Easy-adhesive film and method for producing the same, polarizing plate, and image display device

By forming an optimized easy-adhesive layer on the surface of the transparent film substrate, the problems of unevenness and unstable adhesion in the prior art under high temperature and high humidity environment are solved, and the stability of the easy-adhesive film is achieved is achieved. and durability, suitable for polarizers of image display devices.

CN114207485BActive Publication Date: 2024-11-01NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080056610.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-09
Filing Date
2020-06-05
Publication Date
2024-11-01
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

In high temperature and high humidity environments, existing easy-to-adhesive films are prone to unevenness when used for polarizer protection, resulting in reduced display characteristics and unstable adhesiveness.

Method used

It forms an easy-adhesive layer on the surface of the transparent film base material, containing binder resin and microparticles. By optimizing the thickness, particle size and alkaline content of the easy-adhesive layer, the dispersion and adhesiveness of the microparticles are improved, and heating and The stretching process forms an easy-to-adhesive film with high adhesion.

Benefits of technology

It is realized that adhesion and optical defects are not easily generated in high temperature and high humidity environments, and the adhesion and durability of polarizers are improved, and it is suitable for polarizers of image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114207485B_ABST
    Figure CN114207485B_ABST
Patent Text Reader

Abstract

The easy-adhesive film (1) has an easy-adhesive layer (15) on the surface of a transparent film substrate (11). The easy-adhesive layer (15) contains a binder resin and microparticles. The thickness of the easy-adhesive layer is preferably 120 to 260 nm, and the average primary particle size of the microparticles is preferably 0.1 to 0.9 times the thickness of the easy-adhesive layer. The easy-adhesive layer can be formed by coating an easy-adhesive composition containing a binder resin or a precursor thereof, microparticles, an alkali component and a solvent on a transparent film substrate and heating it.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an easy-adhesion film having an easy-adhesion layer on the surface of a transparent film substrate and a method for producing the same. Furthermore, the present invention relates to a polarizing plate having an easy-adhesion film bonded to the surface of a polarizer, and an image display device having the polarizing plate. Background Art

[0002] Liquid crystal display devices and organic EL display devices are widely used as various image display devices such as mobile devices, car navigation devices, personal computer displays, and televisions. From the perspective of its display principle, a liquid crystal display device is provided with a polarizing plate on the surface of the identification side of the liquid crystal unit. In a transmissive liquid crystal display device, polarizing plates are provided on both sides of the liquid crystal unit. In an organic EL display device, in order to suppress external light from being reflected by a metal electrode (cathode) and being identified as a mirror surface, a circular polarizing plate (typically, a laminate of a polarizing plate and a 1 / 4 wavelength plate) is sometimes provided on the surface of the identification side.

[0003] Polarizing plates usually have a transparent film (polarizer protective film) on one or both sides of a polarizer for the purpose of protecting the polarizer, etc. As a polarizer, a polyvinyl alcohol (PVA) film adsorbed with iodine and oriented in molecules by stretching or the like is widely used.

[0004] As a polarizer protective film attached to the surface of the polarizer, cellulose-based films such as cellulose acetate are widely used due to their excellent adhesion to PVA-based polarizers. As a transparent protective film, films formed of resin materials such as acrylic, polyester, polycarbonate, and cyclic polyolefin are also beginning to be used. Films formed of these resin materials have lower moisture permeability than cellulose-based films. