Nanofiltration membrane and preparation method thereof
Through the preparation method of polyaryl ether sulfone block polymer composite membrane, the problems of low flux and insufficient tolerance caused by disordered membrane pores of nanofiltration membranes are solved, and a nanofiltration membrane with high flux and good stability is achieved, which is suitable for Water treatment and resource recovery.
Patent Information
- Application Number
- CN202010969023.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-15
AI Technical Summary
The membrane pores of existing nanofiltration membranes are disordered, resulting in low flux, insufficient chlorine resistance, oxidation resistance and temperature resistance, making it difficult to meet the needs of water treatment and resource recovery.
The preparation method of the polyaryl ether sulfone block polymer composite membrane is adopted. The polymer solution is coated on the support and heat treated to form an ordered nanoscale pore structure and improve the flux and chemical and mechanical stability of the membrane.
A nanofiltration membrane with narrow pore size distribution, high flux and good temperature resistance is realized, which is suitable for large-scale production, water treatment and resource recovery.
Smart Images

Figure QLYQS_1 
Figure BDA0002683392590000021 
Figure BDA0002683392590000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiltration membranes, and in particular relates to a polyarylethersulfone block polymer composite membrane which can be used as a nanofiltration membrane and a preparation method thereof. Background Art
[0002] With the continuous improvement of the understanding of environmental protection and comprehensive utilization of resources, more and more membrane technologies are used in sewage treatment. In order to achieve the reuse of resources, people hope to recover valuable substances while treating wastewater. Nanofiltration is a membrane separation process between reverse osmosis and ultrafiltration. The pore size of nanofiltration membranes ranges from a few nanometers. Based on this feature, the nanofiltration process is mainly used for water softening, purification, separation, classification and concentration of substances with a relative molecular mass of hundreds (such as dyes, antibiotics, peptides, polysaccharides and other chemical and bioengineering products classification and concentration), decolorization and deodorization, etc. For example, it can be used to remove Ca in drinking water. 2+ Mg 2+ Hardness components such as ions, trihalomethane intermediates, odor, color, pesticides, synthetic detergents, soluble organic matter and evaporation residues.
[0003] At present, nanofiltration membranes are usually prepared by interfacial polymerization, and are mostly used for proton conduction membranes, and are rarely used for water treatment. For example, the polypiperazineamide nanofiltration membrane prepared by interfacial polymerization has disordered membrane pores on the membrane surface. In actual application, the presence of amide bonds will lead to low chlorine resistance, oxidation resistance and temperature resistance of the membrane, while the disordered state of the surface pores leads to more closed pores in the membrane surface pores, resulting in low flux.
[0004] Therefore, there is a need in the art for a nanofiltration membrane having orderly arranged nanoscale membrane pores, high flux, and good chemical stability, temperature resistance, and mechanical properties. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a method for preparing a polyarylethersulfone block polymer composite membrane that can be used as a nanofiltration membrane, which can prepare an ordered pore nanofiltration membrane with narrow pore size distribution, high flux, good chemical stability, temperature resistance and mechanical properties. In addition, the method of the present invention is simple to operate, has strong feasibility, low cost, and is suitable for large-scale production.
[0006] Specifically, the present invention provides a polymer solution, wherein the polymer solution contains a polyarylethersulfone block polymer having a structure shown in the following formula I, a good solvent, a poor solvent, and an additive:
[0007]
[0008] In formula I, m, n1 and n2 are integers, and 20≤m≤100, n1≥1, n2≥1, the ratio of m / (n1+n2) is between 0.5 and 5, a, b and c are each independently an integer of 0-4, R1, R2 and R3 are each independently selected from: C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl, A and B are each independently selected from H, C1-C5 straight-chain alkyl and C3-C5 branched alkyl, and the number average molecular weight of the polyarylethersulfone block polymer is 10,000-50,000.
[0009] In one or more embodiments, the polymer solution has one or more of the following characteristics:
[0010] (1) In formula I, 20≤m≤40;
[0011] (2) In formula I, the ratio of m / (n1+n2) is between 1.8 and 2.0;
[0012] (3) In formula I, a, b and c are 0;
[0013] (4) In formula I, A and B are both H;
[0014] (5) The number average molecular weight of the polyarylethersulfone block polymer is 10000-30000;
[0015] (6) The good solvent is one or a mixture of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide;
[0016] (7) the poor solvent is one or a mixture of C1-C5 alcohol, water, tetrahydrofuran, acetone, ethylene glycol monomethyl ether and ethylene glycol dimethyl ether; and
[0017] (8) The additive is an inorganic salt, nanoparticles, a surfactant, a co-solvent, a hydrophilic polymer or a combination thereof; preferably, the additive is an inorganic salt and / or nanoparticles; preferably, the inorganic salt is selected from lithium chloride, magnesium sulfate, potassium chloride or a combination thereof, and the nanoparticles are selected from titanium dioxide, graphene or a combination thereof.
