Application of reverse supported catalysts in Fenton-like catalytic degradation of pollutants
The combination of the reverse-supported catalyst prepared by the ion exchange method and the oxidant H2O2 or PMS solves the problems of insufficient activity of traditional catalysts and secondary pollution, and achieves efficient degradation and low-cost treatment of organic pollutants in water.
Patent Information
- Application Number
- CN202111417831.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-11-25
AI Technical Summary
In existing advanced oxidation technologies, transition metal catalysts are prone to secondary pollution problems caused by active metal agglomeration and metal leaching when treating persistent organic pollutants in water, and traditional oxide materials are insufficiently active.
The reverse-loaded transition metal catalyst prepared by the ion exchange method can effectively activate the oxidant to degrade pollutants in water by combining with the oxidant H2O2 or PMS, and by optimizing the dosage and pH value of the catalyst, the catalytic activity and degradation efficiency can be improved.
It achieves efficient degradation of organic pollutants in water, reduces the amount of catalyst, improves catalytic activity and the dispersion of active metals, reduces water treatment costs, maintains excellent performance in a wide pH environment, and the catalyst is easy to separate.
Smart Images

Figure HDA0003375793030000011 
Figure HDA0003375793030000012 
Figure HDA0003375793030000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Fenton-like activation in advanced oxidation technology, and relates to the application of a reverse-loaded catalyst in Fenton-like catalytic degradation of pollutants. Background Art
[0002] Among organic pollutants, compared with general organic pollutants and environmental hormones, persistent organic pollutants have higher toxicity, complex structure, low biodegradability and higher stability, and pose great harm to the environment. Therefore, it is particularly important to remove persistent organic pollutants from water bodies.
[0003] At present, the methods for treating persistent organic pollutants in water bodies include photocatalysis, advanced oxidation, membrane treatment and adsorption. Among them, advanced oxidation technology, especially Fenton-like technology, has been studied a lot and has been widely used in industry. In Fenton-like systems, transition metal catalyst materials have been widely recognized due to their efficient catalytic performance. However, during the use of transition metal catalysts, active metals are prone to agglomeration and are difficult to recover. At the same time, metal leaching will cause secondary pollution to the water body. The construction of multi-active component metal oxide Fenton-like catalysts can effectively solve the above problems. Reverse-loaded catalysts can effectively improve the problem of insufficient activity of traditional oxide materials. Therefore, investigating the application of reverse-loaded catalysts in Fenton-like systems has become one of the research focuses. Summary of the invention
[0004] The purpose of the present invention is to provide an application of a reverse-loaded catalyst in Fenton-like catalytic degradation of pollutants in water. The present invention prepares a reverse-loaded transition metal catalyst by an ion exchange method, and the obtained catalyst can efficiently activate an oxidant (H2O2, PMS) to degrade pollutants in water.
[0005] The technical solutions to achieve the purpose of the present invention are as follows:
[0006] A reverse-loaded catalyst is used in Fenton-like catalytic degradation of pollutants. The reverse-loaded catalyst and an oxidant H2O2 or PMS are added to a pollutant solution.
[0007] Among them, in the ratio of pollutants to oxidants, the molar ratio of pollutants to H2O2 is 1:10-200, and the optimal ratio is 1:100; the molar ratio of pollutants to PMS is 1:5-40, and the optimal ratio is 1:10.
[0008] Among them, in the study of catalyst dosage, when H2O2 is used as the oxidant, the catalyst dosage is 10-100 mg / L, and the optimal dosage is 50 mg / L; when PMS is used as the oxidant, the catalyst dosage is 5-25 mg / L, and the optimal dosage is 10 mg / L.
[0009] Among them, in the study of the initial pH of the degradation system, when H2O2 was used as the oxidant, the initial pH of the degradation system was 3.0-9.0, and the optimal initial pH was 4.0; when PMS was used as the oxidant, the initial pH of the degradation system was 3.0-9.0, and the optimal initial pH was 7.0.
