A method for recycling lithium batteries

By using concentrated sulfuric acid digestion and wet chemical extraction, the problems of low recovery rates of graphite and lithium and low metal efficiency in lithium batteries have been solved, achieving high-purity recovery and high-efficiency lithium battery resource recycling.

CN114174544BActive Publication Date: 2024-11-26DUESENFELD GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980098748.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-26
Publication Date
2024-11-26
Estimated Expiration
2039-07-26

AI Technical Summary

Technical Problem

In existing lithium battery recycling methods, the recovery rates of graphite and lithium are low, the recovery efficiency of metals such as cobalt, nickel, and manganese is less than 50%, and the treatment of fluorides is complicated, resulting in high recycling costs and low efficiency.

Method used

The material is digested and pulverized using concentrated sulfuric acid to remove fluorides. Subsequently, metals such as lithium, cobalt, manganese, and nickel are recovered through wet chemical extraction. The digestion temperature and exhaust emissions are controlled using recovery equipment to ensure safe and high-purity recovery.

Benefits of technology

It achieves high-purity recovery of graphite and lithium, and efficient recovery of metals such as cobalt, manganese, and nickel, with a recovery rate of over 50%, reducing energy consumption and safety risks, and simplifying fluoride treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114174544B_ABST
    Figure CN114174544B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for recycling lithium batteries, comprising the following steps: (a) using concentrated sulfuric acid (12) at a decomposition temperature (T of at least 100°C, in particular at least 140°C) A ) decomposing a ground material (10) containing ground components of an electrode of a lithium battery, thereby producing an exhaust gas (14) and a decomposed material (16); (b) discharging the exhaust gas (14); and (c) wet chemically extracting at least one metal component of the decomposed material (16).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for recycling lithium batteries. According to a second aspect, the present invention relates to a recycling device for processing lithium batteries. Background Art

[0002] Lithium batteries are batteries that store electrical energy via lithium-based electrochemical reactions. Lithium batteries have a wide range of uses. The recycling of lithium batteries remains problematic. It is currently not possible to recover the graphite contained in the electrodes to a quality that can be reused in the production of lithium batteries. The recycling of lithium also poses problems. In addition, the cobalt, nickel and manganese that may be present in lithium batteries can usually only be recovered to a certain quality, so that using them in new lithium batteries is not economically possible. When considered as a whole, the material recovery efficiency of the known recycling methods in terms of battery cells is less than 50% by weight.

[0003] US 2004 / 0028585 A1 describes a method for recovering vanadium from lithium metal-polymer batteries. According to one variant, this involves mixing the pulverized material with 30% dilute sulfuric acid. The vanadium is then obtained from the resulting aqueous solution in the form of vanadium pentoxide. This method is therefore only practical if the vanadium content in the pulverized material is sufficiently high. However, this is not the case, for example, in commonly used lithium-ion batteries. In addition, other metal components, such as cobalt, nickel and manganese, are rather difficult to extract. For a number of reasons, including safety reasons, the use of concentrated sulfuric acid is not recommended.

[0004] US 2017 / 0077564 A1 describes a method for recycling lithium-ion batteries, in which the pulverized material is leached with dilute sulfuric acid and aqueous hydrogen peroxide solution. The disadvantage of this method is that it is very complicated to achieve the highest recovery rate.

[0005] Nayl et al., in the article entitled “Acid leaching of mixed spent Li-ion batteries” in the Arabian Journal of Chemistry, 2017, 10, S3632-S3639, also described a method for leaching lithium batteries using dilute sulfuric acid and hydrogen peroxide. It has been found that the degree of leaching initially increases with increasing sulfuric acid concentration and then decreases from 3M. The highest concentration detected was 4M. Summary of the invention

[0006] The present invention aims to improve the recycling rate of lithium batteries.

[0007] The present invention solves the problem through a method for recycling lithium batteries, which includes the steps of: (a) digesting pulverized material containing pulverized components of lithium battery electrodes using sulfuric acid, especially concentrated sulfuric acid, thereby producing waste gas and digested material, (b) discharging the waste gas and (c) wet chemical extraction of at least one metal component of the digested material, especially at least one metal component from the list containing cobalt, lithium, manganese, nickel and titanium (preferably two, three, four or more metal components).

[0008] The digestion is preferably carried out at a digestion temperature of at least 100° C., preferably at least 120° C., particularly preferably at least 140° C. However, digestion temperatures below 100° C. are also possible.

[0009] According to a second aspect, the invention solves the problem by a recycling device for processing lithium batteries, in particular used lithium batteries, which has: (a) a reactor for digesting a pulverized material containing pulverized components of lithium battery electrodes with concentrated sulfuric acid at a digestion temperature of at least 100° C., (b) a sulfuric acid supply device for adding sulfuric acid to the pulverized material, and (c) a discharge device for discharging waste gases out of the reactor. In particular, the discharge device is designed in a hydrogen fluoride-proof manner. In other words, hydrogen fluoride cannot escape into the surrounding environment.

[0010] An advantage of the present invention is that any fluoride that may be present in the pulverized material can be completely removed during digestion of the pulverized material with sulfuric acid, which is preferably concentrated. Fluorine compounds form hydrogen fluoride, which is very problematic from an occupational safety point of view. Hydrogen fluoride is also highly corrosive. By digesting the pulverized material with sulfuric acid, fluoride is removed from the pulverized material, so that subsequent steps in the process can be carried out with fewer safety precautions and a lower degree of material wear. Certain separation methods (such as membrane separation, bipolar membrane electrodialysis) cannot be carried out in fluids with high fluorine levels; however, such a preparation will make this possible. In addition, impurities caused by fluorine substances will not be present, so that other components in the pulverized material can generally be recovered in high purity.

[0011] Also advantageously, battery graphite can often be recovered at such high purity that it can be used to produce new electrodes.

[0012] It is also practical that the method can generally be carried out in a manner that the lithium is recovered to a sufficiently high purity to make it suitable for use in the production of new lithium batteries. Where cobalt and / or manganese are present in the comminuted material, they can also be recovered to a high purity, making them suitable for reuse in batteries.

[0013] It is particularly advantageous that in most cases, recycling efficiencies of more than 50% by weight can be achieved with respect to the battery cells.

[0014] It should be noted that specified advantages may occur, but they are not required.

[0015] Known methods focus on the recovery of cobalt and nickel because they represent the highest material value in used lithium batteries. Other components in used lithium batteries, such as graphite and / or lithium, cannot be recovered. The recovery of fluoride is also not a priority for known methods because of its relatively low resale value.

[0016] It is particularly advantageous that the method according to the invention can in most cases be designed such that it requires less energy than a pyrometallurgical method. In particular, according to a preferred embodiment, the method does not comprise a pyrometallurgical step.

[0017] According to DE 102015207843 A1, it is known that it is advantageous to dry the battery at low temperature after comminution in order to prevent the formation of fluorinated organic substances. In this drying process, organic carbonates present in the electrolyte are removed. As a result, the fluorine compounds remain in the comminuted material. According to a preferred embodiment, the comminuted material containing at least one fluorine compound is digested.

[0018] Within the scope of this specification, a method for recycling lithium batteries is to be understood as referring in particular to a method for recycling metal components of lithium batteries. In this sense, the method according to the invention is also a method for extracting metal components from lithium batteries. The metal components are, for example, lithium and / or transition metals, in particular metals from the sixth, seventh and eighth groups. The transition metals are preferably manganese and / or cobalt and / or nickel. It is also practical if copper and / or titanium are recovered.

[0019] In the context of this description, a lithium cell is to be understood in particular as meaning a rechargeable cell whose electrochemical reaction involves lithium and / or lithium ions and / or lithium compounds. A cell comprises at least a galvanic cell element.

[0020] Preferably, the lithium batteries are at least partly lithium ion batteries. It is particularly preferred if the comminuted material comprises at least 40% by weight, in particular 60% by weight, of lithium ion batteries. Lithium ion batteries contain a fluid electrolyte containing fluorides: said electrolyte makes the recycling of lithium batteries considerably more difficult.

[0021] The fluoride content in the pulverized material is preferably less than 7% by weight, in particular less than 5% by weight.

[0022] The fluoride content in the pulverized material is preferably at least 0.5% by weight, in particular at least 1% by weight.

[0023] A recycling plant is to be understood as meaning, in particular, an apparatus by which one, two, three or more metal components of a lithium battery are separated from other components of the lithium battery so that they can be processed further.

[0024] When temperatures are specified in the following description, they always refer to the average temperature of the respective object. For example, digestion at a digestion temperature of at least 100° C. is to be understood in particular to mean that the temperature of the pulverized material mixed with sulfuric acid is 100° C. on average. It is immaterial that there may be locally higher or lower temperatures. If no temperature is explicitly mentioned, the respective step in the process is preferably carried out at room temperature and the ambient pressure of the surrounding atmosphere.

[0025] Any use of the indefinite article should be understood to mean that at least one of the corresponding objects is available. For example, a recycling device can mean not only exactly one shredding unit, but also two, three or more shredding units.

