Preparation and application of gelatin fiber separator for lithium metal battery

The gelatin fiber separator prepared by electrospinning technology solves the problem of lithium ion deposition control in lithium metal batteries, inhibits the growth of lithium dendrites, improves the cycle life and capacity retention ability of the battery, and meets the high energy density and high power density need.

CN114188659BActive Publication Date: 2024-11-01ZHEJIANG UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111483794.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-07
Publication Date
2024-11-01
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

Lithium ion deposition in lithium metal batteries is difficult to control, resulting in lithium dendrites growth, resulting in battery capacity loss and safety problems. In addition, traditional diaphragms are unstable, making it difficult to meet the needs of high energy density and high power density.

Method used

The gelatin fiber membrane was prepared by electrospinning technology, and the film was formed by dissolving gelatin in anhydrous 2,2,2-trifluoroethanol, and the film material with nanostructures was formed by drying and tableting, which was used to replace the traditional Separator, regulates the deposition of lithium ions and SEI membrane structure.

Benefits of technology

It realizes uniform deposition of lithium ions, inhibits the growth of lithium dendrites, improves the cycle life and Coulomb efficiency of the battery, enhances the capacity retention ability of the battery, and is simple and efficient in the process and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114188659B_ABST
    Figure CN114188659B_ABST
Patent Text Reader

Abstract

The present invention discloses the preparation and application of a gelatin fiber diaphragm for lithium metal batteries. The method for preparing the gelatin fiber diaphragm for lithium metal batteries comprises the following steps: (1) dissolving gelatin in an organic solvent and stirring for 8 to 12 hours to obtain a gelatin spinning solution; the organic solvent is anhydrous 2,2,2-trifluoroethanol; the mass ratio of gelatin to anhydrous 2,2,2-trifluoroethanol is 0.8-1.2:10; (2) using electrostatic spinning technology, spinning the solution prepared in step (1) at a constant voltage to form a film, and collecting the sprayed gelatin film; (3) taking out the gelatin film obtained in step (2), drying and pressing the film to obtain a gelatin fiber diaphragm. The method of the present invention is simple and efficient, low in cost, and can be prepared on a large scale; when the prepared gelatin fiber diaphragm is used for lithium metal batteries, it has higher ionic conductivity, better battery cycle life, high coulomb efficiency and charge and discharge capacity compared with traditional polymer diaphragms.
Need to check novelty before this filing date? Find Prior Art

Description

(I) Technical field

[0001] The invention belongs to the field of lithium batteries and relates to a preparation method of a gelatin (GE) fiber diaphragm for a lithium metal battery and an application of the diaphragm in a lithium metal battery. (II) Background technology

[0002] With the rapid expansion of electronic devices and electric vehicle markets, the demand for high energy density and high power density lithium-ion batteries is also increasing. However, the theoretical capacity is only 372mAh g -1 The traditional graphite anode can no longer meet the needs of modern development. In order to replace the graphite anode, lithium metal anode is a promising anode material with a theoretical capacity of up to 3860mAh g -1 , which is ten times the capacity of graphite. In addition, lithium metal has excellent properties such as the lowest standard electrode potential (-3.04V relative to the standard hydrogen electrode) and good conductivity.

[0003] However, there are still many problems with lithium metal negative electrodes. Due to the difficulty in controlling the lithium ion deposition process, the high reactivity of lithium metal will produce a fragile and unstable solid electrolyte film with the electrolyte, leading to the growth of lithium dendrites, which will lead to the loss of battery capacity and the expansion of the battery volume. The continuous growth of lithium dendrites during the cycle will eventually pierce the diaphragm, causing safety problems such as battery short circuit. Therefore, the large-scale application of lithium metal batteries still faces severe challenges. It is crucial to regulate and improve the composition and structure of the SEI film and inhibit the growth of dendrites to extend the cycle life of lithium metal batteries. The present invention selects a gelatin fiber diaphragm, and prepares the natural biomass material gelatin into a nanostructured thin film material through electrospinning technology to replace the diaphragm of the lithium battery. In addition, the effective ingredients in the gelatin can regulate the deposition of lithium, generate a stable SEI film, and achieve rapid transfer and uniform deposition of lithium ions. (III) Summary of the invention

[0004] The first technical problem to be solved by the present invention is to provide a method for preparing a gelatin fiber separator for a lithium metal battery by electrospinning.

[0005] The second technical problem to be solved by the present invention is to provide application of the prepared gelatin fiber separator in lithium metal batteries.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a gelatin fiber separator for a lithium metal battery, comprising the following steps:

[0008] (1) dissolving gelatin in an organic solvent and stirring for 8 to 12 hours to obtain a gelatin spinning solution; the organic solvent is anhydrous 2,2,2-trifluoroethanol; the mass ratio of gelatin to anhydrous 2,2,2-trifluoroethanol is 0.8-1.2:10;

[0009] (2) using electrospinning technology, spinning the solution prepared in step (1) at a constant voltage to form a film, and collecting the sprayed gelatin film, wherein the spinning voltage range is 8 to 12 kV, the injection speed is 0.2 to 0.6 mm / min, the distance between the needle and the receiving device is 12 to 16 cm, and the spinning time is 0.5 to 1 h;

[0010] (3) The gelatin film obtained in step (2) is taken out, and a gelatin fiber membrane is obtained by drying and pressing.

[0011] In step (1) of the present invention, the concentration of the film-forming solution directly affects the film-forming effect of the gelatin fibers in step (2). It is generally best to allow the solution to be spun smoothly and the collected fibers to be smooth and uniform in diameter. In a specific embodiment of the present invention, the optimal mass ratio of gelatin to anhydrous 2,2,2-trifluoroethanol is 1:10.

[0012] In step (2) of the present invention, the best spinning conditions are when the voltage is 12 kV, the injection speed is 0.4 mm / min, the distance between the needle and the receiving device is 15 cm, and the spinning time is 1 hour.

[0013] In step (3) of the present invention, the drying condition is preferably: vacuum drying at 50-70°C, generally drying until the film is slightly rolled up. The tablet is formed by one-step pressing using a tablet press, preferably with a controlled pressure of 8-10 MPa.

[0014] In a second aspect, the present invention provides the use of the gelatin fiber membrane prepared by electrospinning as a membrane in a lithium metal battery.

[0015] In the present invention, the lithium metal battery can be prepared according to conventional methods. The electrolyte can be selected from DOL / DME (1:1w / w) with 1MLiTFSI+1wt%LiNO3 as an additive and EC / DEC / EMC (1:1:1v / v / v) with 1MLiPF6+1wt%LiNO3 as an additive. The electrolyte used in the present invention is DOL / DME (1:1w / w) with 1M LiTFSI+1wt%LiNO3 as an additive.

[0016] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in:

[0017] (1) The gelatin fiber membrane prepared by electrospinning in the present invention is simple and efficient. Biomass gelatin is natural and pollution-free, and has low cost. The gelatin fiber membrane can be prepared by simple dissolution, electrospinning, drying and tableting, and can be prepared on a large scale.

[0018] (2) The gelatin fiber membrane prepared by the present invention has excellent electrolyte wettability through electrospinning technology.

[0019] (3) When the gelatin fiber diaphragm prepared by the present invention is used in a lithium metal battery, the diaphragm can induce uniform deposition of lithium ions and effectively inhibit the growth of lithium dendrites during the charge and discharge process. Compared with traditional polymer diaphragms, the diaphragm has higher ionic conductivity, better battery cycle life, high coulombic efficiency and charge and discharge capacity. (IV) Description of the drawings

[0020] Figure 1a , 1b 1a and 1c are SEM plan views of the gelatin membranes prepared in Example 1, Example 2, and Example 3, respectively.

[0021] Figure 2 are the contact angles of the commercial polypropylene separator (a) and the gelatin separators prepared in Example 1 (b), Example 2 (c) and Example 3 (d).

[0022] Figure 3 is the ionic conductivity of the commercial polypropylene separator and the gelatin separators prepared in Examples 1, 2 and 3.

[0023] Figure 4 It is a comparison chart of the coulombic efficiency of lithium metal half-cells prepared using commercial polypropylene separators and the films prepared in Examples 1, 2, and 3 as separators under different current density conditions.

[0024] Figure 5 It is a comparison chart of the cycle performance of lithium-lithium symmetric batteries prepared using commercial polypropylene separators and the films prepared in Examples 1, 2, and 3 as separators.

[0025] Figure 6 It is a comparison chart of the capacity and cycle performance of lithium metal full batteries prepared using commercial polypropylene diaphragms and the films prepared in Examples 1, 2, and 3 as diaphragms. (V) Specific implementation methods

[0026] The technical solution of the present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.

[0027] The commercial polypropylene film used in the examples was purchased from Celgard.

