Cobalt-based single-atom dehydrogenation catalyst with good selectivity and regeneration stability and method for preparing corresponding olefins from paraffin using the same

By modifying the zirconia core in silica surface, supporting a single-atom cobalt catalyst to form a tetrahedral structure, the problem of insufficient reaction stability of cobalt-based catalysts at high temperatures is solved, and efficient preparation of olefins and commercialization of catalysts is achieved. application.

CN114192129BActive Publication Date: 2024-11-05SK INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111095052.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-18
Filing Date
2021-09-17
Publication Date
2024-11-05
Estimated Expiration
2041-09-17

AI Technical Summary

Technical Problem

The existing cobalt-based single-atom dehydrogenation catalysts are insufficient in reaction stability and regeneration stability at high temperatures, resulting in rapid catalyst deactivation and increased side reactions, making it difficult to use in commercial processes.

Method used

By modifying the zirconia core in the silica surface, a cobalt catalyst with a single atom form is prepared, and a silica-modified zirconia support is used to support cobalt to form a cobalt active site in the tetrahedral structure, and under specific conditions Carry out dehydrogenation reaction.

Benefits of technology

It improves the long-term reaction stability and regeneration stability of the catalyst, enhances the selectivity and conversion of olefins, and is suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114192129B_ABST
    Figure CN114192129B_ABST
Patent Text Reader

Abstract

The present invention relates to a dehydrogenation catalyst using a support body whose zirconium oxide core is surface-modified with silicon dioxide to support cobalt in a single atomic form and a preparation method thereof, and to a method for dehydrogenating alkanes, particularly hard alkanes, in the presence of the dehydrogenation catalyst to prepare olefins corresponding thereto.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cobalt-based single-atom dehydrogenation catalyst with good selectivity and regeneration stability and a method for preparing corresponding olefins from paraffin using the dehydrogenation catalyst. More specifically, it relates to a dehydrogenation catalyst using a support body with a zirconium oxide core surface modified with silicon dioxide to support single-atom cobalt and a preparation method thereof, and to a method for preparing corresponding olefins by dehydrogenating paraffins, particularly hard paraffins, in the presence of the dehydrogenation catalyst. Background Art

[0002] In recent years, the catalyst technology of using active metals on supports has attracted much attention. In particular, with the development of nanotechnology, research on using active metals of nanometer size on supports is being actively conducted. However, nanometer-sized active metals have a wide size distribution and irregular morphological characteristics. Therefore, although they are more active than existing catalysts, they are pointed out to cause side reactions or rapid catalyst deactivation when used as catalysts.

[0003] In addition, in the case of a catalyst with a single atomic size load, the catalyst activity can be maximized by reducing the size of the metal active site to an atomic level below the nanometer size. In particular, due to having an extremely simplified and ideal structure, it is provided to be suitable for simulating the theoretical results obtained by computational science etc. and to carry out the advantages of related research. To this, there are the following examples, where transition metals such as zinc (Zn), cobalt (Co) etc. are loaded on a support of silicon dioxide etc. in a single atomic form to be used as a dehydrogenation catalyst for hard paraffins. In addition, it is reported that when the active metal in the form of a single atom is loaded, there is the advantages such as minimization of cracks (cracking) and suppression of the formation of coke in the reaction (for example, ACS Catal.2014,4,4,1091-1098).

[0004] However, in the above-mentioned documents, in order to keep the concentration of the reactant at a low level, a mixed gas (the reactant is 3% propane, and the remaining components are a mixed gas composed of argon (Ar) as an inert gas) is used to suppress by-products while converting the paraffin into the corresponding olefin as selectively as possible, and the reaction is carried out at a low temperature to increase the life of the catalyst, etc., which is difficult to apply in actual commercial processes. In addition, in the method of carrying out the dehydrogenation reaction of paraffin in the presence of a catalyst in which cobalt active metal is supported on a support in the form of a single atom, in the dehydrogenation reaction carried out at a high temperature, a cobalt metal generation reaction occurs due to the mutual aggregation phenomenon or reduction phenomenon of the cobalt element fixed on the support, so there is a limitation in ensuring long-term reaction stability or regeneration stability.

[0005] In order to suppress the above problems, various methods have been studied and reported (for example, Korean Patent Publication No. 2020-0049209), but since the strength or durability of silica as a support is reduced due to continuous exposure to high temperatures during the dehydrogenation reaction, the yield may decrease as the reaction is repeated.

[0006] Therefore, there is a need for a single atom catalyst with good long-term reaction stability or regeneration stability compared with the prior art. Summary of the invention

[0007] Technical issues to be solved

[0008] In a specific embodiment of the present invention, a catalyst loaded with cobalt (Co) in single atom form and a method for preparing the same are provided, wherein the catalyst can improve the long-term reaction stability or regeneration stability of a dehydrogenation catalyst used in the reaction of preparing olefins from alkanes.

[0009] Technical Solution

[0010] According to a first aspect of the present invention, there is provided a method for preparing a cobalt-based catalyst in the form of a single atom, the method comprising the following steps: a) modifying the surface or the outer portion of zirconia with silica to prepare a silica-modified zirconia support; b) preparing a water-based dispersion of the silica-modified zirconia support; c) adding an alkali component to the water-based dispersion of the silica-modified zirconia support to adjust the pH to at least 10, thereby preparing a pH-adjusted water-based dispersion of the silica-modified zirconia support; d) separately preparing an aqueous solution of a cobalt precursor having an oxidation number of 3+, and adding an alkali component to prepare a pH-adjusted cobalt precursor aqueous solution; e) by combining the pH-adjusted f) removing the cobalt ions not adsorbed on the surface of the silica-modified zirconia support; and g) heat-treating the silica-modified zirconia support adsorbed with cobalt ions obtained from step f); wherein the cobalt with an oxidation number of 2+ in the cobalt-based catalyst exists in the form of an isolated single atom on the silica-modified zirconia support, and the cobalt with an oxidation number of 2+ forms a tetrahedral structure and is coordinated in the three-membered hydroxyl ring present on the surface of the silica-modified zirconia support.

[0011] According to a second aspect of the present invention, a dehydrogenation catalyst is provided, which is a cobalt-based catalyst in a single-atom form, and the cobalt-based catalyst comprises: a silica-modified zirconia support in which zirconia as a core is surface-modified with silica; and cobalt as an active metal supported on the silica-modified zirconia support, wherein the cobalt having an oxidation number of 2+ exists in the form of an isolated single atom on the silica-modified zirconia support, and the cobalt having an oxidation number of 2+ forms a tetrahedral structure and is coordinated in a three-membered hydroxyl ring present on the surface of the silica-modified zirconia support.

