Thermoplastic polyimide resin and preparation method thereof

By adjusting the structure and reaction conditions of the polyimide resin, the melting index and the extrusion temperature are improved, and the problem of difficult viscosity control and high extrusion temperature in the prior art is solved, and better processing performance is achieved. Mechanical properties.

CN114181391BActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202010962688.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-12-03
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

The viscosity of existing thermoplastic polyimide resins is difficult to control, with low melting index and high extrusion temperature, which limits its processing and application range.

Method used

By adjusting the structure of the polyimide resin, introducing isomer structural units of phthalidan and specific capping agents, the viscosity and reaction conditions of the polyamic acid solution are controlled, the melt index is increased, and the extrusion temperature is reduced.

Benefits of technology

The melt index of the polyimide resin is improved, the extrusion temperature is reduced, the reaction stability and processing performance are enhanced, while the mechanical properties of the resin are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114181391B_ABST
    Figure CN114181391B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of thermoplastic polyimide materials, and discloses a thermoplastic polyimide resin and a preparation method thereof. The polyimide resin has a structure shown in formula (1): #imgabs0# wherein Ar is a residue of a dibasic primary amine monomer; Ar is selected from one or more of the following groups: #imgabs1# x is 0.45-0.9; EG is a capping agent residue, selected from one of the following groups: #imgabs2# The viscosity of the thermoplastic polyimide resin at 30°C is 0.35-0.55 dL / g. The polyimide resin has the characteristics of high melt index and low extrusion temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermoplastic polyimide materials, and in particular to a thermoplastic polyimide resin and a preparation method thereof. Background Art

[0002] Polyimide is a resin material with excellent comprehensive performance, with good thermal stability, excellent mechanical properties, good dimensional stability, excellent chemical stability, high breakdown voltage, low dielectric constant, high flame retardancy, low expansion coefficient and other advantages, and is widely used in high-tech fields such as electronic appliances, aerospace, automobiles, chemical machinery. On the other hand, due to the rigid molecular chain of polyimide and the extremely strong interaction force between molecules, it is difficult for polymers to melt, which limits the processing and application range of polyimide, so a lot of methods have been developed to improve the thermoplastic processability of polyimide. For example, flexible groups are introduced into the main chain molecule, such as -O-, -S-, -CH2-, etc., to reduce the rigidity of the molecular chain, reduce the intermolecular force, but the glass transition temperature of polyimide will be caused to decline. CN102634021A discloses a thermoplastic polyimide resin and a preparation method thereof. The thermoplastic polyimide resin is a polyimide resin having good thermal stability and excellent thermoplastic processability obtained by reacting a mixed dianhydride composed of 1,2,3,4-benzene tetracarboxylic dianhydride and other commonly used tetracarboxylic dianhydrides, diamine and phthalic anhydride or aniline, so that the mixed dianhydride and diamine are polymerized, and phthalic anhydride or aniline is used as a capping agent to control the molecular weight. The inherent logarithmic viscosity can reach 0.22-0.90 dL / g, and the glass transition temperature is 220-420°C. Therefore, the polyimide resin can be widely used in the preparation of high-temperature resistant engineering plastics, films, adhesives and other materials.

[0003] However, the thermoplastic polyimide resin provided by the above patent has the disadvantages of low melt index and high extrusion temperature required for extrusion injection molding. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of the prior art that the viscosity of polyimide resin is difficult to control, the melt index is low and the extrusion temperature is high, and to provide a polyimide resin and a preparation method thereof. The polyimide resin has the characteristics of high melt index and low extrusion temperature.

[0005] In order to achieve the above object, the first aspect of the present invention provides a thermoplastic polyimide resin, characterized in that the polyimide resin has a structure shown in formula (1):

[0006]

[0007] Wherein, Ar is the residue of a diamine monomer; Ar is selected from one or more of the following groups:

[0008]

[0009] x is 0.45-0.9;

[0010] EG is a capping agent residue selected from one of the following groups:

[0011]

[0012] The thermoplastic polyimide resin has a viscosity of 0.35-0.55 dL / g at 30°C.

[0013] The second aspect of the present invention provides a method for preparing the above-mentioned polyimide resin, characterized in that the method comprises the following steps:

[0014] (1) Preparation of polyimide solution: In the presence of a solvent and an inert atmosphere, a diamine monomer and a dianhydride monomer are subjected to a first reaction to obtain a polyamic acid solution; when the viscosity of the polyamic acid solution reaches 0.35-0.55 dL / g, a capping agent is added, a second reaction is carried out, and then an imidization agent is added to carry out a third reaction to obtain a polyimide solution;

[0015] (2) Preparation of polyimide resin: The polyimide solution obtained in step (1) is diluted, precipitated in a precipitant, washed, and dried to obtain the thermoplastic polyimide resin.

[0016] The third aspect of the present invention provides a polyimide resin prepared by the above method.

[0017] Through the above technical scheme, the polyimide resin and the preparation method thereof provided by the present invention achieve the following beneficial effects:

[0018] (1) The polyimide resin provided by the present invention can improve the melt index and reduce the extrusion temperature without affecting the mechanical properties of the resin;

[0019] (2) In the present invention, the reaction stability is greatly improved by changing the feeding method, especially adding the end-capping agent after the viscosity of the polyimide reaches a certain value, instead of adding all the raw materials into the reaction container at one time.

[0020] (3) The reaction temperature after adding the imidization agent is controlled at 60-90° C., and the reaction time is controlled at 1-3 hours. Under the condition that the polyamic acid is not degraded, the imidization reaction time is greatly shortened and the reaction stability is improved.

[0021] (4) The polyimide solution is diluted to a certain concentration and then precipitated in a precipitant, which can effectively control the particle size of the precipitated polyimide powder. At the same time, after drying, it is further crushed by a pulverizer to ensure the particle size of the polyimide powder before processing. DETAILED DESCRIPTION

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0023] The first aspect of the present invention provides a thermoplastic polyimide resin, characterized in that the polyimide resin has a structure shown in formula (1):

[0024]

[0025] Wherein, Ar is the residue of a diamine monomer; Ar is selected from one or more of the following groups:

[0026]

[0027] x is 0.45-0.9;

[0028] EG is a capping agent residue selected from one of the following groups:

[0029]

[0030] The thermoplastic polyimide resin has a viscosity of 0.35-0.55 dL / g at 30°C.

[0031] In the present invention, the polyimide resin having the above-mentioned specific structure has the performance characteristics of high melt index and low extrusion temperature due to the isomeric structural units of phthalic anhydride in the polyimide resin, which causes the molecular chain to be twisted and introduces a specific end-capping agent structure.

[0032] In the present invention, x represents the weight percentage of the structural unit in the polyimide resin. x can be measured by FI-IR or calculated based on the feed and residual amount.

[0033] According to the present invention, Ar is selected from one or more of the following groups:

[0034]

[0035] According to the present invention, the capping agent is selected from at least one of the structures shown below:

[0036]

[0037] According to the present invention, x is 0.5-0.8.

[0038] According to the present invention, the melt index of the thermoplastic polyimide resin at 360°C and a load of 12.5 kg is 0.5-5 g / 10 min; and the extrusion temperature of the thermoplastic polyimide resin is 300-360°C.

[0039] In the present invention, the viscosity of the polyimide resin is measured by the national standard GB / T 10247-2008 method, and the melt index is measured by the national standard GB / T 3682.1-2018 method.

[0040] In one embodiment of the present invention, the polyimide has a structure shown in formula (2):

[0041]

[0042] Formula (2);

[0043] wherein x is 0.5-0.8, and Ar is as described above.