[0028] Example 1

[0029] Take 0.8g of gelatin and dissolve it in 10g of anhydrous 2,2,2-trifluoroethanol, stir for 12 hours to prepare gelatin spinning solution; the stirred solution is spun into film through a spinning machine, the voltage is 12kv, the injection speed is 0.4mm / min, the distance between the needle and the receiving device is 15cm, the spinning time is 1h, and the sprayed film is collected; the collected gelatin film is placed in a 60℃ vacuum oven for drying (drying until the film is slightly rolled up), and then pressed into a small disc with a diameter of 16mm by a tablet press at 10MPa, which is a gelatin fiber diaphragm. The thickness of the gelatin diaphragm is 20-40μm.

[0030] The obtained gelatin fiber membrane was used as a separator to test the ionic conductivity and assemble lithium metal batteries, including Li / Cu half-cells, Li / Li symmetric cells and Li / LiFePO4 full cells. The coulombic efficiency, stability and capacity retention were tested respectively.

[0031] The gelatin fiber separator prepared in Example 1 was used to test the ionic conductivity in the following manner and assembled into a Li / Cu half-cell, a Li / Li symmetric cell and a Li / LiFePO4 full cell.

[0032] For the test of ionic conductivity, the prepared membrane was sandwiched between two stainless steel gaskets and assembled in an argon glove box (H2O < 0.01 ppm, O2 < 0.01 ppm) using DOL / DME (1:1 w / w) with 1 M LiTFSI and 1 wt% LiNO3 as additives. A commercial polypropylene membrane (Celgard 2400) was selected as the membrane for the control group. The ionic conductivity of the membrane was calculated based on the measured impedance, contact area, and membrane thickness using the same steps as above.

[0033] For Li / Cu half-cells, the cut copper sheets were first washed with dilute hydrochloric acid, then washed with a large amount of deionized water until neutral, and finally washed twice with alcohol and air-dried at room temperature. The washed copper sheets were used as current collectors, and DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives was used as the electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm as the diaphragm, and the same steps were followed.

[0034] For Li / Li symmetric cells, 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). A commercial polypropylene separator was selected as the separator for the control group, and the above steps were followed.

[0035] For the Li / LiFePO4 full cell, LiFePO4, PVDF and acetylene black were prepared into slurry in a mass ratio of 8:1:1, applied on the washed carbon-coated aluminum foil using a coater, dried in an oven at 80°C, and then pressed into pole pieces using a tablet press at 10MPa. 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolytes, and assembled into full cells in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm, and the same steps were followed.

[0036] The gelatin fiber membrane prepared in Example 1 was used to test the ionic conductivity, and Li / Cu half-cell, Li / Li symmetric cell and Li / LiFePO4 full cell were assembled and electrochemically tested according to the following method.

[0037] The assembled stainless steel gasket battery was tested for impedance using an electrochemical workstation at a scan rate of 0.1 Hz. Based on the measured impedance, diaphragm contact area (2 cm -2 ), membrane thickness (20 μm), calculate the ionic conductivity of each membrane, as shown in the attached Figure 3 As shown, the conductivity of the diaphragm prepared in Example 1 is 0.7 ms / cm -1 , while the conductivity of commercial polypropylene separator is 0.35ms / cm -1 .

[0038] The assembled half-cell, symmetrical cell and full cell were tested on the Xinwei battery rack. For the Li / Cu half-cell coulombic efficiency test, the battery was first activated at a current density of 0.05mA in the voltage range of 0.01-1V. Then it was discharged (a certain capacity of lithium was plated on the copper sheet with a certain current), and then charged (the plated lithium was pulled out with a certain voltage). The pulled out lithium was compared with the plated lithium to calculate the coulombic efficiency of the half-cell, as shown in the attached figure. Figure 4 As shown in the figure, the battery assembled with the separator prepared in Example 1 can cycle 100 times with a coulombic efficiency of 97%, while the battery with the commercial polypropylene separator can only cycle 60 times with a coulombic efficiency of less than 80%. For the Li / Li symmetric battery, the same amount of lithium is pulled out and plated under 1C conditions, and the growth of lithium dendrites is judged according to the level of overpotential, as shown in the attached figure. Figure 5 As shown in the figure, the battery assembled with the separator prepared in Example 1 can cycle for 800 hours with an overpotential of 23mv, while the battery with the commercial polypropylene separator can only cycle for 600 hours with an overpotential greater than 25mv. For the capacity retention test of the Li / LiFePO4 full battery, the battery was first activated at 0.2C, and then the battery was charged and discharged within 1.8-2.6V to test the capacity retention of the full battery, as shown in the attached figure. Figure 6The full battery with gelatin separator prepared in Example 1 can be cycled for 200 times, the coulombic efficiency is close to 100%, and the capacity is maintained at 108 mAh g -1 , the battery with commercial polypropylene separator can only cycle 150 times and the capacity is less than 100 mAh g -1 .

