Method for recovering methane from waste gas produced by oxidative coupling of methane to produce ethylene

By using catalysts loaded with CexZr1-xO2 and CuO to efficiently remove carbon monoxide and hydrogen in OCM exhaust gas, the recovery and recycling of methane is achieved, and the problem of methane in the exhaust gas is solved, and the utilization efficiency of raw methane is improved.

CN114181033BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010962915.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-12-06
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

In the prior art, carbon monoxide and hydrogen in the exhaust gas during the preparation of ethylene by methane oxidative coupling (OCM) is difficult to effectively remove, resulting in methane not being effectively recycled and affecting the utilization efficiency of the raw material methane.

Method used

Molded alumina supported by CexZr1-xO2 is used as a support and combined with CuO as a catalyst for active components to obtain methane by reacting with an oxygen source, thereby achieving efficient conversion of carbon monoxide and hydrogen in the exhaust gas and recycling of methane.

Benefits of technology

The catalyst can efficiently convert carbon monoxide and hydrogen, ensure low conversion of methane, reaching carbon monoxide conversion rate >70%, hydrogen conversion rate >70%, methane conversion rate <4.5%, and recycle the recovered methane to the reactor to continue the reaction. Improve the utilization efficiency of methane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002681164800000111
    Figure BDA0002681164800000111
Patent Text Reader

Abstract

The present invention provides a method for recovering methane from waste gas produced by oxidative coupling of methane to produce ethylene, which comprises reacting the waste gas produced by oxidative coupling of methane to produce ethylene with an oxygen source in the presence of a formed catalyst; wherein the formed catalyst is loaded with Ce x Zr 1‑x The formed alumina of O2 is used as a carrier, x=0-1, and CuO is used as an active component. In the method provided by the present invention, the catalyst has a high mechanical strength and can better remove carbon monoxide and hydrogen in the tail gas of the methane oxidative coupling reaction to produce ethylene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recovering methane from waste gas produced by oxidative coupling of methane to prepare ethylene. Background Art

[0002] The technology of producing ethylene by oxidative coupling of methane (OCM) has potential application value in the field of petrochemical industry. After the raw material passes through the catalyst bed once, about 50wt% of methane will be converted into the main products ethylene and ethane and the byproducts hydrogen, carbon monoxide and carbon dioxide. After the material output from the reactor is subjected to the removal of carbon dioxide and the separation of ethylene and ethane, the main byproducts are unreacted methane, carbon monoxide and hydrogen. In order to improve the utilization efficiency of raw methane, patent CN 109456139 A treats the OCM reaction product by rapid cooling, compression and pressure increase, impurity removal, and gas-liquid separation, and uses membrane separation technology to separate the methane in the non-condensable gas and return it to the OCM reactor for recycling. Patent CN 108137435 A uses an adsorption-desorption method to recycle unreacted methane. Selective catalytic oxidation can also be used to purify OCM tail gas, that is, the OCM tail gas passes through the catalyst bed at a certain temperature, carbon monoxide and hydrogen are oxidized, and methane is not consumed or consumed very little. After the methane is purified, it can be fed together with fresh methane to improve the efficiency of methane utilization. The use of powder catalyst can remove carbon monoxide and hydrogen in the tail gas.

[0003] Having the necessary mechanical strength is one of the properties that industrial heterogeneous catalysts must have, so catalyst molding is one of the important steps in the industrial catalyst preparation process. So far, there has been no report on the molding method of catalyst carriers suitable for OCM tail gas purification. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the object of the present invention is to provide a catalyst with high mechanical strength, which can better remove carbon monoxide and hydrogen in the tail gas of the methane oxidative coupling reaction to produce ethylene, thereby recovering methane.

[0005] The first aspect of the present invention provides a method for recovering methane from waste gas produced by oxidative coupling of methane to produce ethylene, which comprises reacting the waste gas produced by oxidative coupling of methane to produce ethylene with an oxygen source in the presence of a formed catalyst; wherein the formed catalyst is loaded with Ce x Zr 1-x The formed alumina of O2 is used as the carrier, x=0-1, and CuO is used as the active component.

[0006] According to some embodiments of the invention, x=0.1-0.7.

[0007] According to some preferred embodiments of the present invention, x=0.1-0.5.

[0008] According to some embodiments of the present invention, the method comprises contacting the waste gas produced by oxidative coupling of methane to produce ethylene with an oxygen source in the presence of a formed catalyst, and then separating and obtaining methane.