[0044] A second aspect of the present invention provides a method for preparing the above-mentioned polyimide resin, characterized in that the method comprises the following steps:

[0045] (1) Preparation of polyimide solution: In the presence of a solvent and an inert atmosphere, a diamine monomer and a dianhydride monomer are subjected to a first reaction to obtain a polyamic acid solution; when the viscosity of the polyamic acid solution reaches 0.3-0.6 dL / g, a capping agent is added, a second reaction is carried out, and then an imidization agent is added to carry out a third reaction to obtain a polyimide solution;

[0046] (2) Preparation of polyimide resin: The polyimide solution obtained in step (1) is diluted, precipitated in a precipitant, washed, and dried to obtain the thermoplastic polyimide resin.

[0047] In the present invention, by changing the feeding method, especially after the viscosity of the polyamide acid reaches a certain value, especially when the viscosity of the polyamide acid solution reaches 0.3-0.6dL / g, the end-capping agent is added instead of adding all the raw materials into the reaction container at one time, the reaction stability is greatly improved.

[0048] In the present invention, the viscosity of the polyamic acid solution is measured using the national standard GB / T10247-2008.

[0049] According to the present invention, the conditions of the first reaction include: reaction temperature 0-35° C., reaction time 8-14 h.

[0050] According to the present invention, the conditions of the second reaction include: reaction temperature 0-35° C., reaction time 1-2 h.

[0051] According to the present invention, the conditions of the third reaction include: reaction temperature 60-90° C., reaction time 1-3 h.

[0052] In the present invention, the inventors have found that by controlling the reaction temperature after adding the imidization agent to 60-90°C and the reaction time to 1-3 hours, the imidization reaction time is greatly shortened and the reaction stability is improved while controlling the polyamic acid not to degrade.

[0053] According to the present invention, preferably, when the viscosity of the polyamic acid solution reaches 0.35-0.55 dL / g, preferably 0.35-0.45 dL / g, when the end-capping agent is added, the polyimide resin obtained thereby has the performance characteristics of high melt index and low extrusion temperature.

[0054] According to the present invention, the end-capping agent is selected from at least one of phthalic anhydride, aniline, p-toluidine and acetic anhydride.

[0055] According to the present invention, the molar ratio of the dianhydride to the end-capping agent is 1:0.02-0.2, preferably 1:0.02-0.1, and more preferably 1:0.05-0.2.

[0056] According to the present invention, the solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

[0057] According to the present invention, the solid content of the polyimide solution is 15-35wt%, preferably 20-30wt%.

[0058] According to the present invention, the molar ratio of the dianhydride to the diamine is 1:0.95-0.995, preferably 1:0.95-0.985, and more preferably 1:0.955-0.985.

[0059] According to the present invention, the diamine monomer is selected from one or more of the following monomers:

[0060]

[0061]

[0062] According to the present invention, the diamine monomer is selected from one or more of the following monomers:

[0063]

[0064] In the present invention, the diamine monomer may specifically be 4,4′-bis(3-aminophenoxy)diphenyl sulfone.

[0065] According to the present invention, the imidization agent is acetic anhydride and a tertiary amine compound, and the volume ratio of the acetic anhydride to the tertiary amine compound is 1:0.5-1, preferably 1:0.5-0.8.

[0066] According to the present invention, the tertiary amine compound is selected from triethylamine and / or pyridine.

[0067] According to the present invention, the molar ratio of the diamine to the acetic anhydride is 1:2.5-3, preferably 1:2.5-2.8.

[0068] According to the present invention, in step (2), the polyimide solution is diluted to a solid content of 5-10 wt %.

[0069] According to the present invention, the method further comprises crushing, drying, extruding and pelletizing the thermoplastic polyimide resin to obtain polyimide resin pellets.

[0070] According to the present invention, the drying conditions include: a drying temperature of 150-200° C. and a drying time of 1-6 hours.

[0071] According to the present invention, the extrusion conditions include: an extrusion temperature of 300-360° C. and a rotation speed of 10-50 rpm.