[0039] As shown in Figure 2, the contact angle of the gelatin membrane prepared in Example 1 in water is 73°, and the contact angle of the commercial polypropylene membrane is 114°, indicating that the gelatin membrane prepared in Example 1 has better electrolyte wettability.

[0040] Example 2

[0041] Take 1g of gelatin and dissolve it in 10g of anhydrous 2,2,2-trifluoroethanol, stir for twelve hours, and prepare a gelatin spinning solution with a mass of 10%; the stirred solution is spun into a film through a spinning machine, the voltage is 12kv, the injection speed is 0.4mm / min, the distance between the needle and the receiving device is 15cm, the spinning time is 1h, and the sprayed film is collected; the collected gelatin film is placed in a 60℃ vacuum oven for drying (drying until the film is slightly rolled up), and then pressed into a small disc with a diameter of 16mm by a tablet press at 10MPa, which is a gelatin fiber diaphragm. The thickness of the gelatin diaphragm is 20-40μm.

[0042] The obtained gelatin fiber membrane was used as a separator to test the ionic conductivity, and lithium metal batteries were assembled, including Li / Cu half-cells, Li / Li symmetric cells and Li / LiFeCoPO4 full cells, and the coulombic efficiency, stability and capacity retention were tested respectively.

[0043] The gelatin fiber separator prepared in Example 2 was used to test the ionic conductivity in the following manner and assembled into a Li / Cu half-cell, a Li / Li symmetric cell and a Li / LiFePO4 full cell.

[0044] For the test of ionic conductivity, the prepared membrane was sandwiched between two stainless steel gaskets, and DOL / DME (1:1w / w) with 1MLiTFSI and 1wt%LiNO3 as additives was used as the electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene membrane (Celgard 2400) as the membrane, and the same steps were followed. The ionic conductivity of the membrane was calculated based on the measured impedance, contact area, and membrane thickness.

[0045] For Li / Cu half-cells, the cut copper sheets were first washed with dilute hydrochloric acid, then washed with a large amount of deionized water until neutral, and finally washed twice with alcohol and air-dried at room temperature. The washed copper sheets were used as current collectors, and DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives was used as the electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm as the diaphragm, and the same steps were followed.

[0046] For Li / Li symmetric cells, 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). A commercial polypropylene separator was selected as the separator for the control group, and the above steps were followed.

[0047] For the Li / LiFePO4 full cell, LiFePO4, PVDF and acetylene black were prepared into slurry in a mass ratio of 8:1:1, applied on the washed carbon-coated aluminum foil using a coater, dried in an oven at 80°C, and then pressed into pole pieces using a tablet press at 10MPa. 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolytes, and assembled into full cells in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm, and the same steps were followed.

[0048] The gelatin fiber membrane prepared in Example 2 was used to test the ionic conductivity, and Li / Cu half-cell, Li / Li symmetric cell and Li / LiFePO4 full cell were assembled and electrochemically tested according to the following method.

[0049] The assembled stainless steel gasket battery was tested for impedance using an electrochemical workstation at a scan rate of 0.1 Hz. Based on the measured impedance, diaphragm contact area (2 cm -2 ) membrane thickness (20 μm), calculate the ionic conductivity of each membrane, as shown in the attached Figure 3 As shown, the conductivity of the diaphragm prepared in Example 2 is 0.83 ms / cm -1 , while the conductivity of commercial polypropylene separator is 0.35ms / cm -1 .