[0012] According to a third aspect of the present invention, there is provided a method for preparing olefins from paraffins, the method comprising the following steps: providing a supply feedstock containing hard paraffins; subjecting the supply feedstock to a dehydrogenation reaction in the presence of the above-mentioned catalyst at a temperature of 500-700°C and a pressure of 0.3-2 bar; and recovering the olefins corresponding to the hard paraffins in the dehydrogenation reaction product.

[0013] Beneficial Effects

[0014] The dehydrogenation catalyst of a specific embodiment of the present invention uses zirconium oxide (ZrO2) as a core, and uses a support body whose surface or outer part of the zirconium oxide is modified with silicon dioxide (SiO2), and cobalt in the form of a single atom is loaded on the support body. Therefore, due to the good strength or durability of zirconium oxide and the change in the electrical characteristics of the cobalt active site, the long-term reaction stability or regeneration stability can be improved during the dehydrogenation reaction of alkanes, specifically during the dehydrogenation reaction of hard alkanes. In addition, during the preparation of the support body, a small amount of silicon dioxide can be used to modify the surface or outer part of the zirconium oxide core to properties suitable for loading cobalt in the form of a single atom, and in particular, the surface modification can be performed using a low-cost silicon dioxide precursor.

[0015] In addition, the catalyst of the specific embodiment of the present invention can also show good conversion rate and olefin selectivity for the supply feedstock containing high content of paraffin in the dehydrogenation reaction, so it is conducive to commercialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 1 is a schematic diagram showing an exemplary state in which the surface or the outer portion of the zirconia core is surface-modified according to an exemplary embodiment.

[0017] Figure 2 are scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS) images showing xSi@Zr catalysts prepared by varying the content of surface-modified silica on zirconia cores (particle size: 16-40 mesh; volume of 6 milliliters (cc)) to 0 wt %, 2 wt % and 4 wt %, respectively.

[0018] Figure 3 is a graph showing the white line intensity of cobalt K-edge XANES of cobalt single atom catalysts prepared by varying the content of surface-modified silica on zirconia cores (particle size: 16-40 mesh; volume 6 ml) from 1 wt % to 6 wt %.

[0019] Figure 4 is a graph showing the results (conversion, selectivity and yield as a function of time) of the dehydrogenation reaction of propane in the presence of a cobalt single-atom catalyst prepared by varying the content of surface-modified silica on a zirconia core (particle size: 16-40 mesh; volume 6 ml) from 0 wt % to 6 wt %.

[0020] Figure 5 is a graph showing the results (conversion, selectivity and yield according to the number of regeneration cycles) of the dehydrogenation reaction of propane in the presence of a cobalt single atom catalyst supported on a silica-modified zirconia (particle size: 16-40 mesh; volume 6 ml; silica content: 2 wt %). DETAILED DESCRIPTION

[0021] The present invention can be fully realized by the following description. It should be understood that the following description describes preferred specific embodiments of the present invention, and the present invention is not necessarily limited thereto. In addition, it should be understood that the accompanying drawings are used to help understand the present invention, and the present invention is not limited thereto.

[0022] The terms used in this specification can be defined as follows.

[0023] "Heterogeneous catalyst" may refer to a catalyst that exists in a different phase from the reactants during a catalytic reaction, for example, it may refer to a catalyst that is insoluble in the reaction medium. In the case of a heterogeneous catalyst, in order for a reaction to occur, at least one reactant needs to diffuse and adsorb on the surface of the heterogeneous catalyst, and the product after the reaction needs to desorb from the surface of the heterogeneous catalyst.

[0024] The term "support" may refer to a material (typically a solid phase material) having a high specific surface area to which a catalyst active component is attached, and may or may not participate in the catalytic reaction.

[0025] The “zirconia” may include various stoichiometric forms of zirconium oxide, and more typically, may refer to zirconium oxide having a stoichiometric formula of ZrO 2 .

[0026] “Silicon dioxide” may refer to a substance having a tetrahedral structure formed by bonding one silicon atom to four oxygen atoms.

[0027] "Modification" or "surface modification" can be understood to include the concepts of coating and doping. For example, it can be understood to include the presence or exposure of the surface or outer part of the base material (substrate) or matrix in the form of mixing, dispersion, embedding, discontinuous domains such as islands, continuous domains, etc.

[0028] "Heat treatment" is contemplated as intentionally raising the temperature of the whole or a portion thereof and may be accompanied by chemical treatment or further physical treatment as necessary to achieve the desired specific structural and physical properties (or changes).

[0029] “Hard paraffin” may refer to paraffins having 2 to 5 carbon atoms, more specifically, paraffins having 3 and 4 carbon atoms, and specifically, ethane, propane, n-butane, isobutane, pentane, etc. may be exemplified. In addition, “olefins corresponding thereto” may refer to olefins having the same carbon atoms as those obtained by removing hydrogen molecules from hard paraffins in the supply raw material for the dehydrogenation reaction.

[0030] The description of "on" or "upper part" can be understood as being used to describe the concept of relative position. Therefore, it can include not only the situation where other constituent elements or layers exist directly on the described layer, but also the situation where other layers (middle layers) or constituent elements are mixed or exist in the middle. Similarly, the descriptions of "on the lower side", "at the lower part", "below" and "between" can also be understood as relative concepts of position. In addition, the description of "in sequence" can also be understood as the concept of relative position.

[0031] In the present specification, unless otherwise specified, when a component is described as “comprising” or “including” a certain component, it may mean that other components and / or steps are also included.

[0032] Dehydrogenation catalyst and method for preparing the same

[0033] According to a specific embodiment of the present invention, a dehydrogenation reaction is provided which is not only suitable for converting a supply feedstock containing paraffins (specifically, hard paraffins) into olefins corresponding thereto with high conversion rate and high selectivity, but also provides good conversion characteristics for a supply feedstock with a high paraffin content, and in particular provides a single-atom form of cobalt-based catalyst showing improved long-term reaction stability or regeneration stability, specifically, provides a heterogeneous catalyst in which single-atom form of cobalt as an active metal is loaded on a silica-modified zirconia support.

[0034] A. Preparation of Silica-Modified Zirconia Support

[0035] According to a specific embodiment, first, zirconium oxide (ZrO2) can be provided as a substrate material or core constituting a support. To this end, zirconium oxide can be synthesized using a type known in the art or by a known method (e.g., such as liquid phase reaction of rapid precipitation (fastprecipitation), sol-gel, solvent evaporation, hydrothermal treatment, etc. or gas phase reaction such as gas phase chemical synthesis method, etc.), for example, a zirconium oxide precursor (e.g., zirconium n-pentoxide (IV)) can be hydrolyzed in an alcohol solvent to synthesize zirconium oxide. In addition, zirconium oxide can show crystallinity, can be divided into monoclinic structure (m-ZrO2), tetragonal structure (t-ZrO2), cubic structure (c-ZrO2), etc., and zirconium oxide known in the art or commercially available can be used without restriction in this specific embodiment.

[0036] In this regard, the mechanical and physical properties of zirconium oxide and silicon dioxide can be exemplified as shown in the following Table 1 (AZO Materials, https: / / www.azom.com).

[0037] [Table 1]

[0038]

[0039] As can be seen from the above table, zirconium oxide can have good mechanical and physical properties compared to silicon dioxide. Therefore, it can suppress the decrease in strength under high temperature environments such as the dehydrogenation reaction of paraffins, stably maintain the catalyst activity under repeated reaction cycles, and help suppress the aggregation of cobalt single atoms. Furthermore, by changing the electronic properties of the active sites of cobalt in the form of supported single atoms, an effect that is beneficial to the dehydrogenation reaction can be provided.

[0040] In an exemplary embodiment, the BET specific surface area of ​​zirconium oxide used for the support body may be, for example, about 10-300 m 2 / g, specifically about 20-150m 2 / g, more specifically about 30-100 m 2 / g, the pore size of the zirconium oxide may be, for example, in the range of about 5-40 nm, specifically in the range of about 10-30 nm, more specifically in the range of about 15-25 nm. In addition, the pore volume of the zirconium oxide may be, for example, in the range of about 0.1-1 cm 3 / g, specifically about 0.2-0.5cm 3 / g, more specifically about 0.25-0.3 cm 3 / g. The properties of this zirconium oxide are factors that affect the content of cobalt single atoms and thermal stability, so it may be beneficial to adjust it within the above range. However, the present invention is not limited thereto.

[0041] According to a specific embodiment, after providing zirconium oxide as a core, a step of modifying the surface of zirconium oxide with silicon dioxide can be performed. At this time, the surface modification by silicon dioxide can be performed based on a known method using a silicon dioxide precursor. For example, an impregnation method (specifically an incipient wetness impregnation method), sol-gel, etc. can be used.

[0042] The method of surface modification of silica on zirconium oxide can be exemplified as follows, but the present invention is not necessarily limited thereto.

[0043] First, a silica precursor (or silicon source) can be dissolved in a water-based medium to prepare a silica precursor aqueous solution. At this time, the water-based medium can be water, specifically distilled water. In addition, the concentration of the silica precursor solution can be adjusted in the range of, for example, about 5-80% (weight / weight (w / w)), specifically in the range of about 10-70% (w / w), and more specifically in the range of about 15-60% (w / w).

[0044] According to an exemplary specific embodiment, the silica precursor may use a soluble silicate, for example, an alkali metal silicate, specifically, an inexpensive precursor or compound such as sodium silicate (or water glass), potassium silicate, etc. Alternatively, an alkoxysilane represented by Si(OR)4 may be used as a silica precursor, for example, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, butyltrimethoxysilane, isobutyltriethoxysilane, hexyltriethoxysilane, oxytriethoxysilane, etc. may also be used.

[0045] Then, the silica precursor aqueous solution and zirconium oxide can be combined to prepare a water-based dispersion. According to an exemplary specific embodiment, when the silica precursor aqueous solution and zirconium oxide are combined, the weight ratio of silica precursor: zirconium oxide can be adjusted to, for example, 1: in the range of about 0.1-50, specifically 1: in the range of about 1-35, more specifically 1: in the range of about 3-25. At this time, the contact temperature between the silica precursor aqueous solution and zirconium oxide is not particularly limited, but can be, for example, at about 10-80 ° C, specifically at about 15-50 ° C, more specifically at room temperature. In addition, the combination or contact can be representatively carried out for about 0.5-5 hours, more representatively for about 1-2 hours, and can be carried out under stirring or without stirring. Zirconium oxide loaded with silica precursor can be formed by this process.

[0046] According to an exemplary specific embodiment, the zirconium oxide loaded with a silica precursor can be obtained by subjecting the zirconium oxide dispersion loaded with a silica precursor to a usual post-treatment step, for example, separation (e.g., filtration, standing, etc.) and / or purification step, specifically removal of the silica precursor solution, washing (specifically water washing) and / or drying (e.g., drying under an inert gas (e.g., nitrogen) atmosphere).

[0047] Afterwards, the zirconium oxide loaded with the silica precursor may be heat-treated to convert the loaded silica precursor into an oxide form, i.e., silica, and as a result, a silica-modified zirconium oxide as a support may be prepared. Exemplarily, the heat treatment may be carried out at a temperature of about 500-1200° C., specifically at a temperature of about 600-1100° C., more specifically at a temperature of about 700-1000° C., for example, for about 1-12 hours, specifically about 2-9 hours, more specifically about 3-5 hours. At this point, the heat treatment may be carried out in an oxygen-containing atmosphere, for example, in an air atmosphere, and the heating rate may be adjusted, for example, in the range of about 0.1-30° C. / minute, specifically in the range of about 1-20° C. / minute, and more specifically in the range of about 2-10° C. / minute.

[0048] In this regard, the amount of silica in the silica-modified zirconia support can be determined, for example, in the range of about 0.5-10 wt%, specifically in the range of about 1-6 wt%, more specifically in the range of about 1.5-4 wt%, and particularly specifically in the range of about 2-3.5 wt%. At this time, when the amount of silica is too small, the phenomenon of reduced propylene selectivity is induced, and when the amount of silica is too large, the propane conversion rate may be reduced, so it may be beneficial to adjust the amount of silica to an appropriate amount within the above range. However, this numerical range can be understood as exemplary.

[0049] On the other hand, the silica present on the surface or outside of the zirconia core in the silica-modified zirconia support may be in various forms. However, in order to support cobalt in the form of single atoms in the subsequent process, it is preferred that at least a portion of the silica is exposed to the outside. In an exemplary embodiment, the silica is Figure 1As shown, it can be formed into a discontinuous domain morphology (e.g., an island morphology). At this time, the size of the silicon dioxide domain can be adjusted in a range of, for example, less than about 50 nm, specifically less than about 20 nm, and more specifically less than about 10 nm. The size of the silicon dioxide domain can vary according to the amount of silicon dioxide loaded on the zirconium oxide core. When the silicon dioxide loading exceeds a certain level, the domain size will also increase (e.g., about 20 nm or more), which may have an adverse effect on the improvement of the conversion rate and / or selectivity during the dehydrogenation reaction (specifically, the dehydrogenation reaction of propane).