[0018] In one or more embodiments, based on the total weight of the polymer solution, in the polymer solution, the content of the polyarylethersulfone block polymer is 1-10wt%, the content of the good solvent is 2-15wt%, the content of the poor solvent is 75-95wt%, and the content of the additive is 0.5-5wt%; preferably, the mass ratio of the good solvent to the poor solvent is 1:5 to 1:35, preferably 1:8 to 3:94.
[0019] In one or more embodiments, the composition of the polymer solution has one or more of the following characteristics, based on the total weight of the polymer solution:
[0020] (1) The content of the polyarylethersulfone block polymer is 2-8wt%;
[0021] (2) The content of the good solvent is 3-10wt%;
[0022] (3) the content of the poor solvent is 80-94 wt %; and
[0023] (4) The content of the additive is 1-2 wt%.
[0024] The present invention also provides a nanofiltration membrane, which comprises a support and a polymer layer, wherein the polymer layer contains a polyarylethersulfone block polymer having a structure shown in the following formula I:
[0025]
[0026] In formula I, m, n1 and n2 are integers;
[0027] 20≤m≤100, preferably 20≤m≤40;
[0028] n1≥1, n2≥1;
[0029] The ratio of m / (n1+n2) is between 0.5 and 5, preferably between 1.8 and 2.0;
[0030] a, b and c are each independently an integer from 0 to 4, preferably 0;
[0031] R1, R2 and R3 are each independently selected from: C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl;
[0032] A and B are each independently selected from H, C1-C5 straight chain alkyl and C3-C5 branched chain alkyl, preferably H;
[0033] The number average molecular weight of the polyarylethersulfone block polymer is 10000-50000, preferably 10000-30000;
[0034] Preferably, the pore size of the nanofiltration membrane is 1-20 nm, preferably 1-10 nm.
[0035] The present invention also provides a method for preparing a nanofiltration membrane, the method comprising the steps of coating the polymer solution described in any embodiment of the present invention on a support, and then performing a heat treatment.
[0036] In one or more embodiments, the heat treatment temperature is 50-90°C, and the heat treatment time is 1-20 min, preferably 3-15 min.
[0037] The present invention also provides a nanofiltration membrane prepared by the method for preparing a nanofiltration membrane described in any embodiment of the text; preferably, the pore size of the nanofiltration membrane is 1-20 nm, preferably 1-10 nm.
[0038] The present invention also provides the use of a polyarylethersulfone block polymer having a structure shown in the following formula I in the preparation of a nanofiltration membrane:
[0039]
[0040] In formula I, m, n1 and n2 are integers;
[0041] 20≤m≤100, preferably 20≤m≤40;
[0042] n1≥1, n2≥1;
[0043] The ratio of m / (n1+n2) is between 0.5 and 5, preferably between 1.8 and 2.0;
[0044] a, b and c are each independently an integer from 0 to 4, preferably 0;
[0045] R1, R2 and R3 are each independently selected from C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl;
[0046] A and B are each independently selected from H, C1-C5 straight chain alkyl and C3-C5 branched chain alkyl, preferably H;
[0047] The number average molecular weight of the polyarylethersulfone block polymer is 10,000-50,000, preferably 10,000-30,000.
[0048] The present invention also provides the use of the nanofiltration membrane described in any embodiment of the present invention in water treatment. DETAILED DESCRIPTION
[0049] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following general description and definition of the terms and expressions mentioned in the specification and claims are provided. Unless otherwise specified, all technical and scientific terms used herein have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.
[0050] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0051] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0052] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0053] Herein, the terms "comprising", "including" or "comprising" indicate that various components can be applied together in the mixture or composition of the present invention. Therefore, the terms "consisting mainly of" and "consisting of" are included in the terms "comprising", "including" or "comprising".
[0054] The inventors of the present invention have found through extensive and in-depth research that by combining the self-assembly phenomenon of polyarylethersulfone block copolymers in solution and the principle of thermally induced phase separation, the prepared nanofiltration membrane has an ordered nanopore size, a narrow pore size distribution, a high flux, and good thermal stability, chemical stability and mechanical properties, and can achieve good separation effects in the fields of high-temperature separation, desalination, solvent separation and material separation. In addition, the preparation method of the nanofiltration membrane provided by the present invention is simple to operate, low in cost, and suitable for industrial production.
[0055] The present invention obtains a polymer solution by mixing polyarylethersulfone block polymer, good solvent, poor solvent and additive, and then coats the polymer solution on a support, and obtains a nanofiltration membrane by heat treatment (i.e., thermal annealing). At the thermal annealing temperature, the block polymer forms an ordered pore structure by self-assembly due to the volatilization of the poor solvent.
[0056] The polyarylethersulfone block polymer suitable for the present invention is a polyarylethersulfone polyether block polymer. In certain embodiments, the polyether block in the polyarylethersulfone block polymer of the present invention is a polyethylene oxide (PEO) block. In certain embodiments, the polyarylethersulfone block polymer suitable for the present invention has a structure shown in the following formula I:
[0057]
[0058] In formula I, m, n1 and n2 are integers, and 20≤m≤100, n1≥1, n2≥1, a, b and c are each independently an integer of 0-4, R1, R2 and R3 are each independently selected from C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl, A and B are each independently selected from H, C1-C5 straight-chain alkyl and C3-C5 branched alkyl, and the number average molecular weight of the polyarylethersulfone block polymer is 10,000-50,000.
[0059] Herein, alkyl refers to a monovalent saturated hydrocarbon group. Examples of C1-C4 alkyls include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl and tert-butyl. Examples of C1-C5 straight-chain alkyls include methyl, ethyl, n-propyl, n-butyl and n-pentyl. Examples of C3-C5 branched-chain alkyls include isopropyl, isobutyl, tert-butyl, 1-methylbutyl and the like.
[0060] Herein, alkenyl refers to a monovalent unsaturated hydrocarbon group containing a carbon-carbon double bond but no carbon-carbon triple bond. Examples of C2-C4 alkenyl include ethenyl, 1-propenyl, 2-propenyl, 3-butenyl, and the like.
[0061] Herein, alkynyl refers to a monovalent unsaturated hydrocarbon group containing a carbon-carbon triple bond. Examples of C2-C4 alkynyl include ethynyl, 2-propynyl, 3-butynyl, and the like.
[0062] In some embodiments, in Formula I, R1, R2 and R3 are each independently selected from C1-C4 alkyl, more preferably each independently selected from C1-C4 straight chain alkyl and C3-C4 straight chain alkyl.
[0063] In some embodiments, in Formula I, a, b and c are 0, ie, substituents R1, R2 and R3 are absent.
[0064] In some embodiments, in Formula I, A and B are H.
[0065] In some embodiments, in Formula I, 20≤m≤40, for example, 25≤m≤35 or m is about 30.
[0066] In a preferred embodiment, in Formula I, the ratio of m / (n1+n2) is between 0.5 and 5, preferably between 1.0 and 3.0, more preferably between 1.8 and 2.0, for example, about 1.875. The present invention has found that a ratio of m / (n1+n2) between 0.5 and 5 is beneficial for the nanofiltration membrane to obtain a desired pore size.
[0067] The number average molecular weight of the polyarylethersulfone block polymer suitable for use in the present invention is preferably 10,000-30,000, such as 10,000-20,000, 12,000-18,000, 14,000-16,000, or about 15,000.
[0068] The polyarylethersulfone block polymer applicable to the present invention can be prepared by methods known in the art, or by methods that are the same or similar to those in the embodiments of the present invention.
[0069] Generally, in the polymer solution of the present invention, the content of the polyarylethersulfone block polymer may be 1-10wt%, preferably 2-8wt%, such as 2-5wt%, 3-8wt%, 5-8wt%, etc., based on the total weight of the polymer solution.
[0070] Herein, the definitions of good solvent and poor solvent are well known in the art. Specifically, a good solvent is a solvent that has a strong solubility for polymer solutes and an interaction parameter (Huggins parameter) χ with the polymer solute that is less than 0.5; a poor solvent is a solvent that has a weak solubility for polymer solutes and an interaction parameter χ with the polymer solute that is greater than 0.5. Therefore, a good solvent suitable for the present invention is a solvent that has an interaction parameter χ with the polyarylethersulfone block in the polyarylethersulfone block polymer described herein that is less than 0.5; a poor solvent suitable for the present invention refers to a solvent that has an interaction parameter χ with the polyarylethersulfone block in the polyarylethersulfone block polymer described herein that is greater than 0.5.