[0009] According to some embodiments of the present invention, the oxygen source is oxygen gas and / or air.

[0010] According to some embodiments of the present invention, in the shaped catalyst, based on the total weight of the carrier, Ce x Zr 1-x The mass content of O2 is 2-15%, for example 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% and any value therebetween.

[0011] According to some embodiments of the present invention, in the shaped catalyst, based on the total weight of the carrier, Ce x Zr 1-x The mass content of O2 is 5-15%.

[0012] According to some embodiments of the present invention, in the shaped catalyst, based on the total weight of the carrier, Ce x Zr 1-x The mass content of O2 is 5-10%.

[0013] According to some embodiments of the present invention, in the molded catalyst, the mass content of CuO is 2-15%, for example, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% and any value therebetween, based on the total weight of the carrier.

[0014] According to a preferred embodiment of the present invention, in the molded catalyst, the mass content of CuO is 5-10% based on the total weight of the catalyst.

[0015] According to some embodiments of the present invention, the method for preparing the catalyst comprises first loading Ce on a shaped alumina carrier; x Zr 1-x O2, and then loaded with CuO.

[0016] According to the present invention, the shaped alumina loads Ce x Zr 1-x The preparation method of O2 is not limited. According to some embodiments of the present invention, the Ce loaded x Zr 1-x O2 can be deposited by precipitation and / or impregnation.

[0017] According to some embodiments of the present invention, the load Ce x Zr 1-x O2 is a single load or multiple loads.

[0018] According to some embodiments of the present invention, the CuO is loaded by an impregnation method.

[0019] According to some embodiments of the present invention, the method for forming a catalyst comprises the following steps:

[0020] S1: Mix the aqueous solution of cerium salt and the aqueous solution of zirconium salt with the formed alumina for impregnation, drying and calcination to obtain Ce-loaded alumina. x Zr 1-x Shaped alumina carrier for O2;

[0021] S2: The aqueous solution of copper salt and the loaded Ce x Zr 1-x The shaped alumina carrier of O2 is mixed and impregnated, dried and calcined to obtain the shaped catalyst.

[0022] According to some other embodiments of the present invention, the method for forming a catalyst comprises the following steps:

[0023] N1: Mix the aqueous solution of cerium salt and zirconium salt with the formed alumina, add alkaline solution for precipitation, wash, dry and calcine to obtain Ce loaded alumina. x Zr 1-x Shaped alumina carrier for O2;

[0024] N2: The aqueous solution of copper salt and the loaded Ce x Zr 1-x The shaped alumina carrier of O2 is mixed and impregnated, dried and calcined to obtain the shaped catalyst.

[0025] According to some embodiments of the present invention, the shaped alumina is spherical alumina.

[0026] According to some embodiments of the present invention, the cerium salt is a water-soluble cerium salt.

[0027] According to some embodiments of the present invention, the cerium salt is selected from at least one of cerium nitrate, ammonium cerium nitrate, cerium sulfate and cerium chloride, and more preferably selected from cerium nitrate.

[0028] According to some embodiments of the present invention, the zirconium salt is a water-soluble zirconium salt.

[0029] According to some embodiments of the present invention, the zirconium salt is selected from at least one of zirconium oxychloride, zirconium chloride, zirconium sulfate and zirconium nitrate, and more preferably selected from zirconium nitrate.

[0030] According to some embodiments of the invention, the copper salt is a water-soluble copper salt.

[0031] According to some embodiments of the present invention, the copper salt is selected from at least one of copper nitrate, copper chloride and copper sulfate, and more preferably selected from copper nitrate.

[0032] According to some embodiments of the present invention, the alkaline solution is selected from aqueous ammonia and / or sodium carbonate solution.

[0033] According to some embodiments of the present invention, in step S1 or N1, the drying temperature is 60-120°C.

[0034] According to some embodiments of the present invention, in step S1 or N1, the calcination temperature is 400-800°C.

[0035] According to some embodiments of the present invention, in step S1 or N1, the time is 2-10 hours.

[0036] According to some embodiments of the present invention, in step S2 or N2, the drying temperature is 60-120°C.

[0037] According to some embodiments of the present invention, in step S2 or N2, the calcination temperature is 400-800°C.

[0038] According to some embodiments of the present invention, in step S2 or N2, the time is 2-10 hours.

[0039] According to some embodiments of the present invention, the waste gas produced by oxidative coupling of methane to produce ethylene comprises methane, carbon monoxide and hydrogen.