[0010] At the same time, the reverse supported catalyst activated oxidant can also degrade a variety of pollutants including ATZ, BPA, Phenol, SMX and 4-CP.
[0011] The invention discloses an application of a reverse-loaded catalyst in activating an oxidant to degrade pollutants in water. The reverse-loaded catalyst is obtained by calcining and reducing a hydroxide obtained by an ion exchange method at high temperature.
[0012] Preferably, the reverse supported catalyst is prepared by the following steps:
[0013] Cobalt hydroxide and copper nitrate were added into deionized water at a molar ratio of 1:0.5-2.5, and hydrothermally reacted at 120° C. for 12 h. After washing with water, the mixture was dried and calcined at high temperature for reduction.
[0014] The specific process of calcination reduction is to calcine the above product at 400°C in an air atmosphere for 2 hours, and then reduce it at 500°C in a H2 / Ar (volume ratio = 5:95) atmosphere for 2 hours to obtain a reverse-loaded catalyst.
[0015] More preferably, the molar ratio of cobalt hydroxide to copper nitrate is 1:1.5.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] (1) In the present invention, the reverse supported catalyst can efficiently activate the oxidant to achieve the degradation of organic pollutants in water. In addition, the reverse supported catalyst has a strong metal-support interaction, which greatly improves the catalytic activity, and the active metal has good dispersion, which can provide more active sites;
[0018] (2) The amount of catalyst used in the present invention is lower than that of existing Fenton-type catalysts, which can effectively reduce the cost of water treatment;
[0019] (3) The reverse-loaded catalyst prepared by the present invention can maintain excellent performance under a wide pH environment and can treat pollutants to the detection limit in a short time (H2O2 <60min; PMS <10min);
[0020] (4) The reverse-loaded catalyst is easy to separate in the aqueous phase and has great practical significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart for the preparation of reverse supported catalysts.
[0022] Figure 2 (a) Performance diagram of the reverse supported catalyst with different Cobalt-Cu ratios for activating H2O2 to degrade ATZ, (b) Performance diagram of the reverse supported catalyst with different Cobalt-Cu ratios for activating PMS to degrade ATZ.
[0023] Figure 3 (a) Effect of different H2O2 dosages on ATZ degradation efficiency, (b) Effect of different PMS dosages on ATZ degradation efficiency.
[0024] Figure 4 (a) Effect of different catalyst dosages on the efficiency of ATZ degradation by activated H2O2, (b) Effect of different catalyst dosages on the efficiency of ATZ degradation by activated PMS.
[0025] Figure 5 (a) Performance diagram of ATZ degradation by H2O2 activation over supported catalyst under different pH conditions, (b) Performance diagram of ATZ degradation by PMS activation over supported catalyst under different pH conditions.
[0026] Figure 6 (a) Performance diagram of the reverse supported catalyst activating H2O2 to degrade various pollutants, (b) Performance diagram of the reverse supported catalyst activating PMS to degrade various pollutants.
[0027] Figure 7 (a) The universality of the application of different reverse-loaded catalysts to activate H2O2 to degrade ATZ, (b) The universality of the application of different reverse-loaded catalysts to activate PMS to degrade ATZ.
[0028] Figure 8 (a) Performance diagram of the supported catalyst and the reference catalyst for activation of H2O2 to degrade ATZ, (b) Performance diagram of the supported catalyst and the reference catalyst for activation of PMS to degrade ATZ.
[0029] Fig. 9 (a) Leakage of metal ions after H2O2 activation with different catalysts, (b) Leakage of metal ions after PMS activation with different catalysts. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0031] Combination Figure 1, cobalt hydroxide and copper nitrate were added to deionized water in a molar ratio of 1:0.5-2.5, stirred at 500 rpm for 10 min, hydrothermally reacted at 120°C for 12 h, calcined in air at 400°C for 2 h, and reduced in H2 / Ar (volume ratio = 5:95) at 500°C for 2 h to obtain a reverse supported catalyst. The reverse supported catalyst and an oxidant (H2O2 or PMS) were added to the pollutant solution, wherein the molar ratio of the pollutant to the oxidant was 1:10-200 (H2O2) and 1:5-40 (PMS), respectively. When the pH value of the degradation system was adjusted to 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, and 9.0, the pollutant ATZ was degraded by activating the oxidant using the reverse supported catalyst, and the pollutant degradation efficiency was investigated under 25°C.
