A method for manufacturing high performance rare earth permanent magnet

By constructing the composite main phase and grain boundary phase structure in the rare earth permanent magnet, the problem of traditional NdFeB rare earth permanent magnet devices' dependence on rare earth resources is solved, the magnetic energy product and coercive force are improved, and the application range of lanthanum and cerium magnets is broadened. , suitable for energy saving and control of motors, auto parts and other fields.

CN114203433BActive Publication Date: 2024-10-25CHINA NORTH MAGNETIC & ELECTRONICS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111546067.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-10-25
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Traditional NdFeB rare earth permanent magnet devices rely too much on rare earth elements, resulting in unbalanced utilization of rare earth resources. Simply replacing praseodymium and neodymium with lanthanum and cerium will affect the heat resistance and magnetic properties of the magnet, limiting its application.

Method used

By adopting high-performance rare earth permanent magnet manufacturing methods, LR-Fe-Ma, NR-Fe-Mb and HR-Fe-Mc alloy sheets are used to prepare ingredients according to specific proportions, and perform vacuum hydrogen treatment, airflow grinding, magnetic field shaping, and vacuum Processes such as sintering and vacuum infiltration of rare earths build a composite main phase and grain boundary phase structure to improve the magnetic energy product, coercive force and corrosion resistance of the magnet.

Benefits of technology

It significantly improves the magnetic energy product, coercivity and corrosion resistance of rare earth permanent magnet materials, reduces the amount of heavy rare earth elements, reduces production costs, and broadens the scope of application. It is especially suitable for automotive parts, wind power generation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 36811DEST_PATH_IMAGE002
    Figure 36811DEST_PATH_IMAGE002
  • Figure 815914DEST_PATH_IMAGE001
    Figure 815914DEST_PATH_IMAGE001
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a high-performance rare earth permanent magnet. The raw materials of the manufacturing method are mainly composed of LR-Fe-Ma alloy sheets, NR-Fe-Mb alloy sheets and HR-Fe-Mc alloy sheets according to a ratio, the weight ratio of LR-Fe-Ma alloy sheets in the raw materials is within the range of 5-55%, the weight ratio of NR-Fe-Mb alloy sheets in the raw materials is within the range of 45-95%; the weight ratio of HR-Fe-Mc alloy sheets in the raw materials is within the range of 0-10%. LR-Fe-Ma alloy sheets, NR-Fe-Mb alloy sheets and HR-Fe-Mc alloy sheets are respectively manufactured by vacuum melting and rapid solidification methods; first, the raw materials of the alloy sheets are induction heated under vacuum or argon protection to melt and refine the raw materials to form molten alloy liquid, and then the molten alloy liquid is cast through a tundish on a rotating roller with water cooling within a temperature range of 1400-1550°C, and the molten alloy liquid is cooled by the rotating roller to form an alloy sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rare earth permanent magnets, and in particular relates to a method for manufacturing a high-performance rare earth permanent magnet. Background Art

[0002] NdFeB rare earth permanent magnets are increasingly used for their excellent magnetic properties. They are widely used in medical MRI, computer hard disk drives, audio, mobile phones, etc. With the requirements of energy conservation and low-carbon economy, NdFeB rare earth permanent magnets have begun to be used in automotive parts, household appliances, energy-saving and control motors, hybrid vehicles, wind power generation and other fields. In 1983, Japanese patents 1,622,492 and 2,137,496 first disclosed the NdFeB rare earth permanent magnet invented by Sumitomo Metal of Japan, announced the characteristics, composition and manufacturing method of NdFeB rare earth permanent magnets, and confirmed that the main phase is Nd 2 Fe 14 B phase, the grain boundary phase is mainly composed of Nd-rich phase, B-rich phase and rare earth oxide impurities; NdFeB rare earth permanent magnets are widely used for their excellent magnetic properties and are known as the king of permanent magnets; U.S. Patent US5.645,651 authorized in 1997 further clarified the addition of Co elements and the main phase has a tetragonal phase structure.

