A method for preparing a strong-bonded double-layer nanofiltration membrane

By blending carboxyl-terminated SMA and polymer membrane materials and performing polyhydroxy polymer esterification and linear diacyl chloride cross-linking, a strongly bonded double-layer nanofiltration membrane is formed, which solves the problem of poor chlorine resistance and bonding of nanofiltration membranes prepared by interfacial polymerization. The problem of weak force is eliminated and efficient drinking water separation performance is achieved.

CN114191989BActive Publication Date: 2024-10-01GUIZHOU MATERIAL IND TECH INSTITUE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111453049.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-01
Publication Date
2024-10-01
Estimated Expiration
2041-12-01

AI Technical Summary

Technical Problem

The existing polyamide nanofiltration membrane prepared by interfacial polymerization has poor chlorine resistance, weak binding force between the separation layer and the support layer, and short service life, making it difficult to meet the high-efficiency separation requirements for drinking water purification.

Method used

A homogeneous film casting liquid is prepared by blending carboxyl-terminated SMA and polymer membrane materials, and a surface carboxylated ultrafiltration membrane is prepared using a phase inversion method. Polyhydroxy polymer esterification and linear diacyl chloride cross-linking are performed on the surface to form a strong Combined double-layer nanofiltration membrane structure.

Benefits of technology

The obtained double-layer nanofiltration membrane has excellent permeability, chlorine resistance and high binding force, can maintain separation performance under high pressure for a long time, and is suitable for drinking water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003385672700000041
    Figure BDA0003385672700000041
Patent Text Reader

Abstract

The invention discloses a method for preparing a strong-bonded double-layer nanofiltration membrane, comprising the following steps: step 1, obtaining a carboxyl-terminated SMA macromolecule, and then blending the carboxylated SMA and a polymer membrane material into a homogeneous casting liquid; step 2, using a phase inversion method to prepare the casting liquid into a surface carboxylated ultrafiltration membrane material; step 3, adding a polyhydroxy polymer to the surface of the surface carboxylated ultrafiltration membrane material, and the polyhydroxy polymer and the carboxyl group undergo an esterification reaction to obtain a single-layer nanofiltration membrane; step 4, adding a linear diacyl chloride monomer to the surface of the single-layer nanofiltration membrane for secondary crosslinking to obtain a strong-bonded double-layer nanofiltration membrane. The invention has the characteristics of simple operation, strong bonding between the composite layers of the prepared nanofiltration membrane, and excellent separation performance. Compared with the traditional interfacial polymerization method for preparing polyamide nanofiltration membranes, the invention can obtain a nanofiltration membrane with a double-layer separation structure on the surface through a secondary reaction. The product obtained according to the method has the characteristics of excellent permeability, good chlorine resistance and high pressure resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the technical field of polymer materials, in particular to a method for preparing a strongly bonded double-layer nanofiltration membrane. [Background technology]

[0002] In membrane separation technology, separation membrane is the most basic and core part. According to the membrane structure characteristics and the size of the retained substances, separation membranes can be mainly divided into microfiltration membranes, ultrafiltration membranes, nanofiltration membranes and reverse osmosis membranes. Among them, the effective separation pore size of nanofiltration membranes is about 1nm, which is between reverse osmosis membranes and ultrafiltration membranes. Based on its unique structure and separation characteristics, nanofiltration membrane separation technology has shown an excellent effect in drinking water purification and is an effective method for preparing high-quality drinking water. At present, there are four main preparation methods for nanofiltration membranes: phase inversion method (immersion precipitation phase inversion method), composite method, charging method and inorganic modification. The interfacial polymerization method in the composite method is the most commonly used method for commercially available nanofiltration.