[0071] The interaction parameter χ between the solvent and the polymer solute can be tested by technical means well known in the art, such as, but not limited to, osmotic pressure method, light scattering method, dilute solution viscosity method, etc. For specific operations, please refer to "Polymer Structure and Properties (Structure)" (Ma Dezhu, Science Press, May 2012).
[0072] In certain embodiments, the good solvent suitable for the present invention can be a good solvent for polyarylethersulfone polymer known in the art, including but not limited to N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide or a combination thereof. In the case where the good solvent is a mixture of multiple good solvents, the ratio between the various good solvents is not particularly limited. In certain embodiments, the good solvent in the polymer solution of the present invention is N-methylpyrrolidone or N,N-dimethylacetamide.
[0073] Generally, in the polymer solution of the present invention, the content of the good solvent can be 2-15wt%, preferably 3-10wt%, such as 3-5wt%, 5-10wt%, based on the total weight of the polymer solution. The suitable good solvent content is conducive to dissolving or swelling the polyarylethersulfone block in the polyarylethersulfone block polymer, and at the same time enables the formation of orderly arranged membrane pores on the surface of the filter membrane after heat treatment; too high or too low good solvent content makes it difficult to form orderly arranged membrane pores on the surface of the filter membrane after heat treatment.
[0074] In certain embodiments, the poor solvent suitable for the present invention may be a poor solvent for polyarylethersulfone polymers known in the art, including but not limited to small molecule alcohols (usually C1-C5 alcohols, which may be monoalcohols or polyols, such as methanol, ethanol, ethylene glycol, n-propanol, isopropanol, glycerol, etc.), water, tetrahydrofuran, acetone, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether or a combination thereof. In certain embodiments, the poor solvent suitable for the present invention is acetone or tetrahydrofuran. In the case where the poor solvent is a mixture of multiple poor solvents, the ratio between the various poor solvents is not particularly limited. For example, in certain embodiments, the poor solvent suitable for the present invention is a mixture of ethylene glycol monomethyl ether and tetrahydrofuran in a mass ratio of 1:5 to 5:1; in certain embodiments, the poor solvent suitable for the present invention is a mixture of isopropanol and water in a mass ratio of 1:5 to 5:1; in certain embodiments, the poor solvent suitable for the present invention is a mixture of ethylene glycol monomethyl ether and acetone in a mass ratio of 1:5 to 5:1.
[0075] In the present invention, the poor solvent can dissolve or swell the polyether (in some embodiments, polyethylene oxide) block portion of the polyarylethersulfone block polymer, thereby forming orderly arranged membrane pores on the surface of the filter membrane. In some embodiments, the membrane pores on the filter membrane are arranged in a honeycomb shape on the surface of the filter membrane.
[0076] Generally, in the polymer solution of the present invention, the content of the poor solvent can be 75-95wt%, preferably 80-94wt%, such as 80-90wt%, 85-94wt%, 85-90wt%, based on the total weight of the polymer solution. Suitable poor solvent content is conducive to dissolving or swelling the polyether block in the polyarylethersulfone block polymer, and at the same time enables orderly arranged membrane pores to be formed on the surface of the filter membrane after heat treatment; too high or too low poor solvent content is difficult to achieve orderly arranged membrane pores on the surface of the filter membrane after heat treatment.
[0077] In a preferred embodiment, in the polymer solution, the mass ratio of the good solvent to the poor solvent is 1:5 to 1:35, preferably 1:7 to 1:32, more preferably 1:8 to 3:94, for example, about 1:18, 3:94, 3:88, 1:30, 3:87 or 1:8, or within the range of any two of these ratios. A suitable mass ratio of the good solvent to the poor solvent enables orderly arranged membrane pores to be formed on the surface of the filter membrane after heat treatment. Too high or too low a mass ratio of the good solvent to the poor solvent makes it difficult to achieve orderly arranged membrane pores on the surface of the filter membrane after heat treatment.
[0078] Herein, additive has the meaning well known in the art, and generally refers to the components other than film-forming polymer, polymerization monomer, solvent / non-solvent added to improve the properties or processing properties of nanofiltration membrane. The additive applicable to the present invention can be the additive commonly used in the preparation of nanofiltration membrane in the art, including but not limited to inorganic salts, nanoparticles, surfactants, cosolvents, hydrophilic polymers, etc. In the present invention, the additive can interact with the partial blocks of the polyarylethersulfone block polymer, which is conducive to the self-assembly of the block polymer. In certain embodiments, the present invention uses inorganic salts and / or nanoparticles as additives.