[0032] Example
[0033] Step 1, 2.00g (0.02mol) of cobalt hydroxide and 2.42g (0.01mol), 4.83g (0.02mol), 7.25g (0.03mol), 9.66g (0.04mol), 12.08g (0.05mol) of copper nitrate trihydrate were added to 40mL of deionized water, stirred at 500rpm for 10min, hydrothermally reacted at 120℃ for 12h, calcined in air atmosphere at 400℃ for 2h, and reduced in H2 / Ar (volume ratio = 5:95) atmosphere at 500℃ for 2h to obtain a reverse supported catalyst. The obtained samples were named Co3O4@CuO-IE-0.5, Co3O4@CuO-IE-1, Co3O4@CuO-IE, Co3O4@CuO-IE-2, and Co3O4@CuO-IE-2.5.
[0034] Application Example 1
[0035] Take 5 mg of Co3O4@CuO-IE-0.5, Co3O4@CuO-IE-1, Co3O4@CuO-IE, Co3O4@CuO-IE-2, and Co3O4@CuO-IE-2.5 samples prepared in the examples respectively, add them to 100 mL, 10 μmol H2O2, and add them to 100 mL, 10 μmol / L ATZ solution. The pH value of the solution is controlled to be 4.0±0.2. Place it in a constant temperature water bath stirrer and stir it at 200 rpm for 60 min at 25°C. Take out the solution for detection.
[0036] Figure 2 a is a performance diagram of the reverse supported catalyst with different cobalt-copper ratios prepared in the examples for activating H2O2 to degrade ATZ. Figure 2From the results of a, it can be seen that the ATZ degradation efficiency is 56.8%, 74.2%, 98.6%, 77.5% and 65.1% under different cobalt-copper ratios, respectively. It can be concluded that the optimal cobalt-copper ratio is 1:1.5.
[0037] Take 1 mg of Co3O4@CuO-IE-0.5, Co3O4@CuO-IE-1, Co3O4@CuO-IE, Co3O4@CuO-IE-2, and Co3O4@CuO-IE-2.5 samples prepared in the examples respectively, add them to 100 mL, 10 μmol / L ATZ solution with 10 μmol PMS, control the pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0038] Figure 2 b is the performance diagram of the reverse supported catalyst with different cobalt-copper ratios prepared in the examples for activating PMS and degrading ATZ. Figure 2 From the results of a, it can be seen that the ATZ degradation efficiency is 79.5%, 85.6%, 99.8%, 71.2% and 65.3% under different cobalt-copper ratios, respectively. It can be concluded that the optimal cobalt-copper ratio is 1:1.5.
[0039] Application Example 2
[0040] Take 5 mg of Co3O4@CuO-IE sample and add it to 100 mL, 10 μmol, 50 μmol, 100 μmol, 150 μmol, and 200 μmol H2O2 respectively. Add the solution to 100 mL, 10 μM ATZ solution, and control the pH value of the solution to 4.0±0.2. Place it in a constant temperature water bath stirrer and stir it at 200 rpm for 60 min at 25°C. Take out the solution for detection.
[0041] Figure 3 a is the effect of different H2O2 dosage on ATZ degradation efficiency. Figure 3 From the results of a, it can be seen that the ATZ degradation efficiency is 25.6%, 58.3%, 98.6%, 98.5% and 98.4% under different H2O2 dosages. It can be seen that with the increase of H2O2 dosage, the ATZ degradation rate increases. When the H2O2 dosage reaches 100μmol, further increasing the H2O2 dosage will not increase the ATZ degradation rate. It is concluded that the optimal ratio of pollutants to H2O2 dosage is 1:100.