[0003] Interfacial polymerization (IP) is one of the most commonly used surface coating methods. There are three basic steps in preparing nanofiltration membranes by interfacial polymerization: (1) preparing a porous support layer base membrane (usually an ultrafiltration membrane), (2) coating the surface of the porous base membrane with an aqueous solution of compounds containing active groups such as polyamines, and (3) removing excess aqueous solution to maintain a uniform distribution of amine groups on the membrane surface, and continuing to coat the membrane surface with an organic phase solution to complete the interfacial polymerization process. For example, commercial polyamide composite membranes are prepared by interfacial polymerization, but the polyamide nanofiltration membranes prepared by this cross-linking reaction have poor chlorine resistance and weak bonding between the separation layer and the support layer. They are subject to greater restrictions during use and are easily affected by the environment, which reduces their service life. [Summary of the invention]

[0004] In order to solve the above technical problems, the present invention discloses a method for preparing a strongly bonded double-layer nanofiltration membrane. The present invention has the characteristics of simple operation, strong bonding between the composite layers of the prepared nanofiltration membrane, and excellent separation performance. Compared with the traditional interfacial polymerization method for preparing polyamide nanofiltration membrane, the present invention can obtain a nanofiltration membrane with a double-layer separation structure on the surface through a secondary reaction. The product obtained according to the method has the characteristics of excellent permeability, good chlorine resistance and high pressure resistance.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] A method for preparing a strong-bonded double-layer nanofiltration membrane comprises the following steps:

[0007] Step 1, obtaining a carboxyl-terminated SMA macromolecule, and then blending the carboxylated SMA and the polymer membrane material into a homogeneous membrane casting solution;

[0008] Step 2: using a phase inversion method to prepare a surface carboxylation ultrafiltration membrane material from the casting solution;

[0009] Step 3: adding a polyhydroxy polymer to the surface of the surface carboxylation ultrafiltration membrane material, and performing an esterification reaction between the polyhydroxy polymer and the carboxyl group to obtain a single-layer nanofiltration membrane;

[0010] Step 4: Add linear diacyl chloride monomers to the surface of the single-layer nanofiltration membrane for secondary cross-linking to obtain a strongly bonded double-layer nanofiltration membrane.

[0011] As a further improvement, the polymer membrane material comprises a polymer membrane main material, an additive and an organic solvent; in the homogeneous casting solution, the mass percentages of the polymer membrane material, the end carboxyl SMA, the additive and the organic solvent are 15-20%; 0.5-8%; 2-12%; 63-80% respectively.

[0012] As a further improvement, the main material of the polymer membrane is one of polyethersulfone, polysulfone and polyvinylidene fluoride; the additive is one of polyethylene glycol and polyvinyl pyrrolidone or a mixture; and the organic solvent is N,N-dimethylacetamide or N,N-dimethylformamide.

[0013] As a further improvement, the polyhydroxy polymer is polyglycerol, the mass concentration of polyglycerol is 0.5%-10%, and the solvent of polyglycerol is deionized water.

[0014] As a further improvement, the linear diacyl chloride is one of succinoyl chloride, adipoyl chloride or succinoyl chloride or any mixture thereof, the mass concentration of the linear diacyl chloride is 0.5%-10%, and the solvent of the linear diacyl chloride is n-hexane.

[0015] As a further improvement, the preparation method of the carboxyl-terminated SMA macromolecule is as follows: SMA with an anhydride content of more than 10% is taken, and the SMA is soaked in a sodium hydroxide aqueous solution for 24 hours, and then filtered and washed with deionized water to obtain the carboxyl-terminated SMA macromolecule.

[0016] As a further improvement, the alkaline solution is a sodium hydroxide alkaline solution with a mass concentration of 5%.

[0017] As a further improvement, in the step 1, the homogeneous casting liquid is mechanically stirred evenly, and then allowed to stand in vacuum to degas for standby use.

[0018] As a further improvement, in the step 2, when the surface carboxylation ultrafiltration membrane material is prepared by the phase inversion method, deionized water is used as the coagulation bath.