[0040] According to some embodiments of the present invention, the volume ratio of methane, carbon monoxide and hydrogen is (12-18):(2-5):1.

[0041] According to a preferred embodiment of the present invention, the volume ratio of methane, carbon monoxide and hydrogen is (15-17):(2-4):1.

[0042] According to some embodiments of the present invention, the total reaction space velocity of the contact is 10-200 L·h -1 ·g -1 .

[0043] According to a preferred embodiment of the present invention, the total reaction space velocity of the contact is 13-150 L·h -1 ·g -1 .

[0044] According to some embodiments of the present invention, the contact temperature is 200-700°C, for example, it can be 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C and any value therebetween.

[0045] According to a preferred embodiment of the present invention, the contacting temperature is 350-600°C.

[0046] The second aspect of the present invention provides an application of the method according to the first aspect in the oxidative coupling reaction of methane to ethylene.

[0047] The cerium-zirconium oxide Ce according to the present invention x Zr 1-x O2 / spherical alumina loaded CuO is used for OCM exhaust gas purification.

[0048] According to the present invention, the tail gas can reach the effects of carbon monoxide conversion rate>70%, hydrogen conversion rate>70%, and methane conversion rate<4.5% by passing through the catalyst bed once. Under the preferred operating conditions, the carbon monoxide conversion rate>90%, hydrogen conversion rate>85%, and methane conversion rate<3% can be achieved. The obtained methane can be circulated and transported to the reactor for further reaction. DETAILED DESCRIPTION

[0049] In order to make the present invention easy to understand, the present invention will be described in detail below with reference to embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.

[0050] Unless otherwise specified, the raw materials or components used in the present invention can be obtained through commercial routes or conventional methods.

[0051] Example 1

[0052] Weigh 0.54g of cerium nitrate hexahydrate and 4.76g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 60℃, heating to 450℃ at 5℃ / min, maintaining for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0053] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0054] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (2.8ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 13vol%, H2 1vol%, and the balance was methane, 40ml / min) and oxygen (2.8ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0055] Example 2

[0056] Weigh 0.72g of cerium nitrate hexahydrate and 2.89g of zirconium nitrate pentahydrate, dissolve in 21ml of water, add 30g of spherical alumina dropwise to the solution while stirring, stir evenly and let stand for 5h, dry at 80℃, heat to 600℃ at 5℃ / min, keep for 5h, cool to room temperature, and repeat the above operation twice to obtain cerium zirconium oxide Ce. 0.2 Zr 0.8 O2 / spherical alumina.

[0057] Weigh 0.48g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.2 Zr 0.8 O2 / spherical alumina 2.98g, rotary evaporate to dryness, dry at 60°C, heat to 600°C at 5°C / min, maintain for 5h, to obtain a molded catalyst.

[0058] In a quartz glass tube reactor (inner diameter of 8mm), 0.15g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (100ml / min) and oxygen (7ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 13vol%, H2 1vol%, and the balance was methane, 100ml / min) and oxygen (7ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0059] Example 3

[0060] Weigh 0.82g of cerium nitrate hexahydrate and 1.90g of zirconium nitrate pentahydrate, dissolve in 100ml of water, add 30g of spherical alumina, slowly add ammonia solution (1mol / L) until the pH of the solution is 10, continue stirring for 30min and filter, wash the filter cake with distilled water, dry at 120℃, heat to 800℃ at 5℃ / min, keep for 5h, cool to room temperature and repeat the above operation twice to obtain cerium zirconium oxide Ce.0.3 Zr 0.7 O2 / spherical alumina.

[0061] Weigh 0.68g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.3 Zr 0.7 O2 / spherical alumina 3.08g, rotary evaporate to dryness, dry at 120°C, heat to 800°C at 5°C / min, maintain for 5h, to obtain a molded catalyst.

[0062] In a quartz glass tube reactor (inner diameter of 8mm), 0.10g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (180ml / min) and oxygen (14ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 13vol%, H2 3vol%, and the balance was methane, 180ml / min) and oxygen (14ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0063] Example 4

[0064] Weigh 0.58g of cerium nitrate hexahydrate and 0.58g of zirconium nitrate pentahydrate, dissolve in 100ml of water, add 30g of spherical alumina, slowly add sodium carbonate solution (1mol / L) until the solution pH is 10, continue stirring for 30min and filter, wash the filter cake with distilled water, dry at 100℃, heat to 600℃ at 5℃ / min, keep for 5h, cool to room temperature and repeat the above operation three times to obtain cerium zirconium oxide Ce. 0.5 Zr 0.5 O2 / spherical alumina.