[0026] Digestion is to be understood in particular to mean that no dilute sulfuric acid is used. In particular, at least at one point in time during the reaction, the concentration of sulfuric acid is more than 90%, in particular more than 95%, particularly preferably more than 98%.

[0027] In particular, the digestion is carried out in such a way that the fluoride components in the pulverized material migrate into the exhaust gas in the form of hydrogen fluoride. In other words, the water present in the mixture of pulverized material and sulfuric acid is so small that the concentration of water-soluble fluoride is less than 100 mg / kg of digested material, in particular less than 10 mg / kg of digested material.

[0028] The aspect of digesting the comminuted material with concentrated sulfuric acid is to be understood in particular as meaning that, during the time interval during which the method is carried out, the concentration of sulfuric acid is so high that the above-specified concentration of water-soluble fluoride per kg of digested material is reached. Preferably, the concentration of sulfuric acid during the carrying out of the method is at least 95%, preferably at least 98%. Using concentrated sulfuric acid means that the digested material contains hardly any fluoride, unlike the case when non-concentrated sulfuric acid is used.

[0029] Specifically, digestion is not leaching, since leaching is always performed with an aqueous fluid.

[0030] In particular, the digestion material is solid. Unlike processes that do not use concentrated sulfuric acid, the reaction products, especially metal sulfates, are insoluble in water and remain as solid matter.

[0031] Crushed material is to be understood in particular as meaning material produced by the crushing of at least one component of a lithium battery or a lithium battery, in particular an electrode, and where applicable from a post-processing procedure, such as drying. Therefore, the crushing may be followed by a plurality of separation steps to separate crushed metal foil, plastic foil or battery housing components and module components. It is practical if the crushed material contains up to 10% by weight, preferably up to 5% by weight, of plastic and / or metal impurities. The crushed material may contain powder components from an electrode of a lithium battery. In a more general form, uncomminuted material, in particular electrode material, may be used instead of the crushed material. However, it is beneficial for such electrode material to be crushed.

[0032] In particular, the pulverized material may be a material which has not been subjected to any pyrometallurgical treatment, in particular calcination and combustion. However, it is also feasible and included in the present invention that the pulverized material has not been subjected to any pyrometallurgical treatment.

[0033] The discharge of waste gases is understood to mean, in particular, that the waste gases are conducted at least to a large extent away from the digestion point. It is possible for the waste gases to be sucked off. The waste gases generally contain fluorine compounds, in particular hydrogen fluoride. It is possible, but not necessary, to remove hydrogen fluoride from the waste gases, in particular by precipitation, preferably with calcium compounds. The waste gases can also be fed to a chemical process.

[0034] Wet-chemical extraction is to be understood in particular to mean that a substance which is liquid at 1013 hPa and room temperature or which is liquid in the added state is added to the digestion material or to a substance from the digestion material which results in the separation of at least one metal-containing substance or the metal itself.

[0035] The sulfuric acid is preferably at least 90%, particularly preferably at least 95%. However, it is possible to add sulfuric acid to the comminuted material at a lower concentration. In this case, the digestion temperature is preferably at least the temperature required to evaporate enough water from the sulfuric acid to ensure that it has a concentration of at least 90%, particularly at least 95%. References to percentages are generally to percentages by weight.

[0036] The digestion of the pulverized material preferably comprises the step of mixing the pulverized material with sulfuric acid. The mixing may comprise spraying sulfuric acid and / or mixing by forced action, such as extrusion, kneading or stirring.

[0037] The digestion temperature is preferably below the boiling point of sulfuric acid to prevent evaporation of the sulfuric acid. Preferably, the digestion temperature is below the binder decomposition temperature of the binder by means of which the active material is bound to its support. Alternatively, the digestion temperature may be above the binder decomposition temperature. This prevents the binder from contaminating the graphite. However, it should be noted that the pulverized material may, but need not, contain a suitable binder. Temperatures of 150° C. to 250° C. are particularly advantageous.

[0038] The digestion can be carried out under a protective gas (such as nitrogen or argon) like the other steps in the method to prevent oxidation of the graphite. The other steps in the method can also be carried out under a protective gas, but it is not necessary.

[0039] Digestion can - like other steps in the method - be performed discontinuously or continuously.

[0040] According to a preferred embodiment, the digestate material contains at most 15% water, in particular less than 10% water, preferably less than 5% water. If there is little or no water, the fluoride will be removed in the form of hydrogen fluoride, so that little or no fluoride compounds remain.

[0041] It is preferred to carry out digestion until the hydrogen fluoride concentration in the waste gas is less than 0.83 mg / m 3 Preferably, the hydrogen fluoride concentration is below a traceability threshold. The traceability threshold is in particular an infrared spectroscopy measurement. This ensures that no significant amounts of hydrogen fluoride are released in subsequent steps of the process.

[0042] Alternatively or in addition, digestion is performed until the fluoride concentration of water-soluble fluoride in the digested material is c F Below 100 mg / kg digestible material, preferably below 10 mg / kg, particularly preferably below the traceability threshold.

[0043] According to a preferred embodiment, the digestion of the pulverized material comprises the steps of (a) mixing concentrated sulfuric acid and pulverized material to produce a mixture, (b) detecting the mixture temperature of the mixture and (c) adjusting (i) the dosage mass flow rate of sulfuric acid and / or (ii) the addition mass flow rate of pulverized material so that the mixture temperature is maintained within a predetermined mixture temperature range. The upper limit of the range of the mixture temperature is preferably at most 330° C., in particular at most 300° C., in particular at most 270° C. Since the reaction is generally exothermic, the lower limit of the range of the mixture temperature is less relevant. For example, the lower limit of the range is 0° C.

[0044] Preferably, (a) concentrated sulfuric acid is quantitatively added to the pulverized material at a dosage mass flow rate to produce a mixture, (b) a mixture temperature of the mixture is detected and (c) the dosage mass flow rate is adjusted so that the mixture temperature is maintained within a predetermined mixture temperature range.

[0045] For example, the comminuted material is charged to the reactor and sulfuric acid is then dosed. Dosing is understood to mean adding sulfuric acid to the comminuted material in such a way that it is ensured that the addition of sulfuric acid can be reduced to such an extent that, in particular, the addition is stopped if the temperature of the mixture is outside a predetermined mixing temperature range. Dosing with a known mass flow and / or in such a way that the mass flow is influenced in a controlled manner is practical, but not essential.

[0046] Preferably, sulfuric acid is added to the pulverized material in at least a stoichiometric amount, but preferably in a superstoichiometric amount. This should be understood in particular to mean that sufficient sulfuric acid is added so that all non-precious metals and copper in the pulverized material can be extracted and, according to a preferred embodiment, extracted in a subsequent step of the method. In particular, sufficient sulfuric acid is added to ensure that all non-precious metals and copper in the pulverized material are dissolved by at least 99% by weight. It should be noted that even in the case of a superstoichiometric addition of sulfuric acid, metal residues that have not reacted with the sulfuric acid may remain due to the limited reaction rate and the regulation of the chemical equilibrium.

[0047] Preferably, concentrated sulfuric acid is used in a weight ratio to the weight of the pulverized material of at most 40: 1, in particular at most 20: 1, preferably at most 10: 1. In other words, at most 40 kg of concentrated sulfuric acid is added per kg of pulverized material.

[0048] For example, it is advantageous if at least 1.8 g H2SO4 is added per g cathode material, in particular 1.8 g H2SO4 per g electrode active material. In particular, the cathode material is LiMO2, wherein M represents a transition metal or aluminum. The cathode is the electrode that is positively charged during discharge.

[0049] The method preferably comprises a step of separating hydrogen fluoride from the waste gas, in particular a step of precipitating hydrogen fluoride from the waste gas. For example, this is achieved by means of a calcium compound, resulting in the formation of calcium fluoride.

[0050] The method preferably comprises leaching the digested material. Leaching is preferably carried out with an aqueous fluid, in particular water. The weight ratio of digested material to aqueous fluid is preferably from 1:2 to 1:20. Leaching is carried out for at least 1 minute, preferably for at most 10 hours.

[0051] During leaching, the pH is preferably between -0.7 and 4. Leaching is preferably carried out at room temperature; however, this is not required.

[0052] The method preferably includes separation of the graphite to obtain a raw material fluid. This is carried out after leaching. The separation is preferably filtration. However, it is also possible to centrifuge or separate the graphite in another way. Digestion with sulfuric acid usually results in a very low concentration of metals, especially metal ions, in the graphite, so that the graphite is suitable for use as electrode graphite for the production of new lithium batteries or other batteries.

[0053] The method may include a step of purifying the separated graphite, which may be achieved, for example, with water or a dilute mineral acid, wherein preferably silicon is removed in this manner.

[0054] The purification is preferably so intensive that at most 10 mg / kg of metal ions remain in the wash water. It has been shown that in the known methods the crystal structure of the graphite is so severely damaged that it cannot be used as electrode graphite. Since, according to a preferred embodiment of the method, no wet chemical oxidation or thermal oxidation takes place before the graphite is separated, the crystal structure of the graphite is only slightly damaged, so that it can generally be reused in batteries.

[0055] Purification of the graphite preferably comprises heating the graphite to a decomposition temperature T of the binder of at least 250° C. and / or at most 700° C., in particular at most 430° C. Z At such temperatures, any binder residues, which usually consist of polyvinylidene fluoride, will decompose. Higher temperatures may damage the graphite. The heating can be carried out under vacuum, in particular at a maximum pressure of 300 hPa, but this is not necessary.

[0056] The heating can be carried out in an oxidizing atmosphere, for example in air or oxygen, with the addition of air or oxygen being preferred.

[0057] Alternatively, the heating may be performed in an inert atmosphere, for example, an atmosphere consisting of nitrogen and / or argon.

[0058] Alternatively, the heating can be carried out in a reducing atmosphere. For example, the atmosphere then contains hydrogen.

[0059] The purification of the graphite may also comprise a classification of the graphite such that at least one fine fraction and one coarse fraction are obtained. The classification is preferably carried out in such a way that the binder content of the binder in the fine fraction is at least twice as high as the binder content of the binder in the coarse fraction. For example, the classification may be a separation.

[0060] Alternatively or additionally, purifying the graphite may comprise flotation of the graphite or the binder, in particular in an aqueous flotation fluid.

[0061] As another alternative or in addition, purification may include dissolving the binder from the graphite using a solvent. For example, water, N-methyl-pyrrolidone or a mixture of the two are suitable solvents. Preferably, purification is performed until the binder content is less than a predetermined maximum binder content. The maximum binder content is preferably at most 2 weight percent, in particular at most 1 weight percent. Typically, a maximum binder content greater than 0.1 parts per thousand is acceptable.

[0062] Dissolution preferably takes place at a solvent temperature of at least 20°C, in particular at least 40°C, particularly preferably at least 60°C.

[0063] It is advantageous if the purification includes a step of regenerating the solvent by (i) reducing the solubility of the binder, in particular by reducing the temperature of the solvent and filtering the binder or (ii) evaporating the solvent and recondensing the sol. Alternatively, the solvent may be continuously replaced until the binder content is less than a maximum binder content.

[0064] As a further alternative or in addition, the purification of the graphite comprises rinsing and / or washing with an acid, in particular an inorganic acid, preferably sulfuric acid. The purification is preferably carried out until the concentration of metallic impurities is at most 10000 ppm. Graphite purified in this way can replace newly produced graphite in many fields of application.

[0065] Preferably, the method comprises a step of separating copper from the feed fluid, producing a decoppered feed fluid. It is possible, but not essential, that the separation of copper is a wet chemical process that takes place immediately after leaching. In particular, it is also possible to separate other metals before separating the copper. In particular, this refers to selective copper separation. The temperature during the copper separation is preferably 0° C. to 100° C. The separation is preferably carried out for 1 minute to 720 minutes.

[0066] The separation may be a diffusion process. In the case of a diffusion process, the copper ions undergo an electrochemical reaction resulting in the formation of elemental copper. For example, a diffusion process is performed with an iron substrate.

[0067] Alternatively, the separation comprises precipitation. For example, copper can be precipitated as copper sulfide. For this purpose, the feed fluid is added to a precipitation substance, for example a sulfur-containing substance. This can refer to sodium hydrosulfide. In this case, copper sulfide, in particular CuS, is precipitated. It is advantageous if the precipitation substance is added in excess of the stoichiometric amount, so that the concentration of copper ions in the decopperized feed fluid is preferably less than 10 mg / L, particularly preferably less than 1 mg / L.

[0068] The method preferably comprises the step of oxidizing the decopperized solution. This is preferably achieved by adding an oxidizing agent. For example, hydrogen peroxide can be used as an oxidizing agent.

[0069] The oxidation is preferably carried out in the form of oxidation of iron ions. It is beneficial if this is followed by a step of precipitating iron. Specifically, the Fe 2+ The ions are oxidized to form Fe 3+ ions. This can be achieved with an oxidizing agent, such as an oxygen compound. For example, the oxygen compound can be hydrogen peroxide or ozone.

[0070] The precipitation of iron preferably takes place in the form of hydroxide. It is particularly advantageous if the aluminum is preferably precipitated in the form of hydroxide. It is also advantageous if the existing titanium is preferably precipitated in the form of titanium oxide. The precipitation of iron and / or aluminum produces a pure fluid.

[0071] The precipitation of iron and / or aluminum and / or titanium is preferably carried out as a result of the addition of NaOH, Na2CO3, KOH, MgO or ammonium hydroxide.

[0072] It should be noted that the term "pure fluid" should only be used with respect to metals that are considered as impurities, such as iron, and where applicable, copper, aluminum and titanium have been removed. In particular, the term "pure fluid" is not intended to give any indication of the concentration of other substances.

[0073] The feature that the oxygen compound is used for oxidation is understood to mean that the oxygen changes its oxidation number during the redox reaction. Alternatively, compounds which contain oxygen but do not change their oxidation number during the redox reaction may be used as oxidizing agents.

[0074] The oxidation is preferably carried out until the electrochemical potential is 0.8 volts to 1.4 volts relative to the standard hydrogen electrode. occurs within this voltage range.

[0075] Preferably, the pH value during oxidation is at most 8.7. During precipitation, the pH value is preferably at least 4.3, particularly preferably 4.8. In particular, the pH value during precipitation is at most 8.7, preferably at most 7.8. Thus, iron and / or aluminum and / or titanium are precipitated in large quantities.

[0076] According to a preferred embodiment, the method comprises an ion exchange step. For this purpose, an ion exchanger is used. The ion exchange is preferably carried out in a manner to remove metal impurities. The metal impurities are zinc and / or copper and / or aluminum and / or iron. It is possible to remove all four elements, three of the elements, two of the elements or only one of the elements. For the ion exchange, an ion exchanger is used, for example, which contains a chelating agent with an aminophosphonic acid group as a functional group.

[0077] It is advantageous if the ion exchange is carried out after the iron and / or aluminum has been precipitated. In this way, the amount of iron and / or aluminum that must be removed by ion exchange remains small.

[0078] According to a preferred embodiment, the method comprises a step of removing solvent residues of the electrolyte, in particular by filtration and / or absorption. This is preferably carried out before the ion exchange and / or after or simultaneously with the precipitation of iron and / or aluminum. It is particularly preferred if the removal takes place in the decopperized raw fluid and / or in the pure fluid. The absorption is preferably carried out using activated carbon.

[0079] It is possible, but not necessary, to remove solvent residues from the electrolyte by loose addition of activated carbon and subsequent removal thereof, in particular by filtration.

[0080] Preferably, manganese is removed from the pure fluid, particularly by solvent extraction, preferably by a manganese complexing agent dissolved in a lipophilic fluid. The lipophilic fluid may be, for example, a mineral oil, such as kerosene. For example, the manganese complexing agent may be di-(2-ethylhexyl) phosphoric acid. The pH value for removing manganese is preferably between 1 and 9.

[0081] It has been shown to be advantageous to extract the manganese before the cobalt. This eliminates the need for Cyanex 301 (bis(2,4,4-trimethylpentyl)dithiophosphinic acid) for the separation of transition metals, which reduces instrument complexity.

[0082] The method preferably comprises solvent extraction of cobalt. It is preferably extracted from a pure fluid or a fluid from which manganese has been removed. It is particularly advantageous to use a cobalt complexing agent for this purpose, for example a complexing agent dissolved in a lipophilic fluid. The lipophilic fluid may be, for example, a mineral oil, such as kerosene. One possibility is to use a phosphinic acid, for example Cyanex 272 (bis(2,2,4-trimethylpentyl)phosphinic acid). The pH value used for extracting the cobalt is preferably between 1 and 10.

[0083] The method preferably comprises a step of extracting the nickel. According to a preferred embodiment, the removal of the nickel is a solvent extraction of the nickel. This is preferably carried out using a nickel complexing agent. For example, this can be di-(2-ethylhexyl)phosphoric acid. The pH value is preferably between 1 and 10. Alternatively, the nickel complexing agent can be neodecanoic acid. In this case, the pH value is preferably between 2 and 10. The complexing agent is preferably dissolved in a lipophilic fluid, such as a mineral oil, such as kerosene. It is beneficial if the solvent extraction is carried out from a pure liquid from which manganese and cobalt have been removed.

[0084] According to an alternative embodiment, the removal of nickel comprises precipitating basic nickel carbonate. The general formula of basic nickel carbonate is xNiCO3·yNi(OH)2·zH2O. The precipitation preferably occurs at a temperature in the temperature range of 0-100°C, in particular at least 70°C. The pH value during precipitation is preferably above pH 7, in particular above pH 9.9.

[0085] It has also been shown to be advantageous to extract the cobalt and nickel prior to extracting the manganese. In this case, the manganese can be precipitated and solvent extraction is not required.

[0086] According to a preferred alternative embodiment for the extraction of transition metals, cobalt and nickel can be extracted from the pure fluid in a joint extraction process, thereby obtaining a fluid rich in cobalt and nickel.