[0079] The inorganic salts applicable to the present invention are not particularly limited, and may be inorganic salts commonly used in preparing nanofiltration membranes, such as but not limited to lithium chloride, magnesium sulfate, potassium chloride or a combination thereof. The nanoparticles applicable to the present invention are not particularly limited, and may be nanoparticles commonly used in preparing nanofiltration membranes, such as but not limited to titanium dioxide, graphene or a combination thereof. In certain embodiments, the additive applicable to the present invention is lithium chloride or titanium dioxide.
[0080] Generally, in the polymer solution of the present invention, the content of the additive may be 0.5-5wt%, preferably 0.5-3wt%, such as 0.5-2wt%, 1-3wt%, 1-2wt%, based on the total weight of the polymer solution.
[0081] The method for preparing the nanofiltration membrane of the present invention comprises the steps of coating the polymer solution described in any embodiment of the present invention on a support body and then performing heat treatment.
[0082] The polymer solution can be coated on a support to form a membrane by conventional methods in the art to obtain a semi-finished nanofiltration membrane. Usually, the polymer solution is stirred evenly, allowed to stand for degassing, and then coated on a support to form a membrane.
[0083] The support body applicable to the present invention can be a conventional support body for nanofiltration membrane in the art, including but not limited to non-woven fabrics or hollow fiber membranes. The polymer constituting the support body is not particularly limited, and can be, for example, polyester, bisphenol A type polysulfone, polyethersulfone, polyphenol, polyetherketone, polysulfoneketone, polyetheretherketone, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylonitrile, polyamide, polyvinyl chloride, cellulose acetate, cellulose nitrate, mixed cellulose ester, polypropylene or any combination thereof.
[0084] The temperature for heat treatment of the nanofiltration membrane semi-finished product is usually between 50-90°C, for example, between 50-70°C or between 70-90°C. A suitable heat treatment temperature enables orderly arranged membrane pores to be formed on the surface of the filter membrane after heat treatment; too high or too low heat treatment temperature makes it difficult to form orderly arranged membrane pores on the surface of the filter membrane after heat treatment. The heat treatment time is usually between 1-20 minutes, for example, between 3-15 minutes. After heat treatment, the membrane obtained by heat treatment can be conventionally cleaned with water. The nanofiltration membrane semi-finished product is heat treated to obtain a nanofiltration membrane finished product.
[0085] Typically, after weighing the polyarylethersulfone block polymer, good solvent, poor solvent, and additive according to the content ratio described herein, the four raw materials are mixed evenly to obtain a polymer solution. In certain embodiments, the polyarylethersulfone block polymer is first weighed and dissolved in a good solvent, and then a poor solvent is added, stirred at 50-70°C, and then the additive is added, and continued to be stirred evenly to obtain a polymer solution. After standing and degassing, the polymer solution is coated on a support to form a film, placed in an oven at 50-90°C and heated for 1-20min, for example, 3-15min, and washed with water to obtain a nanofiltration membrane.
[0086] The present invention also includes a nanofiltration membrane, which includes a support and a polymer layer, wherein the polymer layer contains a polyarylethersulfone block polymer having a structure shown in the following formula I:
[0087]
[0088] In formula I, m, n1 and n2 are integers;
[0089] 20≤m≤200, preferably 20≤m≤40;
[0090] n1≥1, n2≥1;
[0091] The ratio of m / (n1+n2) is between 0.5 and 5, preferably between 1.8 and 2.0;
[0092] a, b and c are each independently an integer from 0 to 4, preferably 0;
[0093] R1, R2 and R3 are each independently selected from C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl;
[0094] A and B are each independently selected from H, C1-C5 straight chain alkyl and C3-C5 branched chain alkyl, preferably H.
[0095] The number average molecular weight of the polyarylethersulfone block polymer in the polymer layer of the nanofiltration membrane of the present invention is usually 10,000-100,000, preferably 10,000-30,000.
[0096] The polyarylethersulfone block polymer contained in the nanofiltration membrane of the present invention may be the polyarylethersulfone block polymer described in any embodiment of the present invention. The nanofiltration membrane of the present invention may be prepared by the method described in any embodiment of the present invention.
[0097] The nanofiltration membrane (polyarylethersulfone block polymer composite membrane) of the present invention has an ordered pore structure, that is, the membrane pores of the nanofiltration membrane of the present invention are orderly arranged on the surface of the nanofiltration membrane. In certain embodiments, the membrane pores of the nanofiltration membrane of the present invention are arranged in a honeycomb shape on the surface of the nanofiltration membrane.