[0019] Compared with the existing technology, the present invention is simple to operate and has excellent composite membrane performance. At the same time, since the SMA and the matrix enhance the bonding ability between the separation layer and the support layer through blending, the prepared composite nanofiltration membrane has the effects of high water flux, strong bonding force, and excellent chlorine resistance. It has good development prospects in the water treatment process for drinking water. [Specific implementation method]

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] A method for preparing a strong-bonded double-layer nanofiltration membrane, the specific steps are as follows:

[0023] 1) Preparation of casting solution: Add 20g polyethersulfone, 5g carboxyl-terminated SMA and 5g polyethylene glycol-800 to 70g DMAC organic solution, heat to 70°C, and stir until homogeneous;

[0024] 2) Vacuum standing degassing: keep the above casting solution in a heated state and evacuate it, stop stirring and perform degassing treatment;

[0025] 3) Preparation of base film: The above casting solution is prepared into a base film by a phase inversion method and placed in deionized water for standby use;

[0026] 4) Preparation of single-layer nanofiltration membrane: Prepare a polyglycerol solution with a mass fraction of 10%, pour the solution on the surface of the base membrane, and obtain a single-layer polyester composite nanofiltration membrane after cross-linking for 2 hours;

[0027] 5) Preparation of double-layer nanofiltration membrane: Prepare a 0.5% by mass fraction n-hexane solution of succinyl chloride, pour the solution on the surface of the single-layer nanofiltration membrane, and obtain a double-layer nanofiltration membrane after cross-linking for 1 minute.

[0028] Embodiment 2:

[0029] A method for preparing a strong-bonded double-layer nanofiltration membrane, the specific steps are as follows:

[0030] 1) Preparation of casting solution: Add 15 g polysulfone, 5 g carboxyl-terminated SMA and 3 g polyvinylpyrrolidone K30 to 77 g DMAC organic solution, heat to 70° C., and stir until homogeneous;

[0031] 2) Vacuum standing degassing: keep the above casting solution in a heated state and evacuate it, stop stirring and perform degassing treatment;

[0032] 3) Preparation of base film: The above casting solution is prepared into a base film by phase inversion method and placed in deionized water for standby use;

[0033] 4) Preparation of composite nanofiltration membrane: Prepare a polyglycerol solution with a mass fraction of 0.5%, pour the solution on the surface of the base membrane, and obtain a single-layer composite nanofiltration membrane after cross-linking for 5 hours.

[0034] 5) Preparation of double-layer nanofiltration membrane: Prepare a 5% by mass hexane solution of adipoyl chloride, pour the solution on the surface of the single-layer nanofiltration membrane, and obtain a double-layer nanofiltration membrane after cross-linking for 30 seconds.

[0035] Embodiment 3:

[0036] A method for preparing a strong-bonded double-layer nanofiltration membrane, the specific steps are as follows:

[0037] 1) Preparation of casting solution: Add 20g polyvinylidene fluoride, 5g carboxyl-terminated SMA and 5g polyvinyl pyrrolidone into 70g DMAC organic solution, heat to 80°C, and stir until homogeneous;

[0038] 2) Vacuum standing degassing: keep the above casting solution in a heated state and evacuate it, stop stirring and perform degassing treatment;

[0039] 3) Preparation of base film: The above casting solution is prepared into a base film by phase inversion method and placed in deionized water for standby use;

[0040] 4) Preparation of composite nanofiltration membrane: Prepare a polyglycerol solution with a mass fraction of 3%, pour the solution on the surface of the base membrane, and obtain the composite nanofiltration membrane after cross-linking for 3 hours.

[0041] 5) Preparation of double-layer nanofiltration membrane: Prepare a 1% by mass hexane solution of adipoyl chloride, pour the solution on the surface of the single-layer nanofiltration membrane, and obtain a double-layer nanofiltration membrane after cross-linking for 2 minutes.

[0042] Embodiment 4:

[0043] A method for preparing a strong-bonded double-layer nanofiltration membrane, the specific steps are as follows:

[0044] 1) Preparation of casting solution: Add 18 g polysulfone, 2 g carboxyl-terminated SMA and 5 g polyethylene glycol-1000 to 75 g DMAC organic solution, heat to 70° C., and stir until homogeneous;

[0045] 2) Vacuum standing degassing: keep the above casting solution in a heated state and evacuate it, stop stirring and perform degassing treatment;

[0046] 3) Preparation of base film: The above casting solution is prepared into a base film by phase inversion method and placed in deionized water for standby use;

[0047] 4) Preparation of composite nanofiltration membrane: Prepare a polyglycerol solution with a mass fraction of 2%, pour the solution on the surface of the base membrane, and obtain the composite nanofiltration membrane after cross-linking for 5 hours.