[0065] Weigh 0.68g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.5 Zr 0.5 O2 / spherical alumina 3.05g, rotary evaporate to dryness, dry at 80℃, heat to 480℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0066] In a quartz glass tube reactor (inner diameter of 8mm), 0.09g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (180ml / min) and oxygen (18ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 180ml / min) and oxygen (18ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0067] Example 5

[0068] Weigh 0.54g of cerium nitrate hexahydrate and 4.76g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, keeping for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0069] Weigh 0.28g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.03g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, to obtain a molded catalyst.

[0070] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0071] Example 6

[0072] Weigh 0.32g of cerium nitrate hexahydrate and 2.80g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, keeping for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0073] Weigh 0.48g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.02g, rotary evaporate to dryness, dry at 80℃, heat to 1000℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0074] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0075] Example 7

[0076] Weigh 1.49g of cerium nitrate hexahydrate and 3.45g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, maintaining for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.3 Zr 0.7 O2 / spherical alumina.

[0077] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.3 Zr 0.7 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0078] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0079] Example 8

[0080] Weigh 2.32g of cerium nitrate hexahydrate and 2.30g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, maintaining for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.5 Zr 0.5 O2 / spherical alumina.

[0081] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.5 Zr 0.5 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0082] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0083] Example 9

[0084] Weigh 3.05g of cerium nitrate hexahydrate and 1.29g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, maintaining for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.7 Zr 0.3 O2 / spherical alumina.

[0085] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.7 Zr 0.3 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0086] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0087] Example 10

[0088] Weigh 3.98 g of cerium nitrate hexahydrate, dissolve it in 50 ml of water, add 30 g of spherical alumina, rotary evaporate to dryness, dry at 80°C, heat to 600°C at 5°C / min, maintain for 5 hours, and cool to room temperature to obtain cerium zirconium oxide CeO2 / spherical alumina.

[0089] Weigh 1.01 g of copper nitrate trihydrate, dissolve it in 30 ml of water, add 3.01 g of cerium zirconium oxide CeO2 / spherical alumina, rotary evaporate to dryness, dry at 80°C, heat to 600°C at 5°C / min, maintain for 5 hours, and obtain a shaped catalyst.

[0090] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0091] Embodiment 11

[0092] Weigh 5.51 g of zirconium nitrate pentahydrate, dissolve it in 50 ml of water, add 30 g of spherical alumina, rotary evaporate to dryness, dry at 80°C, heat to 600°C at 5°C / min, maintain for 5 h, and cool to room temperature to obtain cerium zirconium oxide ZrO2 / spherical alumina.

[0093] Weigh 1.01 g of copper nitrate trihydrate, dissolve it in 30 ml of water, add 3.01 g of cerium zirconium oxide ZrO2 / spherical alumina, rotary evaporate to dryness, dry at 80°C, heat to 600°C at 5°C / min, maintain for 5 hours, and obtain a shaped catalyst.

[0094] In a quartz glass tube reactor (inner diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 600°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0095] Example 12

[0096] Weigh 0.54g of cerium nitrate hexahydrate and 4.76g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, keeping for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0097] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0098] In a quartz glass tube reactor (internal diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 400°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0099] Embodiment 13

[0100] Weigh 0.54g of cerium nitrate hexahydrate and 4.76g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, keeping for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0101] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0102] In a quartz glass tube reactor (internal diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 500°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0103] Embodiment 14

[0104] Weigh 0.54g of cerium nitrate hexahydrate and 4.76g of zirconium nitrate pentahydrate, dissolve in 50ml of water, add 30g of spherical alumina, evaporating to dryness, drying at 80℃, heating to 600℃ at 5℃ / min, keeping for 5h, and cooling to room temperature to obtain cerium zirconium oxide Ce. 0.1 Zr 0.9 O2 / spherical alumina.

[0105] Weigh 1.01g of copper nitrate trihydrate, dissolve it in 30ml of water, add cerium zirconium oxide Ce 0.1 Zr 0.9 O2 / spherical alumina 3.01g, rotary evaporate to dryness, dry at 80℃, heat to 600℃ at 5℃ / min, maintain for 5h, and obtain a molded catalyst.