[0003] With the widespread application of NdFeB rare earth permanent magnets, rare earths are becoming increasingly scarce, especially in recent years, with the continuous growth of the total output of NdFeB rare earth permanent magnet devices, the problem of unbalanced use of rare earth metals has also become prominent. Traditional NdFeB rare earth permanent magnet devices are too dependent on rare earth elements Pr, Nd and heavy rare earth elements Dy, Tb, which makes the crustal reserves of such elements stretched in the face of increasing production demand. Rare earth resources stored in the crust mostly exist in a symbiotic manner, of which lanthanum and cerium account for more than 70%, praseodymium and neodymium account for about 20%, and heavy rare earth elements account for less than 10%. Since the abundance of lanthanum and cerium in rare earth ores is much higher than that of praseodymium and neodymium, the rapid development of the NdFeB rare earth permanent magnet industry will cause a large backlog of lanthanum and cerium, a byproduct produced in the process of extracting praseodymium-neodymium alloys, exacerbating the contradiction of unbalanced application of rare earth elements.

[0004] In this case, if lanthanum and cerium can be used to replace part of praseodymium and neodymium in NdFeB rare earth permanent magnet devices, it can not only greatly reduce the cost of sintered NdFeB rare earth permanent magnet devices, but also achieve comprehensive and balanced utilization of rare earth resources. However, simply replacing praseodymium and neodymium with lanthanum and cerium will have a great impact on the heat resistance and magnetism of the magnet, limiting the use of lanthanum and cerium in NdFeB rare earth permanent magnet devices. Therefore, how to replace praseodymium and neodymium in NdFeB rare earth permanent magnet devices with lanthanum and cerium while maintaining high magnetic properties of the device has become a research hotspot at home and abroad. Summary of the invention

[0005] Through research and exploration, the present invention proposes a method for manufacturing a high-performance rare earth permanent magnet, which overcomes the shortcomings of the prior art, significantly improves the magnetic energy product, coercive force, corrosion resistance and processing performance of lanthanum-cerium-neodymium-iron-boron rare earth permanent magnet materials, is suitable for mass production, and reduces the amount of heavy rare earth elements that are expensive and scarce in resources. It is of great significance to expand the application market of neodymium iron boron rare earth permanent magnets, especially in the fields of energy saving and control motors, automotive parts, new energy vehicles, wind power generation, etc.

[0006] A method for manufacturing a high-performance rare earth permanent magnet. The raw materials of the high-performance rare earth permanent magnet are mainly composed of LR-Fe-Ma alloy sheets, NR-Fe-Mb alloy sheets and HR-Fe-Mc alloy sheets according to a proportion. The weight ratio of the LR-Fe-Ma alloy sheets in the raw materials is in the range of 5-55%, the weight ratio of the NR-Fe-Mb alloy sheets in the raw materials is in the range of 45-95%; the weight ratio of the HR-Fe-Mc alloy sheets in the raw materials is in the range of 0-10%. In the high-performance rare earth permanent magnet, the weight content of LR is in the range of 2-19%, the weight content of NR is in the range of 14-33%, and the weight content of the rare earth element Tb or Dy is in the range of 0.1-1.2%. represents at least one selected from the rare earth elements La and Ce; NR represents at least one selected from the rare earth elements Nd and Pr; HR represents at least one selected from the rare earth elements Gd, Tb, Dy and Ho, and includes at least Tb or Dy; Ma represents at least one selected from the elements Al, Co, Ga, Cu, and B; Mb represents at least one selected from the elements Al, Co, Nb, Ga, Zr, Cu, Mo, and B; Mc represents at least one selected from the elements Al, Co, Nb, Ga, Zr, Cu, and B; and the manufacturing method thereof mainly comprises the following steps:

[0007] (1) Ingredients

[0008] LR-Fe-Ma alloy flakes, NR-Fe-Mb alloy flakes and HR-Fe-Mc alloy flakes are mixed according to the ratio requirements and loaded into the material basket of the vacuum hydrogen treatment furnace after mixing;

[0009] (2) Vacuum hydrogen treatment

[0010] The basket containing the LR-Fe-Ma alloy sheet, the NR-Fe-Mb alloy sheet and the HR-Fe-Mc alloy sheet is sent into a vacuum hydrogen treatment furnace, and after vacuuming, hydrogen is filled in for hydrogen absorption at a temperature of 50-300° C. After the hydrogen absorption is completed, heating is performed and vacuuming and dehydrogenation is performed at a temperature of 550-850° C. After dehydrogenation, the alloy sheet is cooled to below 200° C. in the vacuum hydrogen treatment furnace and then loaded into an alloy sheet storage tank;

[0011] (3) Airflow milling

[0012] Under nitrogen protection, the alloy sheet storage tank is placed in a mixer for mixing, and then air flow milling is performed to obtain rare earth permanent magnet alloy powder with an average particle size in the range of 1.5-3.5 μm;

[0013] (4) Magnetic field forming

[0014] The rare earth permanent magnet alloy powder prepared in the previous step is fed into a protective atmosphere magnetic field forming press under nitrogen protection for magnetic field forming to form a rare earth permanent magnet compact;

[0015] (5) Vacuum sintering

[0016] Under protective atmosphere conditions, the rare earth permanent magnet compact is sent into a vacuum sintering furnace for vacuum sintering to form a rare earth permanent magnet blank;

[0017] (6) Vacuum infiltration of rare earth

[0018] Then, under vacuum conditions, at least one vacuum coating method selected from magnetron sputtering, multi-arc ion plating, and evaporation is used to attach rare earth elements Tb or Dy to the surface of the rare earth permanent magnet block, and then the rare earth permanent magnet block with rare earth Tb or Dy attached to the surface is placed in a vacuum rare earth infiltration device, and under vacuum conditions, the rare earth permanent magnet block with rare earth Tb or Dy attached to the surface is heated to 750-1020°C and kept warm for more than 3 hours, and then cooled under argon protection to below 300°C, and then the rare earth permanent magnet block is heated to 400-700°C, kept warm for more than 2 hours, and then cooled; the rare earth permanent magnet block is either a sintered rare earth permanent magnet blank, or a block obtained by machining the rare earth permanent magnet blank;

[0019] After vacuum rare earth infiltration, the rare earth permanent magnet block undergoes at least one post-processing step of mechanical processing and surface treatment to be made into a high-performance rare earth permanent magnet.

[0020] The LR-Fe-Ma alloy sheet, NR-Fe-Mb alloy sheet and HR-Fe-Mc alloy sheet are respectively manufactured by vacuum melting and rapid solidification methods; first, the raw materials of the alloy sheet are induction heated under vacuum or argon protection to melt and refine the raw materials to form molten alloy liquid, and then the molten alloy liquid is cast through a tundish onto a rotating roller with water cooling at a temperature range of 1400-1550°C, and the molten alloy liquid is cooled by the rotating roller to form an alloy sheet.

[0021] The weight content of LR in the LR-Fe-Ma alloy sheet is in the range of 28-33%. The weight content of NR in the NR-Fe-Mb alloy sheet is in the range of 30-35%. The weight content of HR in the HR-Fe-Mc alloy sheet is in the range of 30-50%. The average grain size of the LR-Fe-Ma alloy sheet is 1.5-3.0μm; the average grain size of the NR-Fe-Mb alloy sheet is 2.0-3.5μm; the average grain size of the HR-Fe-Mc alloy sheet is 0.5-2.8μm.