[0050] Furthermore, according to exemplary embodiments, zirconium oxide modified with silica may exhibit a higher specific surface area under heat treatment compared to unmodified zirconium oxide (e.g., may increase by at least about 30%, specifically by at least about 40%, and more specifically by at least about 50%), which may be considered to be a result of increased thermal stability of zirconium oxide due to the introduction of silica.

[0051] B. Loading cobalt in single atomic form

[0052] According to a specific embodiment of the present invention, silica-modified zirconia can be used as a support for a single-atom cobalt-based catalyst. In this regard, by surface-modifying zirconia with silica, the negatively charged SiO2 on the surface of silica (e.g., silica domains) exposed on the zirconia core can be - The cobalt ions with an oxidation number of 2+ are combined in an isolated single atom form through electrostatic interaction or adsorption. The present invention is not limited to a specific theory, but as shown in Table 2 below, although the isoelectric point of the zirconia support is higher than the isoelectric point of silicon dioxide of about 2, the zirconia support also has an isoelectric point of about 4, which is lower than other metal oxides, so it is judged that it may be beneficial to load cobalt under alkaline conditions. In addition, it is judged that the thermal stability / mechanical stability of zirconia is good compared with silicon dioxide, so the cobalt single atom active site formed on the support is also more stable.

[0053] [Table 2]

[0054] Metal oxides Isoelectric Point Silicon dioxide 2 Zirconia 4 Titanium Dioxide (Anatase) 3.5 Titanium Dioxide (Rutile) 6.5 Alumina 8-9

[0055] Furthermore, in this specific embodiment, zirconium oxide is used as the core, so cobalt can be effectively induced to be loaded in a single atomic form through silicon dioxide domains having appropriate morphology and size, and due to the excellent thermal stability of the support, cobalt can be stably maintained in a single atomic form without agglomeration or aggregation.

[0056] At this time, the cobalt in the form of a single atom is coordinated by forming a tetrahedral structure in a three-membered hydroxyl ring through three hydroxyl groups on the surface of the silica in the support. The support of the cobalt in the form of a single atom can be performed as follows.

[0057] Prepare the water-based dispersion of the silica-modified zirconia support. At this time, the water-based medium used to prepare the dispersion (dispersion liquid) can be water, specifically distilled water, and the content of the silica-modified zirconia support in the water-based dispersion can be, for example, in the range of about 1-30 weight %, specifically in the range of about 3-20 weight %, and more specifically in the range of about 5-10 weight %.

[0058] On the other hand, an alkali component is added to the water-based dispersion of the silica-modified zirconia support to prepare a pH-adjusted silica-modified zirconia dispersion, and the pH of the water-based dispersion of the silica-modified zirconia can be adjusted to, for example, at least about 10, specifically at least about 11, more specifically within the range of about 10.5-11.5. The reason for increasing the pH of the dispersion is to deprotonate the surface of the silica exposed to the zirconia, specifically, hydrogen ions can be removed from the hydroxyl groups present on the surface of the silica to make it negatively charged. That is, the ions are not adsorbed and retain the hydroxyl groups at the zero charge point of the silica, so the silica surface can be deprotonated by adjusting the pH to make it display a negative charge. As a result, the hydroxyl anions on the surface of the deprotonated silica and the hydroxyl groups present on the surface of the silica, specifically the trivalent hydroxyl groups, form 3 hydroxyl anions in the alkaline water-based medium, which can correspond to the position where the cobalt is fixed in the form of a single atom in the subsequent steps.

[0059] According to an exemplary specific embodiment, the alkali component can be, for example, an aqueous solution of sodium hydroxide, potassium hydroxide, ammonium hydroxide, etc., specifically, an alkali containing ammonium is used, and more specifically, ammonium hydroxide (ammonia water) is used. At this time, as the added alkali, it is preferred to use a type that does not cause precipitation when combined or mixed with the aqueous solution of the cobalt precursor.

[0060] On the other hand, according to a specific embodiment of the present invention, in addition to the step of preparing the pH-adjusted aqueous dispersion of silica-modified zirconia, a step of preparing an aqueous solution of a cobalt precursor and adding an alkali component to prepare the pH-adjusted aqueous solution of a cobalt precursor may be additionally performed.

[0061] In this regard, the cobalt precursor may be a precursor containing a cobalt (Co(III)) complex ion having an oxidation number of 3+, for example, Co(NH3)6Cl3 may be used directly, or a precursor containing a cobalt complex ion obtained by treating at least one cobalt compound (precursor) selected from Co(NO3)2, CoCl2, Co(acac)3, etc. with ammonia water and filtering. However, in order to smoothly form a cobalt single atom catalyst, it is preferred to use Co(NH3)6Cl3 as a precursor that can minimize the preparation steps.

[0062] In an exemplary embodiment, the concentration of the cobalt precursor in the aqueous precursor solution may be, for example, in the range of about 0.1-20 wt %, specifically in the range of about 0.5-10 wt %, and more specifically in the range of about 1-5 wt %.

[0063] In addition, the pH of the cobalt precursor solution can be adjusted by adding an alkali component, which can also stably maintain the surface of the silica exposed on the support in a deprotonated state (i.e., a modified state so as to have a negative charge) when combined with the pH-adjusted silica-modified zirconia aqueous dispersion in a subsequent step, thereby reducing the cobalt ions (Co) of the positively charged precursor. 3+ ) can be fixed on the silica surface of the silica-modified zirconia support by electrostatic adsorption.

[0064] At this time, the alkali component can select and use at least one of the types described in connection with the preparation of the above-mentioned water-based dispersion. Exemplarily, all the same alkali components or alkali compounds can be used. However, the alkali component preferably uses a type that does not cause precipitation when mixed with the aqueous solution of the cobalt precursor as described above. In addition, according to an exemplary specific embodiment, by adding an alkali component, the pH of the cobalt precursor aqueous solution can be adjusted to, for example, at least about 10, specifically at least about 11, more specifically within the range of about 10.5-11.5.

[0065] When preparing the aqueous solution of the Co(III) precursor adjusted by pH, a step of combining with the aqueous dispersion of the silica-modified zirconia adjusted by pH is performed. At this time, the mixing ratio of the aqueous solution of the cobalt precursor adjusted by pH and the aqueous dispersion of the silica-modified zirconia adjusted by pH can be determined by considering the amount of cobalt ions in the aqueous solution of the cobalt precursor fixed in the form of single atoms (specifically, in the form of single atoms of a single layer) on the surface of the silica in the silica-modified zirconia support.