[0072] The present invention will be described in detail below by way of examples. In the following examples,

[0073] The viscosity of the polyamic acid solution was measured using the national standard GB / T 10247-2008 method;

[0074] The viscosity of polyimide powder was measured using the national standard GB / T 10247-2008 method;

[0075] The melt index of polyimide powder is measured using the national standard GB / T 3682.1-2018 method;

[0076] The mechanical properties of polyimide specimens were measured using GB / T 1040-2006;

[0077] 1,2,3,4-benzenetetracarboxylic dianhydride is synthesized in the laboratory. The specific synthesis method is as follows (see the 2018 Shanghai University master's thesis, Preparation and Performance Study of Highly Soluble Phenylethyne-Terminated Thermosetting Polyimide Resin, author Li Hanyuan):

[0078] Add 100g cyclohexene, 200mL carbon tetrachloride and 10mL anhydrous ethanol into a 1000mL three-necked flask, then place it in an ice-water bath at 0°C, dissolve 160g liquid bromine in 100mL carbon tetrachloride and add dropwise into the flask, and control the dripping to be completed within 10 hours. After the reaction is completed, evaporate the excess carbon tetrachloride and cyclohexene, and then obtain 188g 1,2'-dibromocyclohexane by vacuum distillation.

[0079] Add 200g of sodium hydroxide to 400mL of ethylene glycol, heat to 210℃, evaporate about 80mL of water, then start to dropwise add 188g of 1,2'-dibromocyclohexane and heat to 230℃. After the dropwise addition is complete, continue to introduce nitrogen and continue to collect fractions for 1h. Use a separatory funnel to separate the water layer of the product and dry it with anhydrous calcium chloride to obtain 72g of cyclohexadiene.

[0080] Take 72g of cyclohexadiene, add 80g of maleic anhydride, start mechanical stirring, and react in a 45°C water bath. Because it is an exothermic reaction, put it in a cold water bath to cool it down as soon as the reaction starts. After the reaction is cooled, stir for 12h, filter to obtain the crude product, concentrate the filtrate to collect the crude product, and wash the crude product with water to obtain 124g of bicyclo[2,2,2]-5-octene-2,3-dianhydride.

[0081] Add 80 mL of 60% concentrated nitric acid into a 500 mL flask, then add 60 mg of ammonium metavanadate and 20 mg of ammonium molybdate, control the reaction temperature at 60 ° C, add 20 g of bicyclo [2,2,2] -5-octene-2,3-dianhydride in batches within 4 hours, and add 30 mL of fuming nitric acid dropwise. After the reaction is completed, cool and filter, and recrystallize from water to obtain 25 g of cis-1,2,3,4-cyclohexanetetraacid.

[0082] Add 10 g of cis-1,2,3,4-cyclohexanetetracarboxylic acid to 120 mL of glacial acetic acid, heat to reflux, and dropwise add 95 mL of glacial acetic acid containing 16 g of bromine. After the dropwise addition, continue to reflux for 3 hours. After cooling, recrystallize with water, filter and dry to obtain 5 g of 1,2,3,4-benzenetetracarboxylic acid.

[0083] Finally, the obtained 1,2,3,4-benzene tetracarboxylic acid is recrystallized in acetic anhydride, and the filter cake is dried and placed in a sublimation tube for sublimation to obtain 1,2,3,4-benzene tetracarboxylic dianhydride.

[0084] 4,4′-Bis(3-aminophenoxy)diphenyl sulfone was purchased from Nanjing Yuezi Chemical Co., Ltd.;

[0085] 1,2,4,5-Pyromellitic dianhydride was purchased from Sinopharm Group Pharmaceutical Co., Ltd.;

[0086] Other raw materials used in the examples and comparative examples are all commercially available.