[0048] 5) Preparation of double-layer nanofiltration membrane: Prepare a 0.2% by mass fraction n-hexane solution of sebacic acid dichloride, pour the solution on the surface of the single-layer nanofiltration membrane, and obtain a double-layer nanofiltration membrane after cross-linking for 1 minute.

[0049] The product performance obtained in the above embodiment is as follows: The chlorine resistance test is carried out by immersing the composite membrane in a 50 mg / L NaClO aqueous solution for 100 hours and then testing its sodium sulfate retention rate and water flux before and after treatment (see Table 1).

[0050] Table 1 Product performance test table of Examples 1-4

[0051]

[0052] Through the above experiments, it is known that the prepared double-layer composite nanofiltration membrane has a high retention rate for divalent salt sodium sulfate, reaching the nanofiltration desalination level. In addition, the composite membrane has excellent permeability and anti-pollution ability, and the membrane structure remains intact for a long time under an operating pressure of 1Mpa, proving that this method is a feasible method for preparing a strongly bonded double-layer nanofiltration membrane.

[0053] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment by any technician familiar with this patent without departing from the scope of the technical solution of the present invention according to the technical essence of the present invention still falls within the scope of the solution of the present invention.

Claims

1. A method for preparing a strong-bonded double-layer nanofiltration membrane, characterized in that: The steps include: Step 1, obtaining a carboxyl-terminated SMA macromolecule, and then blending the carboxylated SMA and the polymer membrane material into a homogeneous casting solution; the preparation method of the carboxyl-terminated SMA macromolecule is as follows: taking SMA with an anhydride content of more than 10%, soaking the SMA in a sodium hydroxide aqueous solution for 24 hours, and then filtering and washing with deionized water to obtain a carboxyl-terminated SMA macromolecule; Step 2: using a phase inversion method to prepare a surface carboxylation ultrafiltration membrane material from the casting solution; Step 3: adding a polyhydroxy polymer to the surface of the surface carboxylation ultrafiltration membrane material, and performing an esterification reaction between the polyhydroxy polymer and the carboxyl group to obtain a single-layer nanofiltration membrane; Step 4: adding linear diacyl chloride monomer to the surface of the single-layer nanofiltration membrane for secondary cross-linking to obtain a strongly bonded double-layer nanofiltration membrane; The polymer membrane material comprises a polymer membrane main material, an additive and an organic solvent; in the homogeneous casting solution, the mass percentages of the polymer membrane material, the end-carboxylation SMA, the additive and the organic solvent are 15-20%; 0.5-8%; 2-12%; 63-80% respectively; The polyhydroxy polymer is polyglycerol, the mass concentration of polyglycerol is 0.5%-10%, and the solvent of polyglycerol is deionized water; The linear diacyl chloride is one of succinyl chloride, adipoyl chloride or sebacoyl chloride or any mixture thereof, the mass concentration of the linear diacyl chloride is 0.5%-10%, and the solvent of the linear diacyl chloride is n-hexane.

2. The method for preparing a strong-binding double-layer nanofiltration membrane according to claim 1, characterized in that: The main material of the polymer membrane is one of polyethersulfone, polysulfone and polyvinylidene fluoride; the additive is one of polyethylene glycol and polyvinyl pyrrolidone or a mixture; the organic solvent is N,N-dimethylacetamide or N,N-dimethylformamide.

3. The method for preparing a strong-binding double-layer nanofiltration membrane according to claim 1, characterized in that: The sodium hydroxide aqueous solution is a sodium hydroxide alkaline solution with a mass concentration of 5%.

4. The method for preparing a strong-binding double-layer nanofiltration membrane according to claim 1, characterized in that: In the step 1, the homogeneous casting liquid is mechanically stirred evenly, and then allowed to stand in vacuum to degas for later use.

5. The method for preparing a strong-bonding double-layer nanofiltration membrane according to claim 1, characterized in that: In the step 2, when the surface carboxylation ultrafiltration membrane material is prepared by the phase inversion method, deionized water is used as the coagulation bath.