[0087] For example, Cyanex 301 (bis(2,4,4-trimethylpentyl)dithiophosphinic acid) is very suitable for the extraction of nickel or cobalt, wherein Cyanex can be used in advance dissolved in kerosene. A loaded organic phase is formed in the process. The nickel and / or cobalt can be re-extracted from the loaded organic phase, for example using hydrochloric acid or sulfuric acid. The cobalt can be removed from the solution containing cobalt and nickel obtained in this way by a cobalt complexing agent. This is achieved, for example, by a complexing agent dissolved in a lipophilic fluid. The lipophilic fluid can be, for example, a mineral oil, such as kerosene. One possibility is to use a phosphinic acid, such as Cyanex 272 (bis(2,2,4-trimethylpentyl)phosphinic acid).

[0088] The nickel is subsequently crystallized in the form of nickel chloride or nickel sulfate. The cobalt can also be re-extracted from the loaded organic phase using, for example, hydrochloric acid and / or sulfuric acid and then crystallized in the form of cobalt chloride or cobalt sulfate.

[0089] The removal of nickel and cobalt produces a solution rich in nickel and cobalt. Manganese can be removed from this solution, in particular by solvent extraction, preferably by a manganese complexing agent. For example, this can be di-(2-ethylhexyl)phosphoric acid. The pH value for removing manganese is preferably 1 to 9. This produces a loaded organic phase from which manganese can be extracted again. Manganese chloride and / or manganese sulfate can then be crystallized from the resulting solution.

[0090] Alternatively, manganese can be precipitated from a solution rich in nickel and cobalt, for example in the form of a carbonate. For this purpose, preferably a carbonate, such as sodium carbonate, is added to the manganese-containing fluid. The pH value is preferably above 7, in particular above 10.5.

[0091] As another alternative or in addition, manganese is precipitated as manganese hydroxide. For this purpose, a hydroxide, such as sodium hydroxide, is preferably added to the manganese-containing target fluid. The pH value is preferably above 7, in particular above 10.5.

[0092] Removal of cobalt, nickel and / or manganese produces a target fluid.

[0093] According to a preferred embodiment, lithium is removed from the target fluid. Preferably, lithium is precipitated from the target fluid. For example, this can be achieved by adding a phosphate (e.g., sodium phosphate) or a carbonate (e.g., sodium carbonate). The precipitation of lithium is preferably carried out at a pH of 7 to 14.

[0094] It is advantageous if the precipitation is preceded by a concentration step, thereby increasing the lithium concentration. Alternatively, the lithium may be precipitated as lithium phosphate; for this purpose, sodium phosphate may be added, for example. Concentration may be performed, for example, by reverse osmosis and / or evaporation.

[0095] If the pure fluid contains neither cobalt nor nickel nor manganese, lithium is preferably precipitated from the pure fluid. This is the case, for example, if the comminuted material is produced using only lithium iron phosphate batteries.

[0096] Alternatively, the lithium is extracted by solvent extraction. For this purpose, preferably a lithium complexing agent is used, such as Cyanex 936 from Solvay. After re-extraction with a mineral acid, a concentrated lithium solution is obtained, from which the lithium can be precipitated or crystallized.

[0097] Preferably, the pulverized material comprises powdered electrode material from lithium-ion batteries. Pulverized electrode foils, separator foils, other foils, battery encapsulation materials and components surrounding the battery module are separated from the pulverized lithium-ion batteries to produce powdered electrode active materials.

[0098] The comminuted material is preferably obtained by comminuting the battery and simultaneously and / or subsequently deactivating the resulting raw comminuted material by drying. It is particularly advantageous if the comminution is carried out in an inert gas atmosphere and / or under vacuum. If the comminution is carried out under vacuum, the pressure is preferably at most 300 hPa. Preferably, the temperature is at most 100° C., preferably at most 80° C. This prevents the formation of fluorinated organic substances. The fluorides remain in the comminuted material and are removed by digestion with sulfuric acid, as described above.

[0099] According to a preferred embodiment, the deactivation is followed by separation of pulverized metal current collector foils, separator foils of battery housing components and module components, resulting in pulverized material.

[0100] If the pulverized material is heated to an electrolyte removal temperature T exceeding 80°C after pulverization, E During deactivation, low boiling point electrolyte components are removed. However, higher boiling point electrolyte components may remain in the pulverized material. These may hinder subsequent steps in the process and therefore it is advantageous to remove them. The electrolyte removal temperature T E It is preferably at least 100°C, in particular at least 150°C, and at most 300°C, in particular at most 250°C.

[0101] The batteries are preferably pre-discharged and / or obtained by disassembling the battery system or the battery module.

[0102] In the case of the recovery plant according to the invention, the reactor is preferably a rotary kiln or a forced action mixer, in particular a heated forced action mixer. This ensures thorough mixing of the sulfuric acid with the pulverized material. For example, the reactor features a temperature control or regulator, by means of which the temperature of the mixture of pulverized material and sulfuric acid is brought to the digestion temperature and maintained at this temperature. The digestion can be carried out continuously or discontinuously.

[0103] According to a preferred embodiment, the recovery device has: a quantitative device for measuring the dosage mass flow rate q m (b) a mixture temperature detection device for detecting the mixture temperature T of the mixture; M The dosing device is preferably configured to adjust the dosage mass flow rate q m , so that the mixture temperature T M Maintain the mixture temperature within the predetermined range I. It has been shown that a large amount of heat is accumulated when sulfuric acid is added. In order to prevent the mixture temperature T M Increase too much, monitor the mixture temperature T M and not exceeding the predetermined mixture temperature target value T M,Soll The dosage mass flow rate q is adjusted by m .

[0104] According to a preferred embodiment, the recovery device comprises a leaching device for leaching the digested material in an aqueous medium.

[0105] The recovery device preferably has a fluoride separator for separating the hydrogen fluoride. For example, the hydrogen fluoride can be precipitated. However, the hydrogen fluoride can also be transferred to a reaction with another substance (for example an organic substance).

[0106] It is advantageous if the recycling device is designed to be mobile. In other words, the recycling device can be moved without having to dismantle it. The recycling device is preferably arranged in a 20-foot container or a 40-foot container.

[0107] The transport of crushed material is usually associated with risks because it contains flammable substances and fluorine compounds. Therefore, there is a risk that the release of hydrogen fluoride will cause a fire, which may be an acceptably small risk. Therefore, it is feasible to locally separate the electrolyte, battery components, electrode foil and electrode powder. It is therefore advantageous if the recycling device includes a battery processing device for crushing lithium batteries, as described in DE 102015207843 A1. The reactor, a sulfuric acid supply device and a discharge device and any other devices specified in the claims can then, but not necessarily, be designed to be movable and are preferably arranged together in a 20-foot container or a 40-foot container.

[0108] The recovery device preferably comprises a graphite recovery device, which is characterized by a graphite separation device, in particular a filter, for separating graphite and is arranged downstream of the reactor in the material flow direction.

[0109] According to a preferred embodiment, the graphite recovery device comprises a washing device for washing the adhering leaching solution from the graphite. The washing device is preferably designed to flush the leaching solution with an aqueous fluid.

[0110] The recovery device preferably has a fluoride detector for detecting fluorine compounds, in particular hydrogen fluoride. The fluoride detector is preferably a hydrogen fluoride analyzer for measuring the concentration of hydrogen fluoride in the exhaust gas.

[0111] According to a preferred embodiment, the recovery device features a control unit connected to the fluoride detector and designed to automatically control the reactor so that it maintains the digestion temperature until the fluoride concentration, in particular the hydrogen fluoride concentration, in the offgas falls below a predetermined threshold.

[0112] According to a preferred embodiment, the recovery device has a precipitated material separator for separating, in particular filtering out, the precipitated Cu or Cu compounds.

[0113] Advantageously, the recovery plant has a transition metal extraction device, in particular a solvent extraction device for extracting cobalt, manganese and / or nickel, which is arranged downstream of the graphite recovery device in the direction of material flow.

[0114] The recovery plant preferably also has an Fe / Al / Ti precipitate material separator for separating, in particular filtering out, precipitated iron and / or aluminum and / or titanium compounds. The Fe / Al / Ti precipitate separator is preferably arranged downstream of a deactivation device, such as a rotary kiln, and, if applicable, upstream of a transition metal removal device, such as in the form of a solvent extraction device, for removing cobalt, nickel and / or manganese in the material flow direction.

[0115] According to a preferred embodiment, the recovery device is characterized by having an ion exchanger for performing an ion exchange during which zinc and / or copper and / or iron and / or aluminum are removed. In particular, the ion exchanger is designed so that cobalt and / or nickel and / or manganese are not removed during the ion exchange. The ion exchanger is preferably arranged behind a copper extractor for extracting copper from the raw material fluid in the material flow direction. It is particularly preferred if the ion exchanger is arranged behind a Fe / Al / Ti precipitation material separator in the material flow direction.

[0116] The recovery device is preferably characterized by an activated carbon filter for removing organic compounds, in particular electrolyte components. The activated carbon filter is preferably arranged downstream of the Fe / Al / Ti precipitation material separator in the material flow direction.