[0066] In this regard, the cobalt ions can be loaded on the silica surface of the silica-modified zirconia support in an amount equivalent to about 0.1-2% by weight, specifically about 0.15-1% by weight, and more specifically about 0.2-0.4% by weight, but the cobalt precursor actually used cannot be completely fixed on the silica surface of the silica-modified zirconia support, so an excess of cobalt (Co(III)) precursor can be dissolved compared to the theoretical amount. In an exemplary embodiment, the mixing ratio of the cobalt precursor aqueous solution and the water-based dispersion of the silica-modified zirconia can be adjusted based on the weight of the silica-modified zirconia, so that the cobalt precursor can be in the range of about 0.1-10% by weight, specifically in the range of about 0.5-8% by weight, and more specifically in the range of about 1-6% by weight.

[0067] According to an exemplary embodiment, the combination of two water-based fluids (water-based dispersion of silica-modified zirconia and aqueous solution of cobalt precursor) can be carried out under stirring, and the stirring speed can be, for example, in the range of about 200-500 rpm, specifically in the range of about 250-400 rpm, and the stirring time can be, for example, at least about 3 minutes, specifically at least about 5 minutes, more specifically in the range of about 5-10 minutes, but it is not necessarily limited to the above conditions. In addition, the temperature during the combination is not particularly limited, and can be set to, for example, about 10-40°C, specifically about 20-30°C, and more specifically room temperature.

[0068] Then, the cobalt ions that are not adsorbed on the surface of the silica-modified zirconia support are removed as completely as possible. This is different from the impregnation loading method, which is to retain only the cobalt (or Co) fixed in the form of single atoms on the silica surface through electrical interaction. 3+ ) and remove the remaining cobalt. When the cobalt precursor is attached to the surface of silica in a bulk state as in the conventional impregnation method, phenomena such as reduction and aggregation that reduce activity may occur in the dehydrogenation reaction.

[0069] Taking the above into consideration, in an exemplary embodiment, the solids in the combined dispersion (a silica-modified zirconia support on which a cobalt precursor is adsorbed (fixed)) can be separated by a conventional solid-liquid separation process such as settling, filtering, etc., and if necessary, the process of adding water, specifically distilled water, to the separated solids and stirring can be repeated to separate the solids again.

[0070] In addition, the separated solid can be washed at least once with water, specifically with distilled water, specifically, washed multiple times, so as to completely remove the unadsorbed and residual cobalt precursor as much as possible. Thereafter, the obtained solid is dried, and the drying temperature is not particularly limited, and can be set to, for example, about 10-40° C., specifically about 20-30° C., and more specifically room temperature. At this time, the oxidation state of the cobalt ion is still maintained at +3.

[0071] As a subsequent step, the silica-modified zirconia support on which cobalt ions are adsorbed (fixed) is heat-treated to convert it into a dehydrogenation catalyst. At this time, the heat treatment can be carried out in an oxygen-containing atmosphere, and the heat treatment temperature can be set, for example, in the range of about 250-1000°C, specifically in the range of about 275-800°C, and more specifically in the range of about 300-600°C. In this specific embodiment, the silica-modified zirconia support on which cobalt is adsorbed (fixed) is heat-treated, so that the cobalt with an oxidation value of 3+ adsorbed on the silica surface of the support can be converted into cobalt with an oxidation value of 2+. In addition, the heating rate during the heat treatment process can be determined, for example, in the range of about 0.1-20°C / minute, specifically in the range of about 1-10°C / minute, and more specifically in the range of about 2-5°C / minute.

[0072] However, optionally, an additional drying step may be performed before the heat treatment step in the oxygen-containing atmosphere, and in this case, the additional drying temperature may be, for example, in the range of about 50-150° C., specifically in the range of about 120-150° C. In this relatively high temperature drying process, at least a portion of the cobalt present with an oxidation number of 3+ may be partially reduced to cobalt with an oxidation number of 2+ in advance.

[0073] In this regard, the present invention is not limited to a specific theory, but the reason why the oxidation value of cobalt is maintained at 2+ after heat treatment can be explained as follows.

[0074] When cobalt is 3+, it occupies 6 electrons in the outermost orbit, so it can only form an octahedral with 6 bonds. In addition, when cobalt is 2+, there are 7 electrons in the outermost orbit, so it mainly forms a tetrahedral, but as in the case of CoO, an octahedral can also be formed. In the case of this specific embodiment, it is necessary to combine with the trivalent hydroxyl group in structure, so it can be seen that it changes to 2+ in order to form a tetrahedral structure. On the other hand, it is judged that if it is to exist as 3+ again, it needs to cooperate with the surrounding to form an octahedron, but silicon (Si) is an element that does not have other structures except tetrahedrons, so it does not conform to the surrounding environment and cannot be converted into 3+ cobalt. In addition, it is judged that the deactivation is due to the fact that the connection (communication) with Si is cut off and condensed with Co metal alone, so when it contacts with oxygen to form an oxide, it may become Co3O4 containing 3+ cobalt.

[0075] In addition, the heat treatment time is not particularly limited as long as it is sufficient time to convert 3+ cobalt into 2+ cobalt, but can be, for example, in the range of about 2-12 hours, specifically in the range of about 2.5-8 hours, and more specifically in the range of about 3-4 hours.

[0076] In the above-mentioned heat treatment step, since the cobalt with an oxidation value of 2+ is heated to above the predetermined temperature, even if the heat treatment is continued in an oxygen-containing (or oxidizing) atmosphere (or calcining atmosphere), it will not be converted again into cobalt with an oxidation value of 3+, because it needs to maintain a tetrahedral structure as a single atom. In addition, even if the catalyst is used in a dehydrogenation reaction operated above a predetermined temperature, this oxidation state will not change, which shows that the catalyst of this specific embodiment has resistance to reduction. In particular, the cobalt single atom catalyst according to a specific embodiment provides favorable characteristics in terms of long-term reaction stability or regeneration stability during the dehydrogenation reaction by forming a base structure of silicon dioxide (specifically, silicon dioxide domains) with zirconium oxide.

[0077] The present invention is not limited to a particular theory, and the cobalt in the catalyst remains in a single atomic form, but as the electrical properties of the cobalt active site change due to the presence of the substrate zirconium oxide, it can be considered that the activity, selectivity and / or stability are adjusted to be favorable for the dehydrogenation reaction described later. That is, when only zirconium oxide is used as a support, the electron density of the cobalt single atom is low, so the cobalt is strongly adsorbed on the reactant / product, resulting in an increase in propane conversion and a decrease in propylene selectivity, thereby increasing the formation of coke. However, the electron density of the cobalt single atom formed by combining silica on the zirconium oxide core increases, and the cobalt is relatively weakly adsorbed on the reactant / product, resulting in a decrease in propane conversion and an increase in propylene selectivity, and the formation of coke can also be suppressed.