[0087] Example 1

[0088] The preparation method of thermoplastic polyimide resin pellets is as follows:

[0089] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8735 g, 150.0 mmol) was added to a reaction bottle, 415 mL of N,N-dimethylacetamide was added, and the mixture was stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (6.4454 g, 29.55 mmol) and 1,2,4,5-pyromellitic acid dianhydride (25.7818 g; 118.2 mmol) were added, and the mixture was stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.45 dL / g, phthalic anhydride (1.3330 g, 9 mmol) was added, and the mixture was stirred at room temperature for 1 hour. Then, 36 mL of acetic anhydride and 18 mL of pyridine as a chemical imidization reagent were added, and the mixture was reacted at 80° C. for 2 hours to obtain a polyimide solution.

[0090] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 10%, and then precipitated in a precipitant. The precipitate was collected, fully washed, dried, and then crushed in a pulverizer for 3 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.40 dL / g and a melt index of 3 g / 10 min.

[0091] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170°C for 4 hours, and then processed using a high-temperature desktop extruder at 340°C with a screw speed of 20 rpm, and extruded and pelletized to obtain pellets.

[0092] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0093]

[0094] Ar is:

[0095]

[0096] Example 2

[0097] The preparation method of thermoplastic polyimide resin pellets is as follows:

[0098] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8769 g, 150.0 mmol) was added to a reaction bottle, and 415 mL of N,N-dimethylacetamide was added and stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (12.8255 g, 58.8 mmol) and 1,2,4,5-pyromellitic acid dianhydride (19.2380 g, 88.2 mmol) were added and stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.37 dL / g, phthalic anhydride (1.7773 g, 12 mmol) was added and stirred at room temperature for 1 hour. Then, 36 mL of chemical imidization reagent acetic anhydride and 18 mL of pyridine were added and reacted at 80° C. for 1.5 hours to obtain a polyimide solution.

[0099] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 10%, and then precipitated in a precipitant. The precipitate was collected, fully washed, dried, and then crushed in a pulverizer for 3 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.36 dL / g and a melt index of 1.8 g / 10 min.

[0100] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170°C for 4 hours, and then processed using a high-temperature desktop extruder at 320°C with a screw speed of 20 rpm, and extruded and pelletized to obtain pellets.

[0101] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0102]

[0103] Ar is:

[0104]

[0105] Example 3

[0106] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8735 g, 150.0 mmol) was added to a reaction bottle, and 415 mL of N,N-dimethylacetamide was added and stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (3.2220 g, 14.78 mmol) and 1,2,4,5-pyromellitic acid dianhydride (29.0050 g, 118.2 mmol) were added and stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.53 dL / g, phthalic anhydride (1.3330 g, 9 mmol) was added and stirred at room temperature for 2 hours. Then, 36 mL of acetic anhydride and 18 mL of pyridine as a chemical imidization reagent were added and reacted at 90° C. for 1 hour to obtain a polyimide solution.

[0107] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 8%, and then precipitated in a precipitant. The precipitate was collected, washed thoroughly, dried, and then crushed in a pulverizer for 5 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.49 dL / g and a melt index of 1 g / 10 min.

[0108] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170° C. for 4 hours, and then processed using a high-temperature desktop extruder at 350° C. with a screw speed of 10 rpm, and extruded and pelletized to obtain pellets.

[0109] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0110]

[0111] Ar is:

[0112]

[0113] Example 4

[0114] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (57.5125 g, 132.98 mmol) was added to a reaction bottle, and 415 mL of N,N-dimethylacetamide was added and stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (3.6361 g, 16.67 mmol) and 1,2,4,5-pyromellitic acid dianhydride (29.0819 g, 133.33 mmol) were added and stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.5 dL / g, aniline (0.8383 g, 9 mmol) was added and stirred at room temperature for 2 hours. Then, 36 mL of chemical imidization reagent acetic anhydride and 18 mL of pyridine were added and reacted at 90° C. for 1 hour to obtain a polyimide solution.

[0115] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 8 wt %, and then precipitated in a precipitant. The precipitate was collected, washed thoroughly, dried, and then crushed in a pulverizer for 5 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.44 dL / g and a melt index of 0.6 g / 10 min.