[0117] Preferably, the maximum temperature to which the comminuted material or digested material is subjected is 1000° C., preferably at most 700° C., in particular below 335° C. The comminuted material is preferably not subjected to a decomposition treatment.

[0118] The recycling device according to the invention preferably features a comminution unit for comminuting lithium batteries, thereby producing shredded material. The recycling device preferably features a deactivation device for deactivating the shredded material. It is advantageous if the deactivation device comprises a drying device configured to dry the shredded material until the electrolyte content of the shredded material is too low to undergo an electrochemical reaction.

[0119] The recycling device may be characterized by an electrolyte removal device for heating the deactivated pulverized material to an electrolyte removal temperature (T E ). The electrolyte removal device is arranged behind the passivation device along the material flow direction.

[0120] The recovery device preferably has a vacuum device which is connected to the drying device to generate a vacuum in the drying device.

[0121] It is feasible if the vacuum device is designed to generate a vacuum of at least 300 hPa. In other words, the vacuum device is designed so that a pressure of 300 hPa or less can be reached. To ensure a low complexity of the instrument, the vacuum device is preferably constructed so that the maximum possible pressure is greater than 0.01 Pa, preferably greater than 1 Pa.

[0122] The recycling device preferably has a carbide separation device for separating carbide from the comminuted material. A carbide separation device is to be understood in particular as meaning a device for separating fragments of peripheral components of a battery system, battery cells and / or electrical contacts of a lithium battery. For example, the carbide separation device has a magnet separation device and / or a separator, in particular a cross-flow separator and / or a sawtooth separator.

[0123] Alternatively or in addition, the recycling device preferably has a light fraction separation device for separating a light fraction, the light fraction comprising, for example, a separator foil and a coating material. The light fraction separation device preferably has a sawtooth separator and / or an air separator, wherein it is advantageous if the air in the light fraction separation device is conducted within the circuit. This reduces the exposure of dust to the environment. The air separator can be an air jet screen.

[0124] Advantageously, the recycling device has a separation device, in particular a classification device, for separating the active material from the carrier, in particular by air jet sieving and / or a second comminution stage, so that an active material fraction and a carrier are obtained. In particular, the carrier fraction comprises aluminum foil and copper foil.

[0125] The recycling plant may, but need not necessarily, have a filling device for filling a transport container with the crushed material. By means of such a transport container, the crushed material can, if necessary, be transported over a longer distance, for example at least 1 km. The crushed material can then be led out of the transport container and fed into the reactor.

[0126] Alternatively, the recycling device may not have a filling device for filling the transport container with the crushed material. In this case, the crushed material is preferably transported to the reactor and introduced into the reactor by a continuous or discontinuous conveyor after crushing. BRIEF DESCRIPTION OF THE DRAWINGS

[0127] In the following, the invention will be explained in more detail by means of the accompanying drawings. They show:

[0128] Figure 1 is a flow chart of a method according to the present invention, and

[0129] FIG. 2 is a schematic diagram of a recycling device according to the present invention,

[0130] Figure 3 is a flow chart of a method for treating a comminuted material free of cobalt, nickel and manganese according to the present invention,

[0131] Figure 4 is a flow chart of a method for processing comminuted material free of cobalt and nickel but containing manganese, and

[0132] Figure 5 is a flow chart of a method for comminuted material free of manganese and nickel but containing cobalt according to the present invention,

[0133] Figure 6 is a flow chart for processing crushed material without manganese but containing cobalt and nickel.

[0134] Figure 7 is a schematic diagram of a recycling device according to the present invention,

[0135] Figure 8a and Figure 8b shows a flow chart of the method according to the present invention,

[0136] Fig. 9 shows a recovery device according to a further embodiment of the present invention, and

[0137] Fig.10 A graphite purification device of a recovery plant according to the invention is schematically depicted. DETAILED DESCRIPTION

[0138] Figure 1 A flow chart of the method according to the invention is shown. First, a comminuted material, for example in the form of comminuted electrode active material, is provided. This can be achieved, for example, using the method described in DE 102015207843A1, which is incorporated by reference. In particular, the battery can first be comminuted, thereby producing a raw comminuted material. In a subsequent step, the raw comminuted material is deactivated by drying, thereby obtaining a deactivated raw comminuted material.

[0139] Deactivation is preferably drying. For example, drying is carried out in an inert gas atmosphere or under vacuum. It is advantageous if the pressure is at most 300 hPa and the temperature during drying is at most 80° C. This has the effect that the comminuted material 10 can no longer react electrochemically to a significant extent, because the proportion of low boilers in the electrolyte is too low.

[0140] After deactivation, the method may comprise a step of removing the electrolyte. To this end, the container 11 is filled with the deactivated comminuted material 10, where it is heated to an electrolyte removal temperature T preferably above 100° C., in particular above T=150° C. E The container 11 may be, but need not be, a vacuum container to which a vacuum of, for example, at least 300 hPa may be applied by a vacuum pump as part of the recovery apparatus. In the container 11, electrolyte that could not be removed during deactivation is removed from the pulverized material 10.

[0141] According to a preferred embodiment of the method, after deactivation and, if applicable, heating to the electrolyte removal temperature T E Afterwards, the electrode active material is separated from the original crushed material. This preferably includes a combination of mechanical stress, magnetic separation, non-ferrous metal separation, screening and density separation. Screening using air jets is practical, where using finer cut sizes will produce a purer screened material.

[0142] The crushed material 10 is mixed with sulfuric acid 12. The mixing can be stirring using a stirrer, for example. However, the mixing can also be simple addition. In particular, this is feasible if the crushed material 10 is in a reactor, for example in the form of a rotary kiln.

[0143] The crushed material and sulfuric acid can also be mixed in a reaction vessel and then the mixed crushed material is added to a reactor, in particular a rotary kiln.

[0144] It is advantageous if the sulfuric acid 12 is metered via a sulfuric acid supply 43 (see FIG. 2 ). The preferred embodiment of this sulfuric acid supply described with respect to FIG. 2 also applies to Figure 1 The method described in .

[0145] The sulfuric acid 12 is preferably at least 95%. The crushed material 10 and the sulfuric acid 12 are heated to a digestion temperature T A , for example, at least T A = 140° C., in particular at least 150° C. To the extent that the pH value can be determined, the pH value of the mixture of comminuted material and sulfuric acid is below 1.5. However, in general, the water content of the mixture is too low to determine the pH value.

[0146] The digestion produces an offgas 14, which contains in particular hydrogen fluoride HF. The digestion is carried out until the content of fluorine compounds, in particular hydrogen fluoride, in the offgas 14 is below a predetermined threshold, for example, 0.83 mg / m 3 , as determined in a discontinuous comparative test in the container without continuous addition of material. This is checked using a fluoride detector 15 which continuously measures the fluoride concentration.

[0147] If digestion occurs during charging, it is carried out until the fluorine compound content, in particular the hydrogen fluoride content, is below a predetermined threshold value, for example 0.83 mg / m 3 .

[0148] Alternatively or in addition, digestion is performed until the fluoride concentration of water-soluble fluoride in the digested material is c F Below 100 mg / kg digested material, preferably below 10 mg / kg, particularly preferably below the traceability threshold. In other words, the retention time of the comminuted material 10 and the sulfuric acid 12 is selected so that the digested material has a fluoride concentration c of water-soluble fluorides that does not exceed a specified value. F .

[0149] Furthermore, the digested material 16 obtained can be considered very approximately fluoride-free. Water 18 is added to the digested material 16, thereby leaching it. The leaching can be carried out in the same container as the comminuted material for digestion; however, this is not required. For example, the digested material can be placed in a container that preferably already contains water. The leaching is carried out at a pH value of -0.7 to 4, and preferably without actively adding heat or exothermic heat.

[0150] After leaching, the graphite 20 is separated using a graphite separation device 22. In the present case, the graphite separation device 22 is a filter with a pore size of at most 15 microns, preferably at most 10 microns. It is beneficial if the pore size is at least 0.5 microns.

[0151] The graphite 20 can be purified in a subsequent step of the method. This is achieved, for example, by adding water, alcohol, organic solvents or mineral acids, thereby obtaining electrode graphite. Electrode graphite is graphite suitable for making electrodes, in particular for lithium batteries. The separation of the graphite 20 produces a raw material fluid 24.

[0152] Purification of graphite 20 may include heating to T 20 >250℃, especially T Z Decomposition temperature T >350℃ 20 Preferably, T Z <= 430° C. Due to the heating, adhesive residues, for example made of polyvinylidene fluoride (PVFD), are decomposed. This preferably takes place in a sealed container.

[0153] Alternatively or in addition, purification may include classification. However, classification is optional. The diameter of the binder residues is generally smaller than the diameter of the graphite particles, so the content of binder residues can be reduced by filtering out smaller components.

[0154] Alternatively or in addition, purification may include flotation.For example, flotation is performed in an aqueous fluid.

[0155] If the purification includes the addition of a mineral acid, such as hydrofluoric acid or hydrochloric acid, the organosilicon content will also be reduced, which is advantageous.

