas throttle along the airflow direction has a nanoporous coating, and its structure is Figure 3 .
[0060] In summary, the gradient pore structure micro gas throttle implemented in the present invention has high production efficiency and good sample consistency, which overcomes the current shortcomings of poor flow consistency of metal porous cores. At the same time, the gradient pore structure micro gas throttle prepared by the present invention is suitable for flexible customization of single or small batch porous core samples, with high control accuracy, excellent mechanical properties, good flow stability, and protection of the safety of the propeller.
[0061] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention of the present invention and do not deviate from the technical principles and inventive concepts of the present invention, they belong to the protection scope of the present invention.
Claims
1. An agile gas throttle with a gradient pore structure, characterized in that: The main component of the throttle is Fe-Ni-Cr-Mo alloy, which is a structure combining an outer dense layer and a middle air-permeable cylindrical part. The outer dense layer is in the form of a tube wall, and the middle air-permeable cylindrical part is arranged in the cavity of the outer dense layer. Fe-Ni-Cr-Mo alloy powder is used as raw material, and a 3D printing method is used to prepare an integrated middle air-permeable cylindrical part and an outer dense layer of the throttle, wherein the cylindrical side wall is a dense structure with a relative density of 100% and a porosity of zero; the middle air-permeable cylindrical part is a tube wall, and the middle air-permeable cylindrical part is arranged in the cavity of the outer dense layer. The cylindrical part is a porous structure with a relative density of 5-92%, so that the throttle presents a gradient material structure from porous to dense in the radial direction; along the air flow direction, a nanoporous coating is also arranged, the nanoporous coating is arranged in the cavity of the outer dense layer and is close to the end of the middle breathable cylindrical part, the nanoporous coating is combined with the middle breathable cylindrical part to form a composite material breathable core; the outer dense layer, the middle breathable cylindrical part and the nanoporous coating form an agile gas throttle with a gradient pore structure.
2. According to the agile gas throttle with gradient pore structure as claimed in claim 1, it is characterized by: The composition of Fe-Ni-Cr-Mo alloy is as follows in terms of mass percentage: Wherein, the main element is Fe.
3. According to the agile gas throttle with gradient pore structure as claimed in claim 1, it is characterized by: The end of the middle air-permeable cylindrical part prepared by the 3D printing method is subjected to a coating heat treatment, and the coating heat treatment process is as follows: The material of the coating is Fe-Cr-Ni-Mo-Al alloy or Fe-Ni-Cr-Mo alloy; the temperature of the coating heat treatment process is 900-1020°C, and the insulation time is 1-4h.
4. According to the agile gas throttle with gradient pore structure as claimed in claim 1, it is characterized by: When using the 3D printing method, the Fe-Ni-Cr-Mo alloy powder is a spherical particle powder with a mesh size of 200–400.
5. The agile gas throttle with gradient pore structure according to claim 4, characterized in that: When using the 3D printing method, the Fe-Ni-Cr-Mo alloy powder uses spherical particle powders with different particle size distributions of 200 mesh, 300 mesh and 400 mesh, and the spherical powders of 200 mesh, 300 mesh and 400 mesh are mixed in a mass ratio of 1:1:(1-2).
6. The agile gas throttle with gradient pore structure according to claim 1, characterized in that: The diameter of the central air-permeable cylindrical part is 5 to 15 mm.
7. The agile gas throttle with gradient pore structure according to claim 1, characterized in that: The height of the central air-permeable cylindrical portion is at least 10 mm.
8. The agile gas throttle with gradient pore structure according to claim 1, characterized in that: In an air flow environment, when the initial gas pressure is 0.2-0.5 MPa, the gas flow rate after being throttled by the gas throttle is 0.1-2000 mg / s.
9. A method for preparing an agile gas throttle with a gradient pore structure according to claim 1, characterized in that: The method of combining 3D printing with lamination heat treatment has the following steps: (1) Preparation of the main structure of density gradient material: Fe-Ni-Cr-Mo alloy spherical particle powders of different particle size distributions of 200-400 mesh are mixed in a set ratio as forming material powders, and a 3D printing method is used to prepare a middle air-permeable cylindrical part with pores on the X and Y axes, so that the porosity is 5-92%; there is no pore on the Z axis of the middle air-permeable cylindrical part, the density is 100%, and the diameter of the middle air-permeable cylindrical part is 5-15mm; a cylindrical side wall dense structure adapted to the middle air-permeable cylindrical part is prepared, the relative density is 100%, and the porosity is zero; the throttle presents a gradient material structure from pores to dense in the radial direction, and a density gradient material main structure is obtained; (2) Preparation of composite material breathable core: The main structure of the density gradient material prepared by 3D printing is heat treated by the coating heat treatment method, and a nanoporous coating of Fe-Cr-Ni-Mo-Al alloy or Fe-Ni-Cr-Mo alloy is used. The nanoporous coating is arranged on the end surface of the middle breathable cylindrical part along the air flow direction, and the temperature of the coating heat treatment process is controlled to be 900-1020℃, and the insulation time is 1-4h, so that the nanoporous coating is tightly combined with the end of the middle breathable cylindrical part to form a composite material breathable core, so that the outer dense layer, the middle breathable cylindrical part and the nanoporous coating form an agile gas throttle with a gradient pore structure.
10. The method for preparing the agile gas throttle with a gradient pore structure according to claim 9, characterized in that: In the step (1), when performing 3D printing, the process parameters are scanning spacing: 0.11-0.12 mm, laser power: 201-130 w, scanning speed: 900-1050 m / s, and layer thickness 15-20 microns; Alternatively, in step (2), when the coating heat treatment process is performed, the temperature is controlled to be 950-980° C. and the insulation time is 2-4 hours.
Citation Information
Patent Citations
Electric propulsion system storage and supply unit and manufacturing method thereof
CN112572840A
Preparation method of micro-throttler of electric propulsion supply system
CN112620648A