[0116] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170° C. for 4 hours, and then processed using a high-temperature desktop extruder at 350° C. with a screw speed of 10 rpm, and extruded and pelletized to obtain pellets.

[0117] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0118]

[0119] Ar is:

[0120]

[0121] Example 5

[0122] The preparation method of thermoplastic polyimide resin pellets is as follows:

[0123] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8735 g, 150.0 mmol) was added to a reaction bottle, and 415 mL of N,N-dimethylacetamide was added and stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (9.6682 g, 44.33 mmol) and 1,2,4,5-pyromellitic acid dianhydride (22.5591 g; 103.43 mmol) were added and stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.45 dL / g, phthalic anhydride (1.3330 g, 9 mmol) was added and stirred at room temperature for 1 hour. Then, 36 mL of acetic anhydride and 18 mL of pyridine as a chemical imidization reagent were added and reacted at 80° C. for 2 hours to obtain a polyimide solution.

[0124] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 10%, and then precipitated in a precipitant. The precipitate was collected, fully washed, dried, and then crushed in a pulverizer for 3 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.41 dL / g and a melt index of 2.7 g / 10 min.

[0125] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170°C for 4 hours, and then processed using a high-temperature desktop extruder at 340°C with a screw speed of 20 rpm, and extruded and pelletized to obtain pellets.

[0126] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0127]

[0128] Ar is:

[0129]

[0130] Example 6

[0131] The preparation method of thermoplastic polyimide resin pellets is as follows:

[0132] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8735 g, 150.0 mmol) was added to a reaction bottle, 415 mL of N,N-dimethylacetamide was added, and the mixture was stirred to completely dissolve. Then, 1,2,3,4-benzenetetracarboxylic acid dianhydride (16.1137 g, 73.88 mmol) and 1,2,4,5-pyromellitic acid dianhydride (16.1139 g, 73.88 mmol) were added, and the mixture was stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.46 dL / g, phthalic anhydride (1.3330 g, 9 mmol) was added, and the mixture was stirred at room temperature for 1 hour. Then, 36 mL of acetic anhydride and 18 mL of pyridine as a chemical imidization reagent were added, and the mixture was reacted at 80° C. for 2 hours to obtain a polyimide solution.

[0133] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 10%, and then precipitated in a precipitant. The precipitate was collected, fully washed, dried, and then crushed in a pulverizer for 3 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.43 dL / g and a melt index of 2.0 g / 10 min.

[0134] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170° C. for 4 hours, and then processed using a high-temperature desktop extruder at 320° C. with a screw speed of 30 rpm, and extruded and pelletized to obtain pellets.

[0135] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0136]

[0137] Ar is:

[0138]

[0139] Comparative Example 1

[0140] The preparation method of thermoplastic polyimide resin pellets is as follows:

[0141] (1) Under nitrogen protection, 4,4′-bis(3-aminophenoxy)diphenyl sulfone (64.8735 g, 150.0 mmol) was added to a reaction bottle, 415 mL of N,N-dimethylacetamide was added, and the mixture was stirred to completely dissolve. Then, 1,2,4,5-pyromellitic dianhydride (32.2272 g, 147.75 mmol) was added, and the mixture was stirred at room temperature for 10 hours to obtain a polyamic acid solution. After the viscosity of the polyamic acid reached 0.50 dL / g, phthalic anhydride (1.3330 g, 9 mmol) was added, and the mixture was stirred at room temperature for 1 hour. Then, 36 mL of acetic anhydride and 18 mL of pyridine as a chemical imidization reagent were added, and the mixture was reacted at 80° C. for 2 hours to obtain a polyimide solution.

[0142] (2) Preparation of polyimide powder: The polyimide solution was diluted to a solid content of 10%, and then precipitated in a precipitant. The precipitate was collected, fully washed, dried, and then crushed in a pulverizer for 3 minutes to obtain a thermoplastic polyimide powder having a viscosity of 0.44 dL / g and a melt index of 0.4 g / 10 min.