[0098] The nanofiltration membrane of the present invention has a narrow pore size distribution, that is, the pore size is relatively uniform. In certain embodiments, the pore size of the nanofiltration membrane of the present invention is 1-20 nm, preferably 1-10 nm, such as 2-8 nm, 4-6 nm, 5 nm or so.
[0099] The nanofiltration membrane of the present invention can be used for softening and purifying water, separating, grading and concentrating substances with a relative molecular mass of 100 (such as grading and concentrating chemical and bioengineering products such as dyes, antibiotics, polypeptides, polysaccharides), decolorizing and removing odors, etc. In particular, the nanofiltration membrane of the present invention can be used to remove hardness components such as Ca and Mg ions, trihalomethane intermediates, odor, chromaticity, pesticides, synthetic detergents, soluble organic matter and evaporation residues in drinking water. Therefore, the present invention also includes the use of the nanofiltration membrane described in any embodiment of the present invention in water treatment; preferably, the water treatment is selected from: softening of water, purification of water, separation, grading and concentration of substances with a relative molecular mass of 100 in water, decolorization of water and removal of odors from water; in some embodiments, the water treatment is to remove hardness components, trihalomethane intermediates, odor, chromaticity, pesticides, synthetic detergents, soluble organic matter and / or evaporation residues in water, such as removing MgSO4 and / or Na2SO4 in water.
[0100] Compared with the traditional nanofiltration membrane and its preparation method, the present invention has the following advantages:
[0101] (1) The nanofiltration membrane preparation method of the present invention is simple to operate, low in cost, and suitable for large-scale production, while the preparation process of the traditional method is complicated;
[0102] (2) The nanofiltration membrane of the present invention has an ordered nanopore structure and a narrow pore size distribution, while the membrane pores of the nanofiltration membrane prepared by the conventional method are generally disordered and have a wide pore size distribution;
[0103] (3) The nanofiltration membrane of the present invention has a very high membrane flux and a good separation effect, and has better thermal stability, chemical stability and mechanical properties than traditional nanofiltration membranes.
[0104] Example
[0105] The present invention is further described in detail below in conjunction with examples. It should be understood that the following examples are implemented according to the technical solution of the present invention, and detailed implementation methods and specific operating procedures are provided, but these examples are merely illustrative, and the protection scope of the present invention is not limited to the following examples. For the reagents, methods, conditions, etc. used herein and in the examples, unless otherwise stated, they are all conventional reagents, methods and conditions.
[0106] The test method used in the examples is as follows:
[0107] (1) Number average molecular weight: The number average molecular weight of the polymer was determined by gel permeation chromatography (GPC) by dissolving the polymer in DMF for testing;
[0108] (2) Aperture: FE-SEM was used to characterize the pore size.
[0109] The block polymers used in Examples 1-6 were prepared by the following method:
[0110] (1) dissolving 4,4'-difluorodiphenyl sulfone and bisphenol Z in dimethyl sulfoxide (DMSO), adding potassium carbonate as a salt-forming agent and a catalyst, and adding toluene as a water-carrying agent, wherein the molar ratio of 4,4'-difluorodiphenyl sulfone to bisphenol Z is 0.9:0.1, the molar amount of potassium carbonate is 120% of the molar amount of 4,4'-difluorodiphenyl sulfone, and the volume ratio of DMSO to toluene is 5:4;
[0111] (2) The reaction was carried out in two stages. The first stage was the azeotropic dehydration stage. The reaction temperature was 120°C and the reaction lasted for 4 hours. The temperature was then raised to 220°C and the reaction lasted for 8 hours.
[0112] (3) Add a DMSO solution of PEO (number average molecular weight 370) and continue the reaction for 4 hours; cool, wash and desalt to obtain a block polymer.
[0113] The number average molecular weight of the polyarylethersulfone block polymer measured by GPC is 15000. According to the number average molecular weight and the preparation process, the block polymer has a structure shown in the following formula II:
[0114]
[0115] In formula II, m is about 30 on average, (n1+n2) is about 16 on average, n1≥1, n2≥1.
[0116] Example 1
[0117] Weigh 3g of block polymer and dissolve it in 5g of N,N-dimethylacetamide (good solvent), add 90g of a mixture of ethylene glycol monomethyl ether and tetrahydrofuran (poor solvent) with a mass ratio of 1:1, stir at 60°C, then add 2g of lithium chloride, continue to stir evenly, let it stand for degassing, and then apply it on a non-woven fabric to form a film. Place it in an oven at 50°C for thermal annealing for 15 minutes, wash it with water, and obtain a nanofiltration membrane.
[0118] Example 2
[0119] The method used in this embodiment is substantially the same as the method in the above-mentioned embodiment 1, except that: in this embodiment, the amount of the block polymer used is 2 g, the amount of the good solvent N-methylpyrrolidone used is 3 g, the amount of the poor solvent mixture of isopropanol and water with a mass ratio of 3:1 is 94 g, the amount of the additive lithium chloride used is 1 g, and the heat treatment temperature and time are 90° C. and 15 min, respectively.
[0120] Example 3
[0121] The method used in this embodiment is substantially the same as the method in the above-mentioned embodiment 1, except that: in this embodiment, the amount of the block polymer used is 8 g, the amount of the good solvent N-methylpyrrolidone used is 3 g, the amount of the poor solvent mixture of isopropanol and water with a mass ratio of 3:1 is 88 g, the amount of the additive lithium chloride used is 1 g, and the heat treatment temperature and time are 90° C. and 15 min, respectively.
[0122] Example 4
[0123] The method used in this embodiment is substantially the same as the method in the above-mentioned embodiment 1, except that: in this embodiment, the amount of block polymer used is 5 g, the amount of good solvent N,N-dimethylacetamide used is 3 g, the amount of poor solvent acetone used is 90 g, the amount of additive lithium chloride used is 2 g, and the heat treatment temperature and time are 70° C. and 3 min, respectively.
[0124] Example 5
[0125] The method used in this embodiment is substantially the same as the method in the above-mentioned embodiment 1, except that: in this embodiment, the amount of block polymer used is 8 g, the amount of good solvent N,N-dimethylacetamide used is 3 g, the amount of poor solvent tetrahydrofuran used is 87 g, the amount of additive lithium chloride used is 2 g, and the heat treatment temperature and time are 70° C. and 3 min, respectively.
[0126] Example 6
[0127] The method used in this embodiment is substantially the same as the method in the above-mentioned embodiment 1, except that: in this embodiment, the amount of block polymer used is 8 g, the amount of good solvent N-methylpyrrolidone used is 10 g, the amount of poor solvent ethylene glycol monomethyl ether and acetone with a mass ratio of 4:1 is 80 g, the amount of additive titanium dioxide used is 2 g, and the heat treatment temperature and time are 50°C and 3 min, respectively.
[0128] Test Case
[0129] This test example is used to test the separation performance of the nanofiltration membranes prepared in Examples 1-6.
[0130] 500 mg / L NaCl, 1000 mg / L MgSO4 and 1000 mg / L Na2SO4 aqueous solutions were used as feed materials, and the permeation water flux of the block polymer nanofiltration membrane was tested using a homemade nanofiltration membrane evaluation device. The relevant concentrations were deduced by measuring the conductivity of the feed liquid and the conductivity of the permeate, and then the desalination rate R was calculated according to formula (1), and the water flux F of the membrane was calculated according to formula (2). In the present invention, the effective area of the membrane is 113.04 cm 2 The test pressure is 0.3MPa.
[0131] R=(Cf-Cp) / Cf×100% (1)
[0132] F=V / At (2)
[0133] Wherein, Cf is the feed solution concentration, Cp is the permeate concentration, V is the volume of permeated water, A is the effective area of the membrane, and t is the time.
[0134] The test results of water flux and salt rejection rate of the nanofiltration membranes prepared in the above Examples 1-6 are shown in Tables 1-6.