[0042] Take 1 mg of Co3O4@CuO-IE sample and add 5 μmol, 10 μmol, 20 μmol, 30 μmol, and 40 μmol of PMS into 100 mL of 10 μM ATZ solution, respectively. Control the pH value of the solution to 7.0±0.2. Place it in a constant temperature water bath stirrer and stir at 200 rpm for 10 min at 25°C. Take out the solution for detection.
[0043] Figure 3 b is the effect of different PMS dosages on ATZ degradation efficiency. Figure 3 From the results of b, it can be seen that the ATZ degradation efficiency is 58.4%, 99.8%, 99.0%, 98.1% and 97.4% under different PMS dosages. It can be seen that with the increase of PMS dosage, the ATZ degradation rate increases. When the PMS dosage reaches 10μmol, further increasing the PMS dosage will not increase the ATZ degradation rate. It is concluded that the optimal ratio of pollutants to persulfate dosage is 1:10.
[0044] Application Example 3
[0045] Using 1000 μmol / L H2O2 as the oxidant, Co3O4@CuO-IE catalysts in amounts of 10 mg / L, 30 mg / L, 50 mg / L, 70 mg / L, and 100 mg / L were added to 100 mL, 10 μmol / L ATZ solution respectively. The initial pH value of the solution was controlled to be 4.0±0.2. The solution was placed in a constant temperature water bath stirrer and stirred at 200 rpm for 60 min at 25°C. The solution was taken out for detection.
[0046] Figure 4 a is the effect of different Co3O4@CuO-IE dosages on ATZ degradation efficiency when the oxidant is H2O2. Figure 4 From the results of a, it can be seen that the ATZ degradation efficiency is 48.1%, 70.8%, 98.6%, 98.5% and 98.6% under different catalyst dosages. As the catalyst dosage increases, the ATZ degradation rate increases. When the catalyst dosage reaches 50 mg / L, the ATZ degradation rate increases slightly when the catalyst dosage continues to increase. It is concluded that the optimal dosage of Co3O4@CuO-IE is 50 mg / L.
[0047] Take the oxidant and Co3O4@CuO-IE catalyst, make the PMS dosage 100μmol / L, the catalyst dosage 5mg / L, 10mg / L, 15mg / L, 20mg / L, 25mg / L respectively, add them into 100mL, 10μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200rpm for 10min at 25℃, take out the solution for detection.
[0048] Figure 4 b is the effect of different Co3O4@CuO-IE dosages on ATZ degradation efficiency when the oxidant is PMS. Figure 4 From the results of b, it can be seen that the ATZ degradation efficiency is 73.1%, 99.8%, 99.7%, 99.1% and 99.5% under different catalyst dosages. As the catalyst dosage increases, the ATZ degradation rate increases. When the catalyst dosage reaches 10 mg / L, the ATZ degradation rate increases slightly when the catalyst dosage continues to increase. It is concluded that the optimal dosage of Co3O4@CuO-IE is 10 mg / L.
[0049] Application Example 4
[0050] Step 1, take 5 mg Co3O4@CuO-IE sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution with initial pH values of 3.0±0.2, 4.0±0.2, 5.0±0.2, 6.0±0.2, 7.0±0.2, 8.0±0.2, 9.0±0.2, respectively, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0051] Figure 5 a is the performance diagram of ATZ degradation by reverse activation of H2O2 by supported catalyst under different initial pH conditions. Figure 5 As shown in a, under different pH conditions, the ATZ degradation efficiency is 98.1%, 98.6%, 91.2%, 86.4%, 73.1%, 70.1%, and 65.2%, respectively. It can be concluded that the Co3O4@CuO-IE sample can effectively activate H2O2 to degrade pollutants in a wide pH range.
[0052] Step 2, take 1 mg Co3O4@CuO-IE sample and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution with initial pH values of 3.0±0.2, 4.0±0.2, 5.0±0.2, 6.0±0.2, 7.0±0.2, 8.0±0.2, 9.0±0.2, respectively, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0053] Figure 5 b is the performance diagram of PMS degradation of ATZ under different initial pH conditions. Figure 5 As shown in (b), under different initial pH conditions, the ATZ degradation efficiency was 96.8%, 97.5%, 98.3%, 99.0%, 99.8%, 99.4% and 99.2%, respectively. It can be concluded that the Co3O4@CuO-IE sample can effectively activate PMS to degrade pollutants in a wide pH range.
[0054] Application Example 5
[0055] Step 1, take 5 mg Co3O4@CuO-IE sample and 100 μmol H2O2 and add them into 100 mL, 10 μmol / L pollutant (ATZ, BPA, Phenol, SMX, 4-CP) solution respectively, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0056] Figure 6 a is the performance diagram of Co3O4@CuO-IE activating H2O2 to degrade various pollutants. Figure 6 As shown in a, the degradation efficiency of the reverse loaded catalyst Co3O4@CuO-IE material for ATZ, BPA, Phenol, SMX, and 4-CP was 98.64%, 98.8%, 97.6%, 96.5%, and 98.7% respectively in 60 minutes. It can be concluded that the Co3O4@CuO-IE sample can remove a variety of pollutants by activating H2O2.
[0057] Step 2, take 1 mg Co3O4@CuO-IE sample and 10 μmol PMS and add them into 100 mL, 10 μmol / L pollutant (ATZ, BPA, Phenol, SMX, 4-CP) solution respectively, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0058] Figure 6 b is the performance diagram of Co3O4@CuO-IE activated PMS for degradation of various pollutants. Figure 6 As shown in b, the degradation efficiency of the reverse loaded catalyst Co3O4@CuO-IE material for ATZ, BPA, Phenol, SMX, and 4-CP was 99.8%, 99.9%, 99.9%, 99.5%, and 98.6% respectively in 10 minutes. It can be concluded that the Co3O4@CuO-IE sample can remove a variety of pollutants by activating PMS.
[0059] Application Example 6
[0060] In this application example, the copper oxide / cerium oxide reverse supported catalyst material is directly used as a catalyst activation oxidant to degrade ATZ.
[0061] Step 1, 1.95 g (0.02 mol) of copper hydroxide and 13.03 g (0.03 mol) of cerium nitrate hexahydrate were added to 40 mL of deionized water, stirred at 500 rpm for 10 min, hydrothermally reacted at 120° C. for 12 h, calcined at 400° C. in an air atmosphere for 2 h, and reduced at 500° C. in a H2 / Ar (volume ratio = 5:95) atmosphere for 2 h to obtain a reverse-supported catalyst, named CuO@CeO2-IE.
[0062] Step 2, take 5 mg of CuO@CeO2-IE sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0063] Step 3, take 1 mg of CuO@CeO2-IE sample and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0064] Figure 7 The performance diagram of different reverse loaded catalytic materials for activating oxidant and degrading ATZ. Figure 7 From the results of a, it can be seen that the material activated with H2O2 can degrade ATZ by 91.2% within 60 min. Figure 7 From the results of b, it can be seen that the material activated PMS can degrade ATZ by 98.6% within 10 minutes.
[0065] Application Example 7
[0066] In this comparative example, the copper oxide / aluminum oxide reverse supported catalyst material is directly used as a catalyst activation oxidant to degrade ATZ.
[0067] Step 1, 1.95 g (0.02 mol) of copper hydroxide and 11.25 g (0.03 mol) of aluminum nitrate nonahydrate were added to 40 mL of deionized water, stirred at 500 rpm for 10 min, hydrothermally reacted at 120° C. for 12 h, calcined at 400° C. in an air atmosphere for 2 h, and reduced at 500° C. in a H2 / Ar (volume ratio = 5:95) atmosphere for 2 h to obtain a reverse supported catalyst, named CuO@Al2O3-IE.