[0106] In a quartz glass tube reactor (internal diameter of 8mm), 0.21g of the above catalyst was loaded, and quartz sand (20-40 mesh) was filled up and down the catalyst. Nitrogen (40ml / min) and oxygen (4ml / min) were introduced, and the temperature was raised to 800°C at a rate of 10°C / min and maintained for 30min. The byproduct reaction gas (which contained CO 15vol%, H2 5vol%, and the balance was methane, 40ml / min) and oxygen (4ml / min) were switched. After 60min of reaction, CO conversion, CH4 conversion and H2 conversion were determined by gas chromatography, and the test results are shown in Table 1.

[0107] Table 1

[0108]

[0109] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A method for recovering methane from waste gas produced by oxidative coupling of methane to produce ethylene, comprising reacting the waste gas produced by oxidative coupling of methane to produce ethylene with an oxygen source in the presence of a formed catalyst; in, The shaped catalyst is loaded with Ce x Zr 1-x O 2 The shaped alumina is used as the carrier, x=0.1-0.7, and CuO is used as the active component; in the shaped catalyst, based on the total weight of the carrier, Ce x Zr 1-x O 2 The mass content of Ce is 5-15%; in the molded catalyst, the mass content of CuO is 5-10% based on the total weight of the molded catalyst; the preparation method of the catalyst comprises first loading Ce on a molded alumina carrier x Zr 1-x O 2 , and then loaded with CuO; the contact temperature is 350-600°C.

2. The method according to claim 1, It is characterized in that x=0.1-0.5。 3. The method according to claim 1, It is characterized in that In the shaped catalyst, based on the total weight of the carrier, Ce x Zr 1- x O 2 The mass content is 5-10%.

4. The method according to claim 1, It is characterized in that The load Ce x Zr 1-x O 2 Using precipitation deposition and / or impregnation methods; and / or The load Ce x Zr 1-x O 2 be a single load or multiple loads; and / or The CuO is loaded by an impregnation method.

5. The method according to claim 4, It is characterized in that The method for preparing the molded catalyst comprises the following steps: S1: Mix the aqueous solution of cerium salt and the aqueous solution of zirconium salt with the formed alumina for impregnation, drying and calcination to obtain Ce-loaded alumina. x Zr 1-x O 2 A shaped alumina carrier; S2: The aqueous solution of copper salt and the loaded Ce x Zr 1-x O 2 The shaped alumina carrier is mixed and impregnated, dried, and calcined to obtain the shaped catalyst.

6. The method according to claim 5, It is characterized in that The method for preparing the molded catalyst comprises the following steps: S1: Mix the aqueous solution of cerium salt and zirconium salt with the shaped alumina carrier, add alkaline solution for precipitation, wash, dry and calcine to obtain the loaded Ce x Zr 1-x O 2 A shaped alumina carrier; S2: The aqueous solution of copper salt and the loaded Ce x Zr 1-x O 2 The shaped alumina carrier is mixed and impregnated, dried, and calcined to obtain the shaped catalyst.

7. The method according to claim 6, It is characterized in that The cerium salt is a water-soluble cerium salt; and / or The zirconium salt is a water-soluble zirconium salt; and / or The copper salt is a water-soluble copper salt; and / or The alkaline solution is selected from aqueous ammonia and / or sodium carbonate solution.

8. The method according to claim 7, It is characterized in that The cerium salt is selected from at least one of cerium nitrate, ammonium cerium nitrate, cerium sulfate and cerium chloride.

9. The method according to claim 8, It is characterized in that The cerium salt is selected from cerium nitrate.

10. The method according to claim 7, It is characterized in that The zirconium salt is selected from at least one of zirconium oxychloride, zirconium chloride, zirconium sulfate and zirconium nitrate.

11. The method according to claim 10, It is characterized in that The zirconium salt is selected from zirconium nitrate.

12. The method according to claim 7, It is characterized in that The copper salt is selected from at least one of copper nitrate, copper chloride and copper sulfate.

13. The method according to claim 12, It is characterized in that The copper salt is selected from copper nitrate.

14. The method according to claim 1, It is characterized in that The exhaust gas includes methane, carbon monoxide and hydrogen, wherein the volume ratio of methane, carbon monoxide and hydrogen is (12-18):(2-5):

1.

15. The method according to claim 14, It is characterized in that The volume ratio of methane, carbon monoxide and hydrogen is (15-17):(2-4):

1.

16. The method according to claim 1, It is characterized in that The total reaction space velocity of the contact is 10-200 L·h -1 ·g -1 .

17. The method according to claim 16, It is characterized in that The total reaction space velocity of the contact is 13-150 L·h -1 ·g -1 .