[0022] In the vacuum hydrogen treatment process, the hydrogen absorption and dehydrogenation of the alloy sheet are completed in different containers respectively, and the maximum pressure of the hydrogen absorption process is not higher than 2MPa. In the air flow grinding process, the working gas pressure is in the range of 0.4-0.7 MPa, the oxygen content in the atmosphere is less than 300ppm, and the yield of rare earth permanent magnet alloy powder is higher than 98%. Magnetic field forming is carried out under nitrogen protection, and the nitrogen purity is higher than 98%; before the rare earth permanent magnet compact is sent into the vacuum sintering furnace, the rare earth permanent magnet compact must be isolated from the air. In the vacuum sintering process, the vacuum sintering furnace is a continuous vacuum sintering furnace. The vacuum sintering process includes degreasing, degassing, sintering, and gas cooling steps, and each step is completed in a separate vacuum chamber.

[0023] In the vacuum rare earth infiltration process, a target made of rare earth metal Tb or Dy, or an alloy containing Tb or Dy, is used, and the target is attached to the surface of the rare earth permanent magnet block in a continuous vacuum coating device to form a film.

[0024] By the manufacturing method of the present invention, a high-performance rare earth permanent magnet is manufactured, and the main components include LR, NR, HR, Ma, Mb, Mc and Fe elements, wherein: Ma represents one or more elements selected from Al, Co, Ga, Cu, and B; Mb represents one or more elements selected from Al, Co, Nb, Ga, Zr, Cu, Mo, and B; Mc represents one or more elements selected from Al, Co, Nb, Ga, Zr, Cu, and B; LR represents one or more rare earth elements La and Ce; NR represents one or more rare earth elements Nd and Pr; HR represents one or more rare earth elements Gd, Tb, Dy, and Ho. , and at least includes Tb or Dy; in the high-performance rare earth permanent magnet, the weight content of LR is in the range of 2-19%, the weight content of NR is in the range of 14-33%, and the weight content of HR is in the range of 0.1-3%, wherein the weight content of Tb or Dy is in the range of 0.1-0.9%; the high-performance rare earth permanent magnet is composed of a composite main phase and a grain boundary phase, the composite main phase includes a main phase whose main components are LR-Fe-Ma and a main phase whose main components are NR-Fe-Mb; the grain boundary phase surrounds the main phase, and the average size of the grains separated by the grain boundary phase is in the range of 2-9μm; the rare earth element Tb or Dy is distributed in the outer layer of the main phase and the grain boundary phase.

[0025] The composite main phase also includes a main phase whose main component is HR-Fe-Mc; the grain boundary phase contains rare earth elements Nd, Pr, and at least one selected from La and Ce, and at least one selected from Dy or Tb. The oxygen content in the high-performance rare earth permanent magnet is less than 2000ppm.

[0026] Preferably, the grain size is in the range of 3-6 μm on average.

[0027] The present invention improves the performance of the magnet by adjusting the main phase composition and controlling the magnet structure, and prepares a new type of lanthanum-cerium-containing permanent magnet material by constructing a composite main phase including three main phases of LR-Fe-Ma, NR-Fe-Mb and HR-Fe-Mc as the main components, thereby obtaining an unconventional composite effect of "1+1>2". LR-Fe-Ma is a phase of low magnetic domain nucleation field HA. By adding the LR-Fe-Ma main phase, LR replaces NR in the rare earth-rich phase to form an NR-LR-Fe phase. At the same time, part of LR enters the grain boundary, which reduces the melting point of the rare earth-rich phase. The magnet can be densified at a relatively low sintering temperature, and low-temperature sintering can be achieved, thereby avoiding grain growth and achieving grain refinement, which is beneficial to improving the coercive force of the magnet. In addition, the entry of LR into the grain boundary phase improves the fluidity of the grain boundary phase and the wettability with the main phase, making the grain boundary phase of the high-performance rare earth permanent magnet material more uniform and continuous. The grains of the composite main phase are wrapped and isolated by a layer of continuous grain boundary phase, and a mutually isolated structure is constructed between different main phase grains, which weakens the mutual coupling between different hard magnetic phases in the magnet and reduces the influence of the stray magnetic field in the magnet on the coercive force. NR-Fe-Mb is a phase with a medium magnetic domain nucleation field HA without LR, so that the remanence Br and coercive force of the magnet will not be significantly reduced. The HR-Fe-Mc main phase in the composite main phase is a phase with a high magnetic domain nucleation field HA. Its addition provides a stronger magnetic domain nucleation field, and the decoupling effect from the above-mentioned grain boundary phase isolation structure containing LR further enhances the coercive force of the magnet. Under the combined effect of the above-mentioned mechanisms, the coercive force of this new type of high-performance rare earth permanent magnet is ultimately greatly improved, and the remanence of the magnet will not be significantly reduced.

[0028] The high-performance rare earth permanent magnet manufactured by the technology of the present invention significantly reduces the dosage of heavy rare earth Dy, Tb and medium rare earth Pr, Nd under the condition of the same coercive force, and adds a large proportion of high-abundance light rare earth components such as La and Ce, thereby saving scarce rare earth resources and broadening the application scope of lanthanum-cerium magnets, so that they can be widely used in industries such as automobiles and wind power generation. DETAILED DESCRIPTION

[0029] The remarkable effects of the present invention are further illustrated by comparison of the following embodiments.

[0030] The vacuum melting and rapid solidification method is used to manufacture LR-Fe-Ma alloy sheets, NR-Fe-Mb alloy sheets and HR-Fe-Mc alloy sheets with the composition ratios listed in Table 1: first, the raw materials of the alloy sheets are induction heated under vacuum to melt and refine the raw materials to form molten alloy liquid, and then the molten alloy liquid is cast onto a rotating roller with water cooling through a tundish at a temperature range of 1400-1550℃, and the molten alloy liquid is cooled by the rotating roller to form alloy sheets. The average grain size of the LR-Fe-Ma alloy sheet is 1.5-3.0μm; the average grain size of the NR-Fe-Mb alloy sheet is 2.0-3.5μm; and the average grain size of the HR-Fe-Mc alloy sheet is 0.5-2.8μm.

[0031] Example 1

[0032] According to the composition ratio of Example 1 listed in Table 1, LR-Fe-B-Ma, NR-Fe-Mb and HR-Fe-B-Mb alloy sheets are selected for batching, mixed and loaded into a vacuum hydrogen treatment furnace for vacuum hydrogen treatment. In the vacuum hydrogen treatment process, hydrogen absorption and dehydrogenation of the alloy sheet are completed in different containers respectively, the maximum pressure of the hydrogen absorption process is not higher than 2MPa, and the dehydrogenation temperature is 650°C; the alloy sheet is loaded into an alloy sheet storage tank, and the alloy sheet storage tank is placed in a mixer under nitrogen protection for mixing. After mixing, air flow grinding is performed to obtain a rare earth permanent magnet alloy powder with an average particle size of about 3μm; the previous rare earth permanent magnet alloy powder is sent to a protective atmosphere magnetic field forming press under nitrogen protection for magnetic field forming to form a rare earth permanent magnet compact; under protective atmosphere conditions, the rare earth permanent magnet compact is sent to a continuous vacuum sintering furnace for vacuum sintering to form a rare earth permanent magnet blank; Then, under vacuum conditions, a vacuum coating method of magnetron sputtering and multi-arc ion plating is used to attach the rare earth element Tb to the surface of the rare earth permanent magnet block, and then the rare earth permanent magnet block with rare earth Tb attached to the surface is placed in a vacuum rare earth infiltration device, and under vacuum conditions, the rare earth permanent magnet block with rare earth Tb attached to the surface is heated to about 820°C and kept warm for 6 hours, and then cooled under argon protection to below 300°C, and then the rare earth permanent magnet block is heated to about 450°C, and after keeping warm for 3 hours, the rare earth permanent magnet block is cooled; the rare earth permanent magnet block is either a sintered rare earth permanent magnet blank, or a block obtained by machining the rare earth permanent magnet blank; the rare earth permanent magnet block after vacuum rare earth infiltration is subjected to at least one post-processing step of machining and surface treatment to make a high-performance rare earth permanent magnet. Then the magnetic properties of the permanent magnet obtained in Example 1 are measured, and the results are listed in Table 1.

[0033] Example 2

[0034] According to the composition ratio of Example 2 listed in Table 1, LR-Fe-B-Ma, NR-Fe-Mb and HR-Fe-B-Mb alloy sheets are selected for batching, mixed and loaded into a vacuum hydrogen treatment furnace for vacuum hydrogen treatment. In the vacuum hydrogen treatment process, hydrogen absorption and dehydrogenation of the alloy sheet are completed in different containers respectively, the maximum pressure of the hydrogen absorption process is not higher than 2MPa, and the dehydrogenation temperature is 650°C; the alloy sheet is loaded into an alloy sheet storage tank, and the alloy sheet storage tank is placed in a mixer for mixing under nitrogen protection. After mixing, air flow grinding is performed to obtain a rare earth permanent magnet alloy powder with an average particle size of about 2.8μm; the previous rare earth permanent magnet alloy powder is sent to a protective atmosphere magnetic field forming press under nitrogen protection for magnetic field forming to form a rare earth permanent magnet compact; under protective atmosphere conditions, the rare earth permanent magnet compact is sent to a continuous vacuum sintering furnace for vacuum sintering to form a rare earth permanent magnet blank; Then, under vacuum conditions, a vacuum coating method of magnetron sputtering and multi-arc ion plating is used to attach the rare earth element Dy to the surface of the rare earth permanent magnet block, and then the rare earth permanent magnet block with rare earth Dy attached to the surface is placed in a vacuum rare earth infiltration device, and under vacuum conditions, the rare earth permanent magnet block with rare earth Dy attached to the surface is heated to about 810°C and kept warm for 6 hours, and then cooled under argon protection to below 300°C, and then the rare earth permanent magnet block is heated to about 430°C, and after keeping warm for 3 hours, the rare earth permanent magnet block is cooled; the rare earth permanent magnet block is either a sintered rare earth permanent magnet blank, or a block obtained by machining the rare earth permanent magnet blank; the rare earth permanent magnet block after vacuum rare earth infiltration is subjected to at least one post-processing step of machining and surface treatment to make a high-performance rare earth permanent magnet. Then the magnetic properties of the permanent magnet obtained in Example 2 are measured, and the results are listed in Table 1.

[0035] Example 3

[0036] According to the composition ratio of Example 2 listed in Table 1, LR-Fe-B-Ma, NR-Fe-Mb and HR-Fe-B-Mb alloy sheets are selected for batching, mixed and loaded into a vacuum hydrogen treatment furnace for vacuum hydrogen treatment. In the vacuum hydrogen treatment process, hydrogen absorption and dehydrogenation of the alloy sheet are completed in different containers respectively, the maximum pressure of the hydrogen absorption process is not higher than 2MPa, and the dehydrogenation temperature is 650°C; the alloy sheet is loaded into an alloy sheet storage tank, and the alloy sheet storage tank is placed in a mixer for mixing under nitrogen protection. After mixing, air flow grinding is performed to obtain a rare earth permanent magnet alloy powder with an average particle size of about 2.6μm; the previous rare earth permanent magnet alloy powder is sent to a protective atmosphere magnetic field forming press under nitrogen protection for magnetic field forming to form a rare earth permanent magnet compact; under protective atmosphere conditions, the rare earth permanent magnet compact is sent to a continuous vacuum sintering furnace for vacuum sintering to form a rare earth permanent magnet blank; Then, under vacuum conditions, a vacuum coating method of magnetron sputtering and multi-arc ion plating is used to attach the rare earth element Dy to the surface of the rare earth permanent magnet block, and then the rare earth permanent magnet block with rare earth Dy attached to the surface is placed in a vacuum rare earth infiltration device, and under vacuum conditions, the rare earth permanent magnet block with rare earth Dy attached to the surface is heated to about 800°C and kept warm for 6 hours, and then cooled under argon protection to below 300°C, and then the rare earth permanent magnet block is heated to about 410°C, and after keeping warm for 3 hours, the rare earth permanent magnet block is cooled; the rare earth permanent magnet block is either a sintered rare earth permanent magnet blank, or a block obtained by machining the rare earth permanent magnet blank; the rare earth permanent magnet block after vacuum rare earth infiltration is subjected to at least one post-processing step of machining and surface treatment to make a high-performance rare earth permanent magnet. Then the magnetic properties of the permanent magnet obtained in Example 3 are measured, and the results are listed in Table 1.

[0037] Comparative Example

[0038] Raw materials with similar composition ratios to those of the permanent magnets obtained in Examples 1-3 were used for batching, and a single alloy sheet was made by ordinary vacuum melting and rapid solidification technology. The alloy sheet was subjected to conventional vacuum hydrogen treatment, air flow grinding, magnetic field forming and vacuum sintering processes to obtain comparative examples 1-3 with substantially the same composition ratios as those of the permanent magnets obtained in Examples 1-3. The magnetic properties were then measured, and the test results are listed in Table 2.

[0039] Although the magnet compositions of Examples 1-3 and Comparative Examples 1-3 are substantially the same, the magnetic energy product and intrinsic coercive force of the permanent magnets of Examples 1-3 obtained using the manufacturing technology of the present invention are significantly higher than those of the comparative examples, so that the high-performance rare earth permanent magnets obtained by adding a large proportion of lanthanum and cerium meet the use requirements of industries such as automobiles and wind power generation.

[0040] Table 1. Main components and magnetic properties test results of the alloy sheets in the examples

[0041]

[0042] Table 2, magnetic properties test results of comparative examples:

[0043]

Claims

1. A method for manufacturing a high-performance rare earth permanent magnet, characterized in that: The raw materials include LR-Fe-Ma alloy sheets, NR-Fe-Mb alloy sheets and HR-Fe-Mc alloy sheets in proportion, the weight ratio of the LR-Fe-Ma alloy sheets in the raw materials is in the range of 5-55%, and the weight content of LR in the LR-Fe-Ma alloy sheets is in the range of 28-33%; the weight ratio of the NR-Fe-Mb alloy sheets in the raw materials is in the range of 45-95%, and the weight content of NR in the NR-Fe-Mb alloy sheets is in the range of 30-35%; the weight ratio of the HR-Fe-Mc alloy sheets in the raw materials is in the range of 0-10%, and the weight content of HR in the HR-Fe-Mc alloy sheets is in the range of 30-50%; in the high-performance rare earth permanent magnet, the weight content of LR is in the range of 2-19%, the weight content of NR is in the range of 14-33%, and the weight content of the rare earth element Dy or Tb is in the range of 0.1-1.2%; wherein: LR represents the rare earth elements La and Ce; NR represents one or more selected from the rare earth elements Nd and Pr; HR represents one or more selected from the rare earth elements Gd, Tb, Dy and Ho, and includes at least Tb or Dy; Ma represents one or more selected from the elements Al, Co, Ga, Cu, and B; Mb represents one or more selected from the elements Al, Co, Nb, Ga, Zr, Cu, Mo, and B; Mc represents one or more selected from the elements Al, Co, Nb, Ga, Zr, Cu, and B; and the manufacturing method thereof comprises the following steps: (1) Ingredients: LR-Fe-Ma alloy flakes, NR-Fe-Mb alloy flakes and HR-Fe-Mc alloy flakes are mixed according to the ratio requirements and loaded into the material basket of the vacuum hydrogen treatment furnace after mixing; (2) Vacuum hydrogen treatment: The basket containing the LR-Fe-Ma alloy sheet, the NR-Fe-Mb alloy sheet and the HR-Fe-Mc alloy sheet is sent into a vacuum hydrogen treatment furnace, and after vacuuming, hydrogen is filled in for hydrogen absorption at a temperature of 50-300°C. After the hydrogen absorption is completed, heating is performed and vacuuming and dehydrogenation is performed at a temperature of 550-850°C. After dehydrogenation, the alloy sheet is cooled to below 200°C in the vacuum hydrogen treatment furnace and then loaded into an alloy sheet storage tank; (3) Airflow milling: Under nitrogen protection, the alloy sheet storage tank is placed in a mixer for mixing, and then air flow milling is performed to obtain rare earth permanent magnet alloy powder with an average particle size in the range of 1.5-3.5 μm; (4) Magnetic field forming: The rare earth permanent magnet alloy powder prepared in the previous step is fed into a protective atmosphere magnetic field forming press under nitrogen protection for magnetic field forming to form a rare earth permanent magnet compact; (5) Vacuum sintering: Under protective atmosphere conditions, the rare earth permanent magnet compact is sent into a vacuum sintering furnace for vacuum sintering to form a rare earth permanent magnet blank; (6) Vacuum infiltration of rare earth: Under vacuum conditions, at least one vacuum coating method selected from magnetron sputtering, multi-arc ion plating, and evaporation is used to attach rare earth elements Tb or Dy to the surface of a rare earth permanent magnet block, and then the rare earth permanent magnet block with rare earth Tb or Dy attached to the surface is placed in a vacuum rare earth infiltration device, and under vacuum conditions, the rare earth permanent magnet block with rare earth Tb or Dy attached to the surface is heated to 750-1020°C and kept warm for more than 3 hours, and then cooled under argon protection to below 300°C, and then the rare earth permanent magnet block is heated to a range of 400-700°C, kept warm for more than 2 hours, and then cooled; the rare earth permanent magnet block is either a sintered rare earth permanent magnet blank, or a block obtained by mechanical processing of the rare earth permanent magnet blank; the rare earth permanent magnet block after vacuum rare earth infiltration is subjected to at least one post-treatment process of mechanical processing and surface treatment to make a high-performance rare earth permanent magnet.