[0078] According to exemplary embodiments, the content (loading amount) of cobalt in the dehydrogenation catalyst may be, for example, in the range of about 0.05-2 wt %, specifically in the range of about 0.1-1.5 wt %, more specifically in the range of about 0.15-1 wt %, and particularly specifically in the range of about 0.2-0.4 wt %.

[0079] Dehydrogenation reaction

[0080] According to another specific embodiment of the present invention, a process is provided for converting paraffins, specifically hard paraffins (more specifically hard paraffins with carbon atoms of 2 to 5) into corresponding olefins by dehydrogenation reaction using the above-mentioned cobalt-based catalyst in single atom form. In particular, the hard paraffins may contain propane. For this, the supply raw material may be provided in gas phase.

[0081] At this point, it should be noted that when the above catalyst is applied, good conversion and selectivity can be achieved even with a feedstock having a high paraffin content. Exemplarily, the paraffin content in the feedstock can be, for example, at least about 50% by volume, specifically at least about 70% by volume, more specifically at least about 80% by volume, and further can be a level exceeding about 99% by volume. This is different from the case where a feedstock containing up to about 20% by volume of paraffin is subjected to a dehydrogenation reaction in experiments related to existing single-atom catalysts (e.g., Zn catalysts).

[0082] In the dehydrogenation reaction of the exemplary embodiment, the reaction temperature can be, for example, in the range of about 500-700° C., specifically in the range of about 550-650° C., more specifically in the range of about 570-620° C., and the reaction pressure can be, for example, in the range of about 0.3-2 bar (bar), specifically in the range of about 0.4-1.5 bar, more specifically in the range of about 0.5-1 bar. In addition, the gas hourly space velocity (GHSV) under standard conditions can be, for example, in the range of about 100-2000 hours (hr) -1 In the range of about 200-1500 hours -1 In the range of about 300-1000 hours -1 The above-mentioned dehydrogenation reaction conditions can be changed by taking into account the type of paraffin in the supply raw material, the loading amount of the active metal (cobalt) in the catalyst, etc.

[0083] According to exemplary embodiments, in the dehydrogenation reaction process, the conversion rate and the selectivity can be, for example, at a level of at least about 30% (specifically at least about 40%, more specifically at least about 45%), and can be at a level of at least about 70% (specifically at least about 80%, specifically at least about 85%), respectively.

[0084] The present invention can be more clearly understood according to the following examples. The following embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0085] Example

[0086] The conversion rate and selectivity of propane in this example are calculated according to the following Mathematical Formula 1 and Mathematical Formula 2.

[0087] [Mathematical formula 1]

[0088]

[0089] [Mathematical formula 2]

[0090]

[0091] Preparation Example 1

[0092] First, commercially available zirconium oxide (SZ31164 from Saint-Gobain; specific surface area: 85 m 2 / g, pore volume: 0.29cm 3 / g, pore size: 8.60nm) as cores, and five batches of zirconia (zirconia particle size: 16-40 mesh; volume: 6 ml) were prepared in 10g.

[0093] In addition, in a beaker, 0.483 g, 0.966 g, 1.449 g, 1.932 g and 2.898 g of Na2SiO3·9H2O were dissolved in 4 ml of distilled water, respectively, so that the content of silica mixed into the prepared zirconium oxide was 1 weight %, 2 weight %, 3 weight %, 4 weight % and 6 weight %, respectively, to prepare a silica precursor aqueous solution.

[0094] Then, the silica precursor aqueous solution was added to 10 g of the zirconia prepared above, and then mixed with a roller mixer for 1 hour, and then dried in an oven at 80° C. to obtain zirconia loaded with silica precursor.

[0095] The silica-precursor-supported zirconia obtained as described above was heated to 750°C at a heating rate of 5°C / min, and then heat-treated in air for 3 hours to prepare 1 wt%, 2 wt%, 3 wt%, 4 wt% and 6 wt% silica-modified zirconia supports, respectively. According to the silica content, they were named 1Si@Zr, 2Si@Zr, 3Si@Zr, 4Si@Zr and 6Si@Zr, respectively.

[0096] Preparation Example 2

[0097] 10 g of the xSi@Zr (x=1, 2, 3, 4, 6) support prepared in Preparation Example 1 was dispersed in 100 ml of distilled water, 28 wt % of concentrated aqueous ammonia (SAMCHUN CHEMICALS) was added, and the pH of the dispersion was adjusted to 11 to prepare pH-adjusted xSi@Zr (x=1, 2, 3, 4, 6) water-based dispersions.

[0098] In addition, in a beaker, 0.5 g of a cobalt precursor (Co(NH3)6Cl3) was dissolved in 50 ml of distilled water, and 28 wt% of concentrated ammonia water (SAMCHUN CHEMICALS) was added to adjust the pH to 11 to prepare pH-adjusted cobalt precursor aqueous solutions.

[0099] Then, the pH-adjusted cobalt precursor aqueous solution was quickly added to the pH-adjusted xSi@Zr aqueous dispersion and stirred at room temperature for 30 minutes. The stirred sample was allowed to stand for 5 minutes, and then the liquid phase was discarded, and then 200 ml of distilled water was poured again and stirred for 10 minutes, and then the sample was filtered under reduced pressure and washed several times with distilled water.

[0100] The filtered samples were dried at room temperature and then dried again at 125° C. The dried samples were heated to 300° C. at a heating rate of 5° C. / min and then heat-treated in air for 3 hours to prepare dehydrogenation catalysts (Co / 1Si@Zr catalyst, Co / 2Si@Zr catalyst, Co / 3Si@Zr catalyst, Co / 4Si@Zr catalyst and Co / 6Si@Zr catalyst).

[0101] Comparative Preparation Example 1

[0102] 10 g of commercially available zirconium oxide (SZ31164 from Saint-Gobain; specific surface area: 85 m 2 / g, pore volume: 0.29cm 3 / g, pore size: 8.60nm) (zirconia particle size: 16-40 mesh; volume of 6 ml) was dispersed in 100 ml of distilled water, and 28 wt% of concentrated ammonia water (SAMCHUNCHEMICALS) was added to the zirconium oxide water-based dispersion, and the pH of the dispersion was adjusted to 11 to prepare a pH-adjusted zirconium oxide water-based dispersion.

[0103] Separately, in a beaker, 0.5 g of a cobalt precursor (Co(NH 3 ) 6 Cl 3 ) was dissolved in 50 ml of distilled water, 28 wt % of concentrated aqueous ammonia (SAMCHUN CHEMICALS) was added, and the pH was adjusted to 11 to prepare a pH-adjusted aqueous cobalt precursor solution.

[0104] Then, the pH-adjusted cobalt precursor aqueous solution was quickly added to the pH-adjusted zirconium oxide aqueous dispersion and stirred at room temperature for 30 minutes. The stirred sample was allowed to stand for 5 minutes, and then the liquid phase was discarded, and then 200 ml of distilled water was poured again and stirred for 10 minutes, and then the sample was filtered under reduced pressure and washed several times with distilled water.

[0105] The filtered sample was dried at room temperature and then dried again at 125° C. The dried sample was heated to 300° C. at a heating rate of 5° C. / min and then heat-treated in air for 3 hours to prepare a dehydrogenation catalyst (Co / Zr catalyst).

[0106] The silica content and cobalt content in the catalysts (Co / Zr, Co / 1Si@Zr, Co / 2Si@Zr, Co / 3Si@Zr, Co / 4Si@Zr and Co / 6Si@Zr) prepared in Preparation Example 2 and Comparative Preparation Example 1 were analyzed by inductively coupled plasma optical emission spectroscopy (ICP-OES), and the results are shown in Table 3 below.

[0107] [Table 3]

[0108] catalyst <![CDATA[SiO2 content (wt%)]]> Co content (weight %) Co / Zr 0 0.2 Co / 1Si@Zr 0.8 0.2 Co / 2Si@Zr 1.5 0.2 Co / 3Si@Zr 2.8 0.2 Co / 4Si@Zr 3.9 0.2 Co / 6Si@Zr 5.6 0.2

[0109] Experimental Example 1

[0110] The domain sizes of the silicon dioxide of Zr, 2Si@Zr and 4Si@Zr prepared in this experimental example were analyzed by scanning transmission electron microscopy-energy dispersive spectroscopy (STEM-EDS), and the results are shown in Figure 2 middle.

[0111] According to the above-mentioned figures, when 4 wt% or more of silica is introduced, silica domains with a size in the range of 20-50 nm are observed. On the other hand, when less than 4 wt% of silica is contained, no silica domains with a size in the range of 20-50 nm are observed by STEM-EDS, indicating that the size of the silica domains is less than 20 nm.

[0112] Experimental Example 2

[0113] In this experimental example, the trend of change in specific surface area according to the introduction of silica into zirconium oxide and heat treatment was analyzed, and the results are shown in Table 4. The analysis was measured using a Micromeritics 3felx device, and all samples were degassed at 573K for 12 hours before analysis. The nitrogen adsorption-desorption isotherm was measured at liquid nitrogen temperature (77K). The measurement results confirmed that the specific surface area of ​​zirconium oxide introduced with silica after heat treatment at 1023K was higher than that of zirconium oxide without silica.

[0114] [Table 4]

[0115]

[0116]

[0117] Experimental Example 3

[0118] In this experimental example, the intensity of the white line of the Co K-edge XANES spectrum of Co / xSi@Zr (x=1-6) generated by introducing silicon dioxide into zirconium oxide was compared, thereby comparing the electron density of cobalt single atoms. The results are shown in Figure 3 At this time, the analysis was performed at the 8C beamline of the Pohang Accelerator Laboratory (PAL).

[0119] With reference to the above-mentioned figures, it was confirmed that the intensity of the white line of the cobalt K-edge XANES gradually decreased as the silicon dioxide content increased, thereby confirming that the electron density of the cobalt single atom increased.

[0120] Experimental Example 4

[0121] In this experimental example, a dehydrogenation reaction for synthesizing olefins from a reactant gas containing a high content of chain alkanes was carried out in the presence of cobalt-based catalysts (Co / Zr, Co / 1Si@Zr, Co / 2Si@Zr, Co / 3Si@Zr, Co / 4Si@Zr and Co / 6Si@Zr) prepared in Preparation Example 2 and Comparative Preparation Example 1, respectively.

[0122] The dehydrogenation reaction for evaluating the catalyst was carried out using a 3 / 4 inch quartz tube reactor (the diameter of the catalyst loading area was 3 / 4 inch, and the diameter of the tube outside was 1 / 4 inch). The flow rates of each gas were adjusted using a mass flow controller, and the product gas passing through the reactor was analyzed by an online gas chromatograph (50 m HP-PLOT column).

[0123] 6 ml of catalyst was weighed and supported at the center of the reaction tube with a quartz wool support, and then N2 (99.999%, DIGAIRGAS) was introduced at a flow rate of 100 ml / min, and the temperature was raised from room temperature to 590°C at a rate of 5°C / min. Thereafter, the same temperature was maintained for 1 hour for stabilization.

[0124] For the dehydrogenation reaction of paraffins, 99.5% propane (RIGAS) was introduced as a reactant gas at 20 ml / min, and N2 (99.999%, DIG AIRGAS) was introduced at 30 ml / min, so that the molar fraction of propane in the supplied raw material was 40%. The reaction was carried out at 590°C and normal pressure, and the composition of the product gas passing through the reactor was analyzed by a flame ionization detector (FID) at intervals of 15 minutes. After reacting for 1 hour, the catalyst was regenerated in an air atmosphere at the same temperature for 30 minutes, and N2 (99.999%, DIG AIRGAS) was introduced for 15 minutes between the reaction and the regeneration. The reaction results (conversion rate, selectivity and yield according to time) are shown in Figure 4 In this case, according to the time, every 4 points constitute a cycle. After measuring 4 points (1 hour), regeneration is performed, and the subsequent 4 points measured constitute the next cycle. Therefore, the first point of each of the 4 points is equivalent to the initial conversion rate / selectivity / yield.

[0125] Referring to the attached figure, the results of the dehydrogenation reaction showed that the initial conversion rate was 80%, which was very high, but the propylene selectivity was 30%, which was low, when the cobalt-supported catalyst (Co / Zr) prepared by using the zirconia support without silica modification was used. In addition, as the regeneration proceeded, it decreased to 60%, and the initial conversion rate also decreased.

[0126] On the other hand, when the silica content in the silica-modified zirconia support was 2 wt% (Co / 2Si@Zr), the initial conversion was at a level of approximately 46%, but the selectivity was at a level of 90%, and no decrease in the initial conversion and selectivity was observed despite the regeneration of the catalyst.