[0135] Table 1: Test results of the nanofiltration membrane prepared in Example 1 for different salt solutions
[0136] Test fluid Flux (LMH) Desalination rate (%) NaCl 70 30% <![CDATA[MgSO4]]> 46 97% <![CDATA[Na2SO4]]> 51 95%
[0137] Table 2: Test results of the nanofiltration membrane prepared in Example 2 for different salt solutions
[0138] Test fluid Flux (LMH) Desalination rate (%) NaCl 75 10% <![CDATA[MgSO4]]> 43 95% <![CDATA[Na2SO4]]> 51 90%
[0139] Table 3: Test results of the nanofiltration membrane prepared in Example 3 for different salt solutions
[0140] Test fluid Flux (LMH) Desalination rate (%) NaCl 54 60% <![CDATA[MgSO4]]> 42 98% <![CDATA[Na2SO4]]> 47 96%
[0141] Table 4: Test results of the nanofiltration membrane prepared in Example 4 for different salt solutions
[0142]
[0143]
[0144] Table 5: Test results of the nanofiltration membrane prepared in Example 5 for different salt solutions
[0145] Test fluid Flux (LMH) Desalination rate (%) NaCl 53 50% <![CDATA[MgSO4]]> 45 97% <![CDATA[Na2SO4]]> 49 92%
[0146] Table 6: Test results of the nanofiltration membrane prepared in Example 6 for different salt solutions
[0147] Test fluid Flux (LMH) Desalination rate (%) NaCl 56 45% <![CDATA[MgSO4]]> 44 96% <![CDATA[Na2SO4]]> 49 90%
[0148] From the experimental results in Tables 1-6, it can be seen that the nanofiltration membrane of the present invention has a very high membrane flux, has a good interception effect on MgSO4 and Na2SO4, can well distinguish the salt solution of monovalent and divalent anions, and exhibits the characteristics of the nanofiltration membrane. The FE-SEM observation results show that the membrane pores on the surface of the nanofiltration membrane of the present invention are orderly arranged in a honeycomb shape, the pore size is about 5nm, the pore size distribution is narrow, and there are fewer closed pores in the nanofiltration membrane, so it has a very high membrane flux and a good separation effect.
[0149] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a nanofiltration membrane, characterized in that: The method comprises the steps of coating a polymer solution on a support and then performing a heat treatment; the polymer solution is composed of a polyarylethersulfone block polymer having a structure shown in the following formula I, a good solvent, a poor solvent and an additive. composition: Formula I In formula I, m, n1 and n2 are integers, and 20≤m≤100, n1≥1, n2≥1, the ratio of m / (n1+n2) is between 0.5 and 5, a, b and c are each independently an integer of 0-4, R1, R2 and R3 are each independently selected from C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl, A and B are each independently selected from H, C1-C5 linear alkyl and C3-C5 branched alkyl, and the number average molecular weight of the polyarylethersulfone block polymer is 10000-50000; Based on the total weight of the polymer solution, in the polymer solution, the content of the polyarylethersulfone block polymer is 1-10wt%, the content of the good solvent is 2-15wt%, the content of the poor solvent is 75-95wt%, and the content of the additive is 0.5-5wt%; the mass ratio of the good solvent to the poor solvent is 1:5 to 1:
35.
2. The method according to claim 1, characterized in that The mass ratio of good solvent to poor solvent is 1:8 to 3:
94.
3. The method according to claim 1, characterized in that The polymer solution has one or more of the following characteristics: (1) In formula Ⅰ, 20≤m≤40; (2) In formula Ⅰ, the ratio of m / (n1+n2) is between 1.8 and 2.0; (3) In formula I, a, b and c are 0; (4) In formula I, A and B are H; (5) The number average molecular weight of the polyarylethersulfone block polymer is 10,000-30,000; (6) The good solvent is one or a mixture of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide; (7) The poor solvent is one or a mixture of C1-C5 alcohol, water, tetrahydrofuran, acetone, ethylene glycol monomethyl ether and ethylene glycol dimethyl ether; and (8) The additive is an inorganic salt, nanoparticles, a surfactant, a co-solvent, a hydrophilic polymer or a combination thereof.
4. The method according to claim 3, characterized in that The additive is an inorganic salt and / or nanoparticles.
5. The method according to claim 4, characterized in that The inorganic salt is selected from lithium chloride, magnesium sulfate, potassium chloride or a combination thereof, and the nanoparticles are selected from titanium dioxide, graphene or a combination thereof.
6. The method according to claim 1, characterized in that The composition of the polymer solution has one or more of the following characteristics, based on the total weight of the polymer solution: (1) The content of the polyarylethersulfone block polymer is 2-8wt%; (2) The content of the good solvent is 3-10wt%; (3) the content of the poor solvent is 80-94wt%; and (4) The content of the additive is 1-2wt%.
7. The method according to claim 1, characterized in that The heat treatment temperature is 50-90° C., and the heat treatment time is 1-20 min.
8. The method according to claim 7, characterized in that The heat treatment time is 3-15min.
9. A nanofiltration membrane prepared by the method according to any one of claims 1 to 8.
10. The nanofiltration membrane according to claim 9, characterized in that The pore size of the nanofiltration membrane is 1-20 nm.
11. The nanofiltration membrane according to claim 9, characterized in that The pore size of the nanofiltration membrane is 1-10 nm.
12. Use of the nanofiltration membrane according to any one of claims 9 to 11 in water treatment.