[0068] Step 2, take 5 mg of CuO@Al2O3-IE sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0069] Step 3, take 1 mg of CuO@Al2O3-IE sample and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0070] Figure 7 The performance diagram of different reverse loaded catalytic materials for activating hydrogen peroxide to degrade ATZ. Figure 7 From the results of a, it can be seen that the material activated with H2O2 can degrade ATZ by 93.6% within 60 min. Figure 7 From the results of b, it can be seen that the material activated PMS can degrade ATZ by 95.4% within 10 minutes.
[0071] Comparative Example 1
[0072] In this comparative example, the Co3O4 / CuO catalytic material prepared by the impregnation method was used to activate the oxidant to degrade ATZ.
[0073] Step 1, take 5.82g (0.02mol) of cobalt nitrate hexahydrate and dissolve it in 10mL of deionized water, add 2.39g (0.03mol) of copper oxide and stir at room temperature for 4h, heat to 80°C to evaporate the solvent, wash with deionized water 3 times, calcine at 400°C in air atmosphere for 2h, and reduce at 500°C in H2 / Ar (volume ratio = 5:95) atmosphere for 2h to obtain a catalyst prepared by impregnation method, named Co3O4 / CuO-IM.
[0074] Step 2, take 5 mg Co3O4 / CuO-IM sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0075] Step 3, take 1 mg of Co3O4 / CuO-IM sample and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0076] Figure 8 The performance diagram of ATZ degradation by activating oxidant of catalytic materials prepared by two different methods. Figure 8 From the results of a, it can be seen that the Co3O4 / CuO-IM material activated with H2O2 can degrade ATZ by 65.2% within 60 min. Figure 8 From the results of b, it can be seen that the Co3O4 / CuO-IM material activated PMS can degrade ATZ by 68.4% within 10 min.
[0077] Comparative Example 2
[0078] In this comparative example, Co3O4 was directly used as a catalyst to activate the oxidant to degrade ATZ.
[0079] Step 1, take 5 mg Co3O4 sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0080] Step 2, take 1 mg of Co3O4 sample and 10 μmol PMS and add them to 100 mL of 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0081] Figure 8 It is the performance diagram of different catalytic materials for activating oxidants to degrade ATZ. Figure 8 From the results of a, it can be seen that Co3O4 material activated H2O2 can degrade ATZ by 17.2% within 60 min. Figure 8From the results of b, it can be seen that Co3O4 material activated PMS can degrade ATZ by 53.2% within 10 min.
[0082] Comparative Example 3
[0083] In this comparative example, CuO was directly used as a catalyst to activate the oxidant to degrade ATZ.
[0084] Step 1, take 5 mg of CuO sample and 100 μmol H2O2, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0085] Step 2, take 1 mg of CuO sample and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0086] Figure 8 It is the performance diagram of different catalytic materials for activating oxidants to degrade ATZ. Figure 8 From the results of a, it can be seen that the CuO material activated H2O2 can degrade ATZ by 50.1% within 60 min. Figure 8 From the results of b, it can be seen that CuO material activated PMS can degrade ATZ by 32.1% within 10 min.
[0087] Comparative Example 4
[0088] In this comparative example, Co3O4@CuO-IE, Co3O4 / CuO-IM, Co3O4 and CuO were used as catalyst activation oxidants to degrade ATZ, and the amount of metal ions leached from the catalyst after the catalytic reaction was tested by inductively coupled plasma (ICP).
[0089] Step 1, take 5 mg Co3O4@CuO-IE, Co3O4 / CuO-IM, Co3O4 and CuO samples and add them to 100 mL, 10 μmol / L ATZ solution with 100 μmol H2O2 respectively, control the initial pH value of the solution to 4.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 60 min at 25°C, and take out the solution for detection.