[0127] In addition, when the silica content in the silica-modified zirconia support was 4 wt% (Co / 4Si@Zr), the selectivity was maintained but the conversion rate gradually decreased. When the silica content was 6 wt% (Co / 6Si@Zr), a further decrease in the conversion rate was observed.

[0128] Experimental Example 5

[0129] In this experimental example, 200 propane dehydrogenation reactions and catalyst regeneration experiments were conducted in the presence of the Co / 2Si@Zr catalyst that showed the best results in Experimental Example 1. Similar to the commercial propane dehydrogenation process (Catofin), the reaction was carried out for 15 minutes, and then the catalyst was regenerated for 15 minutes in an air atmosphere at the same temperature, and N2 (99.999%, DIGAIRGAS) was introduced for 15 minutes between the reaction and regeneration. The results of the 200 catalytic reactions-regeneration are shown in Figure 5 middle.

[0130] With reference to the above-mentioned figures, it can be confirmed that the conversion rate and the selectivity remain constant regardless of the recycling of the catalyst.

[0131] Those skilled in the art may easily utilize simple modifications or changes of the present invention, and it is considered that such modifications or changes belong to the scope of the present invention.

Claims

1. A method for preparing a cobalt-based catalyst in single-atom form, comprising the following steps: a) modifying the surface or outer portion of zirconium oxide with silicon dioxide to prepare a silicon dioxide-modified zirconium oxide support; b) preparing a water-based dispersion of the silica-modified zirconia support; c) adding an alkali component to the water-based dispersion of the silica-modified zirconia support to adjust the pH to at least 10, thereby preparing a pH-adjusted water-based dispersion of the silica-modified zirconia support; d) separately preparing an aqueous solution of a cobalt precursor having an oxidation number of 3+, and adding an alkali component to prepare a pH-adjusted aqueous solution of the cobalt precursor; e) preparing an aqueous dispersion in which at least a portion of the cobalt ions having an oxidation number of 3+ are adsorbed on the surface of the silica-modified zirconia support by combining the pH-adjusted aqueous dispersion of the silica-modified zirconia support and the pH-adjusted aqueous solution of a cobalt precursor; f) removing cobalt ions that are not adsorbed on the surface of the silica-modified zirconia support; and g) heat treating the silica-modified zirconia support having adsorbed cobalt ions obtained in step f); wherein the cobalt with an oxidation number of 2+ in the cobalt-based catalyst exists in the form of an isolated single atom on the silica-modified zirconia support, and the cobalt with an oxidation number of 2+ forms a tetrahedral structure and is coordinated in a three-membered hydroxyl ring existing on the surface of the silica-modified zirconia support, The content of silicon dioxide in the silicon dioxide-modified zirconia support is more than 1 wt % and less than 6 wt %. The cobalt precursor in step d) is a precursor containing a cobalt complex ion having an oxidation number of 3+.

2. The method according to claim 1, characterized in that The BET specific surface area of ​​the zirconium oxide is 10-300m 2 In the range of 200 μm / g, the pore size of the zirconium oxide is determined to be in the range of 5-40 nm.

3. The method according to claim 2, characterized in that The pore volume of the zirconium oxide is 0.1-1cm 3 / g is determined within the range.

4. The method according to claim 1, characterized in that: The step a) is performed by an impregnation method.

5. The method according to claim 4, characterized in that The step a) comprises the following steps: a1) dissolving a silicon dioxide precursor in a water-based medium to prepare a silicon dioxide precursor aqueous solution having a concentration of 5-80 wt %; a2) combining the aqueous solution of silica precursor and zirconium oxide to prepare a water-based dispersion of zirconium oxide loaded with silica precursor; a3) separating the silica precursor-loaded zirconium oxide from the silica precursor-loaded zirconium oxide aqueous dispersion; and a4) heat-treating the zirconium oxide supporting the silica precursor at 500-1200° C. in an oxygen-containing atmosphere.

6. The method according to claim 1, characterized in that The silica-modified zirconia support has a morphology in which at least a portion of silica is exposed outside of zirconia.

7. The method according to claim 6, characterized in that The silica exposed to the outside of the silica-modified zirconia support has a discontinuous domain morphology.

8. The method according to claim 7, characterized in that The domain size is less than 50 nm.

9. The method according to claim 1, characterized in that: The concentration of the water-based dispersion of the silica-modified zirconia support prepared in step b) is in the range of 1-30 wt %.

10. The method according to claim 1, characterized in that The alkali components used in the step c) and the step d) are the same or different, and the alkali component is at least one selected from sodium hydroxide, potassium hydroxide and ammonium hydroxide.

11. The method according to claim 1, characterized in that: The concentration of the cobalt precursor in the cobalt precursor aqueous solution is in the range of 0.1-20 wt %.

12. The method according to claim 1, characterized in that The silica-modified zirconia support body on which the cobalt ions are adsorbed has the cobalt ions loaded in an amount of 0.1-2 wt % on the silica surface of the zirconia support body.

13. The method according to claim 11, characterized in that The cobalt precursor may be directly Co(NH3)6Cl3 or a precursor containing cobalt complex ions obtained by treating at least one cobalt compound selected from Co(NO3)2, CoCl2 and Co(acac)3 with aqueous ammonia and then filtering the resultant.

14. The method according to claim 1, characterized in that The heat treatment is performed in an oxygen-containing atmosphere at a temperature of 250-1000°C.

15. A dehydrogenation catalyst, which is a cobalt-based catalyst in single-atom form, the cobalt-based catalyst comprising: A silica-modified zirconia support in which zirconia as a core is surface-modified with silica; and Cobalt as an active metal supported on the silica-modified zirconia support, in, Cobalt having an oxidation number of 2+ exists on the silica-modified zirconia support in the form of an isolated single atom, and the cobalt having an oxidation number of 2+ forms a tetrahedral structure and is coordinated in a three-membered hydroxyl ring existing on the surface of the silica-modified zirconia support, The content of silica in the silica-modified zirconia support is more than 1 wt % and less than 6 wt %.

16. The dehydrogenation catalyst according to claim 15, characterized in that The cobalt content in the catalyst is in the range of 0.05-2 wt%.

17. A method for preparing olefins from paraffins, comprising the following steps: Providing a supply of raw materials containing hard paraffins; Dehydrogenating the feedstock in the presence of the catalyst of claim 15 or 16 at a temperature of 500-700° C. and a pressure of 0.3-2 bar; as well as The olefins corresponding to the hard paraffins in the dehydrogenation reaction product are recovered, and the hard paraffins are paraffins having 2 to 5 carbon atoms.

18. The method for preparing olefins from paraffins according to claim 17, characterized in that: The content of hard paraffins in the supplied raw material is at least 50 volume %.