[0143] (3) Preparation of polyimide pellets: The polyimide powder was dried in a conventional oven at 170° C. for 4 hours, and then processed using a high-temperature desktop extruder at 370° C. with a screw speed of 20 rpm, and extruded and pelletized to obtain pellets.

[0144] According to the feed amount and the residual amount, the structure of the polyimide is shown in the following formula:

[0145]

[0146] Ar is:

[0147]

[0148] Table 1

[0149] serial number x PAA viscosity (dl / g) PI viscosity (dl / g) Melt index (g / 10min) Extrusion temperature(℃) Example 1 0.80 0.45 0.40 3.0 340 Example 2 0.60 0.37 0.36 1.8 320 Example 3 0.89 0.53 0.49 1.0 350 Example 4 0.89 0.50 0.44 0.6 360 Example 5 0.70 0.45 0.41 2.7 340 Example 6 0.5 0.46 0.43 2.0 320 Comparative Example 1 0.50 0.44 0.4 370

[0150] It can be seen from the results in Table 1 that Examples 1-6 in which the polyimide is prepared by adding 1,2,3,4-phthalic anhydride monomers in the present invention have a higher melt index (0.6-3.0 g / 10 min) under the same conditions (360° C. / 12.5 kg), and the temperature of the pellets extruded by the extruder is also reduced from the initial 370° C. to 360-320° C., which has a significant effect of reducing the extrusion temperature and greatly improves the thermal stability of the resin processing.

[0151] Test Case

[0152] The polyimide pellets of Examples 1-6 and Comparative Example 1 were injection molded and formed at 340° C. and 210 bar to obtain polyimide samples. The mechanical properties of the obtained polyimide samples were tested. The test results are shown in Table 2.

[0153] Table 2

[0154] serial number Tensile strength(MPa) Tensile modulus(GPa) Elongation at break (%) Example 1 110.6 3.0 5.0 Example 2 112.9 2.9 4.2 Example 3 120.2 2.9 4.0 Example 4 116.4 2.9 4.1 Example 5 115.0 2.9 4.4 Example 6 103.2 2.9 4.7 Comparative Example 1 107.7 2.9 4.2

[0155] It can be seen from Table 2 that the samples obtained by injection molding the polyimide pellets provided by the present invention have comparable tensile strength, tensile modulus and elongation at break, indicating that the thermoplastic polyimide resin provided by the present invention not only has a high melt index and a low extrusion temperature, but also does not affect the mechanical properties of the resin.

[0156] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A thermoplastic polyimide resin, characterized in that: The polyimide resin has a structure shown in formula (1): Wherein, Ar is the residue of a diamine monomer; Ar is selected from one or more of the following groups: x is 0.5-0.8; EG is a capping agent residue selected from one of the following groups: The viscosity of the thermoplastic polyimide resin at 30° C. is 0.35-0.55 dL / g; The melt index of the thermoplastic polyimide resin at 360° C. and a load of 12.5 kg is 1.8-5 g / 10 min; the extrusion temperature of the thermoplastic polyimide resin is 300-340° C.; The preparation method of the thermoplastic polyimide resin comprises: (1) Preparation of polyimide solution: In the presence of a solvent and an inert atmosphere, a diamine monomer and a dianhydride monomer are reacted in a first step to obtain a polyamic acid solution; when the viscosity of the polyamic acid solution reaches 0.35-0.46 dL / g, a capping agent is added, a second step reaction is carried out, and then an imidization agent is added to carry out a third step reaction to obtain a polyimide solution; (2) Preparation of polyimide resin: The polyimide solution obtained in step (1) is diluted, precipitated in a precipitant, washed, and dried to obtain the thermoplastic polyimide resin; The diamine monomer is selected from one or more of the following monomers:

2. The thermoplastic polyimide resin according to claim 1, wherein Ar is selected from one or more of the following groups:

3. The thermoplastic polyimide resin according to claim 1 or 2, wherein The capping agent is selected from at least one of the structures shown below:

4. A method for preparing the thermoplastic polyimide resin according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) Preparation of polyimide solution: In the presence of a solvent and an inert atmosphere, a diamine monomer and a dianhydride monomer are reacted in a first step to obtain a polyamic acid solution; when the viscosity of the polyamic acid solution reaches 0.35-0.46 dL / g, a capping agent is added, a second step reaction is carried out, and then an imidization agent is added to carry out a third step reaction to obtain a polyimide solution; (2) Preparation of polyimide resin: The polyimide solution obtained in step (1) is diluted, precipitated in a precipitant, washed, and dried to obtain the thermoplastic polyimide resin; The diamine monomer is selected from one or more of the following monomers:

5. The method according to claim 4, wherein: The conditions of the first step reaction include: reaction temperature of 0-35° C., and reaction time of 8-14 h.

6. The method according to claim 4 or 5, wherein: The conditions of the second step reaction include: reaction temperature 0-35°C, reaction time 1-2h.

7. The method according to claim 4 or 5, wherein: The conditions of the third step reaction include: reaction temperature 60-90° C., reaction time 1-3 h.

8. The method according to claim 4 or 5, wherein: The end-capping agent is selected from at least one of phthalic anhydride, aniline, p-toluidine and acetic anhydride.

9. The method according to claim 4 or 5, wherein: The molar ratio of the dianhydride to the end-capping agent is 1:0.02-0.

2.

10. The method according to claim 9, wherein: The molar ratio of the dianhydride to the end-capping agent is 1:0.02-0.

1.

11. The method according to claim 4 or 5, wherein: The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

12. The method according to claim 4 or 5, wherein: The solid content of the polyimide solution is 15-35 wt %.

13. The method according to claim 12, wherein: The solid content of the polyimide solution is 20-30 wt %.

14. The method according to claim 4 or 5, wherein: The molar ratio of the dianhydride to the diamine is 1:0.95-0.

995.

15. The method according to claim 14, wherein: The molar ratio of the dianhydride to the diamine is 1:0.95-0.

985.

16. The method according to claim 4 or 5, wherein: The dianhydride monomer is selected from 1,2,3,4-benzenetetracarboxylic dianhydride and / or 1,2,4,5-pyromellitic dianhydride.

17. The method according to claim 4 or 5, wherein: The diamine monomer is selected from one or more of the following monomers:

18. The method according to claim 4 or 5, wherein: The imidization reagent is acetic anhydride and a tertiary amine compound, and the volume ratio of the acetic anhydride to the tertiary amine compound is 1:0.5-1.

19. The method according to claim 18, wherein: The volume ratio of the acetic anhydride to the tertiary amine compound is 1:0.5-0.

8.

20. The method according to claim 18, wherein: The tertiary amine compound is selected from triethylamine and / or pyridine.

21. The method according to claim 18, wherein: The molar ratio of the diamine to the acetic anhydride is 1:2.5-3.

22. The method according to claim 21, wherein: The molar ratio of the diamine to the acetic anhydride is 1:2.5-2.

8.

23. The method according to claim 4 or 5, wherein: In step (2), the polyimide solution is diluted to a solid content of 5-10 wt %.

24. The method according to claim 4 or 5, further comprising crushing, drying, extruding and pelletizing the thermoplastic polyimide resin to obtain polyimide resin pellets.

25. The method according to claim 24, wherein: The drying conditions include: a drying temperature of 150-200° C. and a drying time of 1-6 hours.

26. The method according to claim 24, wherein: The extrusion conditions include: extrusion temperature of 300-360° C. and rotation speed of 10-50 rpm.

Citation Information

Cited By

  • Thermoplastic polyimide resin containing biphenyl structure and preparation method thereof

    CN120248324A