[0156] Metallic copper Cu is obtained, for example, by plating from the raw material fluid 24. For this purpose, for example, metallic iron is brought into contact with the raw material fluid 24, so that the iron ions are dissolved and the copper is precipitated in metallic form.

[0157] Alternatively, copper is separated in the form of copper sulfide. For example, this is achieved by adding sodium hydrosulfide NaHS for precipitation. The separation of copper produces a decopperized feed stream 26. It has a pH value of 0 to 4, for example pH 1.

[0158] Fe in the copper removal raw material fluid 26 2+ The ions are then oxidized to form Fe 3+ ions. In the present case, this is achieved by adding hydrogen peroxide H2O2. However, different oxidants can also be used. Before oxidation, the pH value of the decoppering feed fluid is below 4.3. This step is preferably carried out without active heat supply or heat release.

[0159] In a subsequent step, iron, aluminum and, if applicable, titanium are precipitated in the form of hydroxides. To this end, the pH is raised to a value between 4.3 and 8.7. This is achieved by adding sodium hydroxide and then separating the resulting precipitate, in particular filtering or centrifuging it. In addition to the separated hydroxides, a pure fluid 28 is obtained.

[0160] It is possible, but not necessary, to purify the pure fluid 28 by removing organic components by means of an activated carbon filter 27 ′. This is not necessary in particular if it has already been purified beforehand, in particular by means of activated carbon 27 .

[0161] It is possible, but not necessary, to remove the zinc and / or copper and / or iron and / or aluminum by ion exchange. This is done using an ion exchanger 29. The stationary phase of the ion exchanger 29 is preferably a chelating agent having aminophosphonic acid groups as functional groups.

[0162] Solvent extraction is used to extract nickel and cobalt from the pure fluid 28. In the present case this is achieved using Cyanex 301 dissolved in an organic solvent, typically kerosene.

[0163] Figure 1 Two solvent extraction steps are shown nested within each other. First, cobalt and nickel are extracted using Cyanex 301 dissolved in kerosene. Stripping with acid, in particular hydrochloric acid or sulfuric acid, is used to obtain a solution 30 containing nickel and cobalt. After further separation using Cyanex 272, they are crystallized separately.

[0164] If a metal, such as manganese, is specifically named as here or generally in the description, this generally refers to the metal in elemental form and compounds containing the metal; it also generally includes metal ions. Thus, the statement that manganese, cobalt and nickel are extracted also means the removal of manganese ions, cobalt ions and nickel ions and any compounds, in particular ions containing manganese, cobalt and nickel.

[0165] Extraction of cobalt and nickel produces a target fluid 32 comprising manganese. The pH of the target fluid 32 may range from -0.7 to 10.5.

[0166] There are (at least) three options for further processing of the target fluid 32. According to a first option, the manganese in the target fluid 32 comprising manganese is removed by solvent extraction. This can happen, for example, using D2EHPA dissolved in kerosene.

[0167] According to the second and third options, the manganese is removed by precipitation, which can be carried out, for example, by adding sodium hydroxide. According to the third option, precipitation can be carried out by adding sodium carbonate.

[0168] The removal of manganese produces a target fluid 34. The most important component of this fluid is lithium ions. According to a first alternative, the lithium can be precipitated as phosphate. For this purpose, sodium phosphate is added to the target fluid 34, for example.

[0169] According to a second alternative, lithium can be precipitated as carbonate from the target fluid 34. This is done, for example, using sodium carbonate. Advantageous temperatures are at most 30 Kelvin below the boiling point of the target fluid 34, preferably above 50° C. As an option, the lithium carbonate is washed with water and / or ethanol at 50-100° C., preferably 80-100° C.

[0170] It is advantageous if the precipitation is preceded by a concentration step, thereby increasing the lithium concentration. Alternatively, the lithium may be precipitated as lithium phosphate; for this purpose, sodium phosphate may be added, for example. Concentration may be performed, for example, by reverse osmosis and / or evaporation.

[0171] According to a third alternative, the lithium is extracted by solvent extraction. Detailed information can be found at Figure 8b Therefore, only the components of the lithium solvent extraction apparatus 84 used to perform the solvent extraction are depicted schematically.

[0172] 2 depicts a schematic diagram of a recycling plant 36 for processing lithium batteries according to the present invention, which in the present case are in the form of pulverized material 10 produced from lithium batteries. Alternatively, electrode materials that do not require pulverization can also be processed in the recycling plant. In the present case, the recycling plant 36 is characterized by having a reactor 40, in which the pulverized material 10 is digested with sulfuric acid 12. The pulverized material 10 and the sulfuric acid 12 are mixed together with a mixer 42. The mixer 42 is advantageous but not necessary. The reactor 40 can be a rotary kiln, but this is not necessary. In particular, the reactor 40 can be a container, as in the present case, which is characterized by having a mixer.

[0173] The sulfuric acid 12 is added through a sulfuric acid supply device 43, which may refer to, for example, a dosing device including a sulfuric acid container 45 and a controllable valve 47. However, the sulfuric acid 12 may also be poured from a container.

[0174] The reactor 40 can be first filled with the pulverized material 10, for example, by means of a conveyor. Then sulfuric acid 12 is quantitatively added via a controllable valve 47. The mixture temperature detection device 41 detects the mixture temperature T of the mixture 39. M Whether the mixture temperature is maintained within the predetermined mixture temperature range I. For example, the mixture temperature detection device 41 is a thermometer. However, the mixture temperature detection device 41 may include a camera and an evaluation unit so that if foam formation is the mixture temperature T of the mixture 39 M The foam formation of the mixture 39 can be detected quantitatively or qualitatively by measuring the foam formation of the mixture 39.

[0175] If the mixture temperature T M If the mixture temperature deviates from the range, the dosage mass flow rate q of sulfuric acid is reduced by further or completely closing valve 47. m If the mixture temperature T M To return to the mixture temperature range I, valve 47 is opened (further).

[0176] Alternatively, the reactor 40 is filled with sulfuric acid 12 and then the crushed material 10 is added, for example, via a conveyor 37, such as a belt conveyor or a screw conveyor. If the mixture temperature T M If the mixture temperature deviates from the range, the mass flow rate q of the crushed material 10 is reduced. 10 , in particular, decreases to zero. If the mixture temperature T M Move back to the mixture temperature range I, then increase the mass flow rate q 10 .

[0177] As another alternative, sulfuric acid 12 and pulverized material 10 are added simultaneously. M If the mixture temperature deviates from the range, the mass flow rate q of the crushed material 10 is reduced. 10, the dose mass flow rate q m Or add mass flow q 10 Or both are reduced, in particular reduced to zero.

[0178] The recovery device 36 has an exhaust device 44 in the form of an exhaust pipe, which can be connected to a vacuum generator to suck the exhaust gas 14 out of the reactor 40. Alternatively, excess pressure in the reactor 40 can push the exhaust gas 14 through the exhaust device 44. The exhaust device 44 can feature a scrubber for scrubbing out hydrogen fluoride. For example, in the scrubber, the exhaust gas 14 is contacted with a calcium compound, such as an aqueous solution containing calcium ions, to scrub hydrogen fluoride from the exhaust gas 14.

[0179] Of course, other methods of removing hydrogen fluoride from the waste gas 14 are conceivable. It is also possible to feed the waste gas 14 via the discharge device 44 to a reactor, wherein the hydrogen fluoride reacts, for example, with organic substances. The fluoride concentration c F Identification was performed using a fluoride detector 15 .

[0180] Arranged downstream of the reactor 40 in the direction of the material flow M is a leaching device 46 , in which the digested material 16 is leached, for example with water.

[0181] A graphite recovery device 48 is arranged downstream of the leaching device 46 in the direction of the material flow M, wherein the graphite recovery device in the present case is characterized only by a graphite separation device 22 in the form of a filter. An optional washing device for washing adhering leaching solution from the graphite is not depicted. It is also possible to first fill the transport container with graphite and then wash the adhering leaching solution after transport to another location.

[0182] The graphite recovery device 48 may include a graphite purification device 49 , which is characterized by a leaching reactor 51 and / or a furnace 53 and / or a classifier 55 .

[0183] The leaching reactor 51 is designed to leach the graphite 20 with a mineral acid, in particular hydrofluoric acid or hydrochloric acid.

[0184] The furnace 53 is designed to heat the graphite 20 to a decomposition temperature T Z When heating is to be carried out in an oxidizing atmosphere, the furnace 53 can be connected to a gas feeder 57 which supplies an oxidizing gas, in particular oxygen or air. If heating is to be carried out in a reducing atmosphere, the gas feeder 57 supplies a reducing gas, for example hydrogen. If heating is to be carried out in an inert atmosphere, the gas feeder 57 supplies a protective gas, for example nitrogen or argon, or alternatively or in addition, a vacuum device is connected to the furnace 57 to apply a vacuum of preferably at least 300 hPa to the furnace.

[0185] The classifier 55 is designed to produce at least a fine fraction and a coarse fraction, wherein the binder content of the binder in the fine fraction is greater than the binder content of the binder in the coarse fraction.