[0090] Step 2, take 1 mg of Co3O4@CuO-IE, Co3O4 / CuO-IM, Co3O4 and CuO samples and 10 μmol PMS, add them into 100 mL, 10 μmol / L ATZ solution, control the initial pH value of the solution to 7.0±0.2, place it in a constant temperature water bath stirrer, stir at 200 rpm for 10 min at 25°C, and take out the solution for detection.
[0091] Fig. 9 It is the leaching diagram of metal ions after different catalytic materials activate the oxidant. Fig. 9 From the results of a, it can be seen that: when H2O2 is used as the oxidant, the metal leaching amount of the reverse supported catalyst Co3O4@CuO-IE is 49μg / L (Co) and 89μg / L (Cu), the metal leaching amount of the catalyst Co3O4 / CuO-IM obtained by the ordinary impregnation method is 351μg / L (Co) and 251μg / L (Cu), the leaching amount of the metal oxide Co3O4 is 374μg / L (Co), and the leaching amount of CuO is 361μg / L (Cu). Fig. 9 From the results of b, it can be seen that: when PMS is used as the oxidant, the metal leaching amount of the reverse supported catalyst Co3O4@CuO-IE is 40μg / L (Co) and 81μg / L (Cu), the metal leaching amount of the catalyst Co3O4 / CuO-IM obtained by the ordinary impregnation method is 251μg / L (Co) and 182μg / L (Cu), the leaching amount of metal oxide Co3O4 is 300μg / L (Co), and the leaching amount of CuO is 210μg / L (Cu).
[0092] From the above results, it can be seen that by optimizing the preparation process and multiple parameters of the degradation system, the reverse-loaded catalyst prepared in this patent can effectively activate the oxidant to degrade pollutants. At the same time, the material can effectively activate the oxidant in a wide pH range, and the removal efficiency of pollutants is higher than that of comparative samples such as Co3O4 / Al2O3-IM obtained by the impregnation method. The experimental results show that the material is applicable to a variety of pollutant degradation systems. At the same time, this application can also be extended to other reverse-loaded catalyst materials, with good universality.
Claims
1. An application of a reverse-loaded catalyst in Fenton-like catalytic degradation of pollutants, characterized in that: Add the reverse supported catalyst and oxidant H2O2 or PMS into the pollutant solution; The molar ratio of pollutants to H2O2 is 1:10~200, and the molar ratio of pollutants to PMS is 1:5~40; the initial pH value of the system is 3.0~9.0; when H2O2 is used as the oxidant, the pH is 4.0; when PMS is used as the oxidant, the pH is 7.0; The reverse loaded catalyst preparation method is: Taking advantage of the difference in solubility products of different metals, metal particles are evenly dispersed through ion exchange; Cobalt hydroxide and copper nitrate were added into deionized water at a molar ratio of 1:0.5 to 2.5, stirred at 500 rpm for 10 min, and hydrothermally reacted at 100 °C for 12 h. The product was washed with water several times and then dried for later use; The above product was further calcined and reduced, specifically, the above product was calcined at 400 °C in an air atmosphere for 2 h, and then reduced at 500 °C for 2 h, with a H2 / Ar volume ratio of 5:95, to obtain a reverse-supported catalyst.
2. The use according to claim 1, characterized in that Contaminants include ATZ or SMX drug residues, BPA, Phenol or 4-CP phenol residues.
3. The use according to claim 1, characterized in that When H2O2 is used as the oxidant, the dosage of the catalyst is 10 ~100 mg / L.
4. The use according to claim 3, characterized in that When H2O2 is used as the oxidant, the dosage of the catalyst is 50 mg / L.
5. The use according to claim 1, characterized in that When PMS is used as the oxidant, the dosage of the catalyst is 5 ~ 25 mg / L.
6. The use according to claim 1, characterized in that The molar ratio of cobalt hydroxide to copper nitrate is 1:1.5.
Citation Information
Patent Citations
Preparation method of supported transition metal catalyst utilizing iron tailings as carrier and method for degrading organic pollutants
CN103464166A