[0050] The assembled half-cell, symmetrical cell and full cell were tested on the Xinwei battery rack. For the Li / Cu half-cell coulombic efficiency test, the battery was first activated at a current density of 0.05mA in the voltage range of 0.01-1V. Then it was discharged (a certain capacity of lithium was plated on the copper sheet with a certain current), and then charged (the plated lithium was pulled out with a certain voltage). The pulled out lithium was compared with the plated lithium to calculate the coulombic efficiency of the half-cell, as shown in the attached figure. Figure 4 As shown in the figure, the battery assembled with the separator prepared in Example 2 can cycle 100 times with a coulombic efficiency of 98%, while the battery with the commercial polypropylene separator can only cycle 60 times with a coulombic efficiency of less than 80%. For the Li / Li symmetric battery, the same amount of lithium is pulled out and plated under 1C conditions. The growth of lithium dendrites is judged according to the level of overpotential, as shown in the attached figure. Figure 5 As shown in the figure, the battery assembled with the separator prepared in Example 2 can cycle for 800 hours with an overpotential of 15mv, while the battery with the commercial polypropylene separator can only cycle for 600 hours with an overpotential greater than 25mv. For the capacity retention test of the Li / LiFePO4 full battery, the battery was first activated at 0.2C, and then the battery was charged and discharged within 1.8-2.6V to test the capacity retention of the full battery, as shown in the attached figure. Figure 6 The full battery with gelatin membrane prepared in Example 2 can be cycled for 200 times, with a coulombic efficiency close to 100% and a capacity of 110 mAh g -1 , the battery with commercial polypropylene separator can only cycle 150 times and the capacity is less than 100 mAh g -1 .

[0051] As shown in Figure 2, the contact angle of the gelatin membrane prepared in Example 2 in water is 26°, and the contact angle of the commercial polypropylene membrane is 114°, indicating that the gelatin membrane prepared in Example 2 has better electrolyte wettability.

[0052] Example 3

[0053] Take 1.2g of gelatin and dissolve it in 10g of anhydrous 2,2,2-trifluoroethanol, stir for twelve hours, and prepare a gelatin spinning solution with a mass fraction of 12%; the stirred solution is spun into a film through a spinning machine, the voltage is 12kv, the injection speed is 0.4mm / min, the distance between the needle and the receiving device is 15cm, the spinning time is 1h, and the sprayed film is collected; the collected gelatin film is placed in a 60℃ vacuum oven for drying (drying until the film is slightly rolled up), and then pressed into a small disc with a diameter of 16mm by a tablet press at 10MPa, which is a gelatin fiber diaphragm. The thickness of the gelatin diaphragm is 20-40μm.

[0054] The obtained gelatin fiber membrane was used as a separator to test the ionic conductivity, and lithium metal batteries were assembled, including Li / Cu half-cells, Li / Li symmetric cells and Li / LiFeCoPO4 full cells, and the coulombic efficiency, stability and capacity retention were tested respectively.

[0055] The gelatin fiber separator prepared in Example 3 was used to test the ionic conductivity in the following manner and assembled into a Li / Cu half-cell, a Li / Li symmetric cell and a Li / LiFePO4 full cell.

[0056] For the test of ionic conductivity, the prepared membrane was sandwiched between two stainless steel gaskets and assembled in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm) using DOL / DME (1:1w / w) with 1MLiTFSI and 1wt%LiNO3 as additives. A commercial polypropylene membrane (Celgard 2400) was selected as the membrane for the control group. The ionic conductivity of the membrane was calculated based on the measured impedance, contact area, and membrane thickness in the same manner as above.

[0057] For Li / Cu half-cells, the cut copper sheets were first washed with dilute hydrochloric acid, then washed with a large amount of deionized water until neutral, and finally washed twice with alcohol and air-dried at room temperature. The washed copper sheets were used as current collectors, and DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives was used as the electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm as the diaphragm, and the same steps were followed.

[0058] For Li / Li symmetric cells, 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolyte in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). A commercial polypropylene separator was selected as the separator for the control group, and the above steps were followed.

[0059] For the Li / LiFePO4 full cell, LiFePO4, PVDF and acetylene black were prepared into slurry in a mass ratio of 8:1:1, applied on the washed carbon-coated aluminum foil using a coater, dried in an oven at 80°C, and then pressed into pole pieces using a tablet press at 10MPa. 1M LiTFSI and 1wt% LiNO3 as additives in DOL / DME (1:1w / w) were used as electrolytes, and assembled into full cells in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The control group selected a commercial polypropylene diaphragm, and the same steps were followed.

[0060] The gelatin fiber membrane prepared in Example 3 was used to test the ionic conductivity, and Li / Cu half-cell, Li / Li symmetric cell and Li / LiFePO4 full cell were assembled and electrochemically tested according to the following method.

[0061] The assembled stainless steel gasket battery was tested for impedance using an electrochemical workstation at a scan rate of 0.1 Hz. Based on the measured impedance, diaphragm contact area (2 cm -2 ) membrane thickness (20 μm), calculate the ionic conductivity of each membrane, as shown in the attached Figure 3 As shown, the conductivity of the diaphragm prepared in Example 3 is 0.54 ms / cm -1 , while the conductivity of commercial polypropylene separator is 0.35ms / cm -1 .