[0186] The graphite purification device 49 may also feature a flotation device for flotation of graphite, by which binder residues may be separated from the graphite 20. The graphite purification device 49 may feature one, two, three or four of the named components. The graphite purification device 49 is also optional.

[0187] As mentioned above, according to Figure 1 According to the embodiment of FIG. 3 , the recovery device 36 may include an ion exchanger 29. Alternatively or in addition, the recovery device 36 may feature one or two activated carbon filters 27, 27'.

[0188] The copper extractor 50 is arranged after the graphite recovery device 48 in the material flow direction. According to a first alternative, the copper extractor comprises a container 52 for infiltrating copper after adding iron, in particular in the form of iron flakes or iron filings, and a precipitated material separator 54 for separating selected copper compounds. For example, the precipitated material separator 54 can be a filter. The pore size of the filter is preferably less than 50 microns and at least 1 micron.

[0189] According to an alternative embodiment, the precipitation material separator is designed to separate copper sulfide and vessel 52 is used for the reaction of feedstock fluid 24 with NaHS, resulting in precipitation of copper sulfide.

[0190] The Fe / Al / Ti separator 56 is arranged behind the copper extractor 50 in the material flow direction, wherein an oxidant 58 is added to the decopperized raw material fluid 26 in the separator. This can be carried out in a first container 60.1. The resulting solution is then transferred, for example pumped, to a second container 60.2. In this second container 60.2, a hydroxide, in particular an alkaline hydroxide, is added. For example, sodium hydroxide is added. This causes aluminum, iron and (if applicable) titanium to precipitate in the form of hydroxides or hydrated oxides. The precipitate is removed by a particle separator 62 arranged downstream in the material flow direction. The particle separator 62 is formed by a filter having a maximum pore size of, for example, 15 microns.

[0191] The resulting pure fluid 28 is fed to a transition metal extraction device 63, in the present case a solvent extraction device 64, which features a Co / Ni solvent extraction device 66. This comprises a plurality of reaction vessels 8.1, 38.2, ... connected to one another as shown in FIG2. The structure of a solvent extraction device is known in the prior art and will therefore not be explained in further detail. This produces a target fluid 32 comprising manganese.

[0192] The target fluid 32 is added to the manganese solvent extraction unit 70 , which generates the target fluid 34 .

[0193] According to an alternative, the target fluid 32 containing manganese is fed to a second precipitation reactor 72 where, after addition of a hydroxide, in particular an alkaline hydroxide such as sodium hydroxide, manganese is precipitated in the form of manganese hydroxide.

[0194] According to a third alternative, the target fluid 32 containing manganese is introduced into a precipitation reactor 74. After the addition of carbonate, in particular sodium carbonate, the manganese is precipitated or separated in the form of manganese carbonate.

[0195] According to a first alternative, the lithium is precipitated as carbonate in a corresponding container by adding sodium carbonate, or according to a second alternative, the lithium is precipitated as phosphate by adding sodium phosphate. The recovery device 36 may include a concentrator 74 for removing water from the target fluid 34 to facilitate precipitation. According to a third alternative, the lithium is extracted by solvent extraction. Detailed information can be found at Figure 8b can be found in the description.

[0196] The recovery device 36 may, but need not necessarily, include a graphite purification device 49. The graphite purification device 49 may include a leaching reactor 51 and / or a furnace 53. As a further alternative or in addition, the graphite purification device 49 may include a classifier 55. This generally applies to all embodiments of the present invention.

[0197] Figure 3 A flow chart of a method for processing pulverized material and / or electrode material free of cobalt, nickel and manganese according to the present invention is shown. It should be noted that the method corresponds to Figure 1 A method in which the steps associated with extracting cobalt, nickel and manganese are omitted. The activated carbon filters 27, 27' are optional, as is the ion exchanger 29.

[0198] Figure 4 A flow chart for processing comminuted material and / or electrode material free of cobalt and nickel but containing manganese is shown. For the extraction of manganese, only the variant of extraction with solvents is depicted. Figure 1 The three alternatives for removing manganese shown in 2 are for Figure 4 The method of is also feasible and represents a preferred embodiment. Three alternatives are precipitation as manganese carbonate, precipitation as manganese hydroxide and solvent extraction.

[0199] An alternative method of recovering the lithium is by precipitation as lithium phosphate or lithium carbonate.

[0200] The activated carbon filters 27 , 27 ′ are optional, as is the ion exchanger 29 .

[0201] Figure 5 A flow chart is depicted of a method for treating electrodes and / or comminuted material free of manganese and nickel but containing cobalt. An alternative method of recovering the lithium is precipitation as lithium phosphate or lithium carbonate. The activated carbon filter 27, 27' is optional, as is the ion exchanger 29.

[0202] Figure 6 A flow chart of a method according to the invention for electrodes and / or comminuted materials that do not contain manganese but contain cobalt and nickel is shown. An alternative method of recovering the lithium is precipitation as lithium phosphate or lithium carbonate. The activated carbon filter 27, 27' is optional, as is the ion exchanger 29.

[0203] Figure 7 A second embodiment of a recovery device 36 according to the invention is depicted, wherein components arranged downstream of the leaching device 46 in the material flow direction are omitted for reasons of clarity.

[0204] It can be seen that the recycling device 36 comprises a comminution unit 118 and a deactivation device 126. The deactivation device 126 is designed as a drying device.

[0205] First, the lithium batteries 110.1, 110.2, ..., in particular the battery system consisting of a plurality of battery modules or battery packs (which in turn consist of a plurality of battery cells), is discharged in the discharge unit 112. If the battery system cannot be conveyed to the shredding unit 118 in another way for geometric or weight reasons, it is necessary to then disassemble the lithium batteries 110 in the disassembly station 114. For this purpose, the battery system is opened and disassembled to such an extent that the modules and / or battery packs can be removed individually, if appropriate. If necessary, the individual lithium batteries can also be separated from the drive electronics.

[0206] The resulting subunits (modules / batteries) and / or units 116.1, 116.2, ... are added to a comminution unit 118. For example, the comminution unit 118 may be a rotary shearing machine having at least one rotor and at least one stator. The comminution unit 118 may also include a cutting mill with one or more rotors.

[0207] The shredding unit 118 shreds the lithium battery 110.i under a protective gas 120, which is drawn, for example, from a protective gas bottle 122. Alternatively or in addition, liquid nitrogen from a liquid nitrogen source 119 may be injected. The protective gas may refer, for example, to nitrogen, a noble gas, carbon dioxide, nitrous oxide or other preferably non-toxic gases.

[0208] During comminution, shredded material 124 is produced which is fed into a deactivation device in the form of a drying device 126. An airlock 128 is arranged between the comminution unit 118 and the drying device 126, which is airtight so that the drying device 126 is substantially separated from the comminution unit 118 and is thus airtight.

[0209] The drying device 126 is connected to a vacuum device 129 including a vacuum pump 130 and generating a vacuum. 126 ≈100±60hPa, preferably 50hPa pressure p 126 It should be noted that within the scope of this description, a vacuum pump should be understood in particular to generally refer to a device that generates a vacuum. A vacuum pump can and preferably, but not necessarily, simultaneously operate as a compressor, so that gas is exhausted therefrom at a pressure greater than the ambient pressure.

[0210] exist Figure 7 In the case shown, the vacuum pump is a compressor which sucks in and compresses the gas 131 present in the drying device 126. Alternatively or in addition, the vacuum device 129 can have a jet pump, in which a jet medium in liquid form is guided at high speed through at least one Venturi nozzle. The jet medium is preferably alkaline and has a pH value of at least pH 1 and is, for example, a 10% potassium hydroxide solution.

[0211] The vacuum device 129 comprises a gas purification device 132 which is arranged between the drying device 126 and the vacuum pump 130 and which in the present case has a condenser 134 and / or an activated carbon filter 136. The condenser is operated at a temperature of, for example, -10°C, so that dimethyl carbonate and ethyl methyl carbonate condense and can be distributed into a condensate container 138. In addition, any water present is separated by freezing. The control valve 140 is designed to be able to cool the gas at a pressure of 10°C. 26 becomes too large and opens at pressure p 126 It is turned off when it becomes too small, i.e. when a predetermined threshold is not reached.

[0212] The drying material is preferably moved in the drying device 126. This can be achieved by stirring with a stirrer 141, such as an anchor stirrer or a rod stirrer having, for example, a rod arranged perpendicular to the stirrer axis. Alternatively, it can be achieved by moving the drying container.

[0213] Drying of the shredded material 124 produces a deactivated comminuted material 10 which is added to the mixer 42 .

[0214] Alternatively, the transport container 146 is then filled with the deactivated pulverized material 10 under vacuum and / or protective gas. The transport container 146 is preferably airtight. It is possible, but not necessary, that the transport container 146 is filled with an inert gas before transportation so that it is at normal pressure. Alternatively, the transport container can also be sealed and transported under vacuum. A vacuum sealing foil can be selected instead of the transport container, for example an aluminum composite foil.