2. The method for manufacturing a high-performance rare earth permanent magnet according to claim 1, characterized in that: LR-Fe-Ma alloy sheet, NR-Fe-Mb alloy sheet and HR-Fe-Mc alloy sheet are respectively manufactured by vacuum melting and rapid solidification method; first, the raw materials of the alloy sheet are induction heated under vacuum or argon protection to melt and refine the raw materials to form molten alloy liquid, and then the molten alloy liquid is cast through a tundish onto a rotating roller with water cooling in the temperature range of 1400-1550°C, and the molten alloy liquid is cooled by the rotating roller to form alloy sheets.

3. The method for manufacturing a high performance rare earth permanent magnet according to claim 1, characterized in that: In the vacuum hydrogen treatment process, hydrogen absorption and dehydrogenation of the alloy sheet are completed in different containers respectively, and the maximum pressure of the hydrogen absorption process is no more than 2MPa.

4. The method for manufacturing a high performance rare earth permanent magnet according to claim 1, characterized in that: The average grain size of the LR-Fe-Ma alloy sheet is 1.5-3.0 μm; the average grain size of the NR-Fe-Mb alloy sheet is 2.0-3.5 μm; and the average grain size of the HR-Fe-Mc alloy sheet is 0.5-2.8 μm.

5. The method for manufacturing a high performance rare earth permanent magnet according to claim 1, characterized in that: In the air flow grinding process, the working gas pressure is in the range of 0.4-0.7 MPa, the oxygen content in the atmosphere is less than 300ppm, and the yield of rare earth permanent magnet alloy powder is higher than 98%.

6. The method for manufacturing a high-performance rare earth permanent magnet according to claim 1, characterized in that: In the vacuum rare earth infiltration process, a target made of rare earth metal Tb or Dy, or an alloy containing Tb or Dy, is used, and the target is attached to the surface of the rare earth permanent magnet block in a continuous vacuum coating device to form a film.