[0062] The assembled half-cell, symmetrical cell and full cell were tested on the Xinwei battery rack. For the Li / Cu half-cell coulombic efficiency test, the battery was first activated at a current density of 0.05mA in the voltage range of 0.01-1V. Then it was discharged (a certain capacity of lithium was plated on the copper sheet with a certain current), and then charged (the plated lithium was pulled out with a certain voltage). The pulled out lithium was compared with the plated lithium to calculate the coulombic efficiency of the half-cell, as shown in the attached figure. Figure 4 As shown in the figure, the battery assembled with the separator prepared in Example 3 can cycle 100 times with a coulombic efficiency of 96%, while the battery with the commercial polypropylene separator can only cycle 60 times with a coulombic efficiency of less than 80%. For the Li / Li symmetric battery, the same amount of lithium is pulled out and plated under 1C conditions. The growth of lithium dendrites is judged according to the level of overpotential, as shown in the attached figure. Figure 5 As shown in the figure, the battery assembled with the separator prepared in Example 3 can cycle for 800 hours with an overpotential of 14mv, while the battery with the commercial polypropylene separator can only cycle for 600 hours with an overpotential greater than 25mv. For the capacity retention test of the Li / LiFePO4 full battery, the battery was first activated at 0.2C, and then the battery was charged and discharged within 1.8-2.6V to test the capacity retention of the full battery, as shown in the attached figure. Figure 6 The full battery with gelatin membrane prepared in Example 3 can be cycled for 200 times, with a coulombic efficiency close to 100% and a capacity of 105 mAh g -1 , the battery with commercial polypropylene separator can only cycle 150 times and the capacity is less than 100 mAh g -1 .

[0063] As shown in Figure 2, the contact angle of the gelatin membrane prepared in Example 3 in water is 63°, and the contact angle of the commercial polypropylene membrane is 114°, indicating that the gelatin membrane prepared in Example 1 has better electrolyte wettability.

Claims

1. Application of a gelatin fiber separator as a separator in a lithium metal battery, characterized in that: The preparation method of the gelatin fiber diaphragm comprises the following steps: (1) dissolving gelatin in an organic solvent and stirring for 8 to 12 hours to obtain a gelatin spinning solution; the organic solvent is anhydrous 2,2,2-trifluoroethanol; the mass ratio of gelatin to anhydrous 2,2,2-trifluoroethanol is 0.8-1.2:10; (2) using electrospinning technology, spinning the solution prepared in step (1) at a constant voltage to form a film, and collecting the sprayed gelatin film, wherein the spinning voltage range is 8 to 12 kV, the injection speed is 0.2 to 0.6 mm / min, the distance between the needle and the receiving device is 12 to 16 cm, and the spinning time is 0.5 to 1 h; (3) The gelatin film obtained in step (2) is taken out, and a gelatin fiber membrane is obtained by drying and pressing.

2. The use according to claim 1, characterized in that: The mass ratio of the gelatin to anhydrous 2,2,2-trifluoroethanol is 1:

10.

3. The use according to claim 1 or 2, characterized in that: In step (2), the voltage is 12 kV; the injection speed is 0.4 mm / min, the distance between the needle and the receiving device is 15 cm, and the spinning time is 1 hour.

4. The use according to claim 1 or 2, characterized in that: In step (3), the drying conditions are: vacuum drying at 50-70°C.

5. The use according to claim 1 or 2, characterized in that: In step (3), the tablet is formed by one-step compression using a tablet press, and the pressure is controlled at 8-10 MPa.

6. The use according to claim 1, characterized in that: The electrolyte of the lithium metal battery is DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives, wherein the mass ratio of DOL and DME is 1:1; or the electrolyte is EC / DEC / EMC with 1M LiPF6 and 1wt% LiNO3 as additives, wherein the volume ratio of EC, DEC and EMC is 1:1:1.

Citation Information

Patent Citations

  • Lithium ion battery and electrolyte thereof

    CN102709588A

  • Electrospinning fibrous membrane production device and method of producing electrospinning fibrous membranes thereby

    CN103911767A

  • Portable electrostatic spinning equipment and using method thereof

    CN104790049A

  • Treatment method and application for improving water solubility of electrospinning gelatin film

    CN108210998A

  • Liquid electrolyte formulation for lithium metal secondary battery and lithium metal secondary battery comprising the same

    CN109962286A