[0215] The comminution unit 118 is fed with protective gas 120 from a vacuum pump 130 via a flushing line 148. If the vacuum pump 130 also serves as a compressor - as in the present case - which represents a preferred embodiment, the protective gas 120 can be drawn from a pressurized gas cylinder 150. Alternatively or in addition, the protective gas 120 can be released into the surroundings after additional purification, if necessary.

[0216] Figure 8a Several variations of another method according to the invention are depicted. Figure 8a It is shown that by extracting cobalt, nickel and silicon from the pure fluid 28, a target fluid 32 containing manganese is obtained.

[0217] According to a first alternative, manganese sulfate or manganese chloride is obtained from the manganese-containing target fluid 32 by crystallization.

[0218] According to a second alternative, the manganese carbonate is obtained by precipitation with a carbonate salt such as sodium carbonate.

[0219] As a third alternative, manganese hydroxide is precipitated, for example, by adding sodium hydroxide. A manganese-free target fluid 76 is produced from a manganese-containing target fluid 32 (from which cobalt has been removed), for example using Cyanex 272. This produces a cobalt-containing fluid 78, from which cobalt is crystallized in the form of cobalt sulfate or cobalt chloride. In addition to the cobalt-containing fluid 78, a cobalt-free fluid 80 is produced, which contains nickel and lithium.

[0220] Figure 8b The further processing of the cobalt-free fluid 80 is shown. First, nickel is extracted by solvent extraction according to a first alternative and the nickel is crystallized as nickel sulfate or nickel chloride from the resulting nickel-containing fluid 82. Alternatively, nickel is precipitated, for example, by adding sodium carbonate. From the resulting target fluid 34, lithium is precipitated as lithium carbonate according to a first alternative, lithium is precipitated as lithium phosphate according to a second alternative, or lithium is extracted, for example, by Cyanex 936 according to a third alternative and then precipitated as lithium carbonate.

[0221] Fig. 9 A recovery device according to another embodiment of the invention is shown.

[0222] Fig.10An embodiment of a graphite purification device 49 is schematically depicted, which has a scrubber 86. The scrubber 86 features a container 88 in which the graphite 20 is mixed with a solvent 90. The temperature of the solvent 90, in the present case water with 10 wt. % N-methyl-pyrrolidone, is heated to T 90 = 60° C. A mixture of solvent 90 and graphite 20 is mixed using a mixer. The solvent is withdrawn from container 88 through separator 92, the temperature is lowered to reduce the solubility of the binder residue in the solvent, and the precipitated binder residue is separated, for example, filtered off. The solvent 90 is then returned to container 88.

[0223] Reference numerals

[0224] 10 Crushed Materials 50 Copper Extractor

[0225] 11 container 51 leaching reactor

[0226] 12 sulfuric acid 52 containers

[0227] 14 Waste gas 53 Furnace

[0228] 15Fluoride detector 54Precipitated material separator

[0229] 16 digestion material 55 classifier

[0230] 18 Water 56 Fe / Al / Ti precipitation material separator

[0231] 57 Gas Supply

[0232] 20 Graphite 58 Oxidant

[0233] 22 graphite separation device 60 container

[0234] 24 Raw material fluid 62 Particle separator

[0235] 26 Copper removal raw material fluid 63 Transition metal extraction device

[0236] 27 Activated carbon filter 64 Solvent extraction device

[0237] 28 Pure Fluid 66 Co / Ni Solvent Extraction Device

[0238] 29 ion exchanger 68 reaction vessel

[0239] 30 solution 70 Mn solvent extraction device

[0240] 32 Target fluid containing manganese 72 Precipitation reactor

[0241] 34 Target fluid 74 Concentrator

[0242] 36 Recovery equipment 76 Target fluid without manganese

[0243] 37 conveyor 78 target fluid containing cobalt

[0244] 38 Electrode materials

[0245] 39 Mixture 80 Target fluid without cobalt

[0246] 82 Nickel-containing target fluid

[0247] 40 reactor 84 lithium solvent extraction device

[0248] 41 mixture temperature detection device 86 scrubber

[0249] 42 mixers 88 containers

[0250] 43 Sulfuric acid supply device

[0251] 44 discharge device 90 solvent

[0252] 45 sulfuric acid container 92 separator

[0253] 46leaching device

[0254] 47 controllable valve 110 lithium battery

[0255] 48 Graphite Recovery Device 114 Disassembly Station

[0256] 49 Graphite Purification Unit 116

[0257] 118 Crushing Unit

[0258] 119 Liquid nitrogen source

[0259] 120 protective gas

[0260] 124 shredded materials

[0261] 126 Drying device

[0262] 128 Airlock

[0263] 129 Vacuum device

[0264] 130 Vacuum Pump

[0265] 131 Gas

[0266] 132 Gas purification device

[0267] 134 Condenser

[0268] 136 Activated carbon filter

[0269] 138 Condensate container

[0270] 140 control valve

[0271] 141 Mixer

[0272] 146 transport container

[0273] 148 flushing line

[0274] 150 pressurized gas cylinder

[0275] c F Fluoride concentration

[0276] MMaterial flow direction

[0277] q m Dose mass flow rate

[0278] T A Digestion temperature

[0279] T Z Decomposition temperature.

Claims

1. A method for recycling lithium batteries, characterized in that: The following steps are involved: (a) using concentrated sulfuric acid (12) at a digestion temperature T less than 100°C A digesting the pulverized material (10) containing the pulverized components of the lithium battery electrode, thereby generating waste gas (14) and digested material (16), (b) discharging the waste gas (14), (c) leaching said digested material (16) and separating graphite (20), thereby producing a feedstock fluid (24) and, wherein said leaching of said digested material is carried out with an aqueous solution, (d) subjecting the digested material (16) to a wet chemical extraction of at least one metal component, (e) purifying graphite (20) to reduce the content of non-metallic impurities, wherein (f) the purification comprises: (i) Heating to the decomposition temperature T of the adhesive Z , the decomposition temperature of the adhesive is T Z is at least 250°C and / or at most 700°C, Wherein, the heating occurs in: In an oxidizing atmosphere, In an inert atmosphere or In reducing atmosphere, or (ii) dissolving the binder from the graphite using a solvent.

2. The method according to claim 1, characterized in that The separation is filtering out the graphite (20).

3. The method according to claim 1, characterized in that The graphite (20) is purified to reduce the content of binder and silicon.

4. The method according to claim 1, characterized in that: Purification includes rinsing and / or washing with acid.

5. The method according to claim 1, characterized in that The method comprises the following steps: - separating copper from the feed fluid (24) to obtain a decoppered feed fluid (26), Therein, an ion exchange is carried out after the copper is separated.

6. The method according to claim 1, characterized in that During wet chemical extraction: - Extraction of manganese before cobalt, and / or - Extract cobalt before nickel.

7. The method according to claim 1, characterized in that The wet chemical extraction comprises the following steps: - removal of cobalt by means of cobalt complexing agents, and / or - Removal of nickel by nickel complexing agents, and / or - removal of manganese by manganese complexing agents, Thus, the target fluid (34) is obtained.

8. The method according to claim 7, characterized in that The method further comprises the following steps: - Extracting lithium from the target fluid (34) by solvent extraction.

9. A recycling device (36) for processing lithium batteries, characterized in that: The recycling device has: (a) a shredding unit (118), the shredding unit (118) being used to shred the lithium battery (110) to obtain shredded material (124), (b) a deactivation unit (126) for deactivating the shredded material (124) to obtain a pulverized material (10), (c) a reactor (40) for digesting with concentrated sulfuric acid (12) at a temperature T of at least 100°C A digesting the pulverized material (10) containing the electrode components of the lithium battery, (d) a sulfuric acid supply device (43) for adding concentrated sulfuric acid (12) to the pulverized material (10), and (e) a discharge device (44) arranged to discharge the waste gas (14) out of the reactor (40), (f) a graphite purification device (49) for reducing the binder content on graphite (20), comprising: (i) a classifier (55), wherein the classifier (55) is used to classify the graphite (20), thereby obtaining at least one fine fraction and one coarse fraction, wherein the binder content in the fine fraction is at least twice as high as the binder content in the coarse fraction, and / or (ii) a scrubber (86) for dissolving the binder from the graphite (20) using a solvent (90), and / or (iii) a leaching reactor (51) for purifying the graphite (20) by flushing and / or washing with an acid and / or an oxidizing agent.

10. A recycling device (36) for processing lithium batteries, characterized in that: The recycling device has: (a) a shredding unit (118), the shredding unit (118) being used to shred the lithium battery (110) to obtain shredded material (124), (b) a deactivation unit (126) for deactivating the shredded material (124) to obtain a pulverized material (10), (c) a reactor (40) for digesting with concentrated sulfuric acid (12) at a temperature T of at least 100°C A digesting the pulverized material (10) containing the electrode components of the lithium battery, (d) a sulfuric acid supply device (43) for adding concentrated sulfuric acid (12) to the pulverized material (10), and (e) a discharge device (44) arranged to discharge the waste gas (14) out of the reactor (40).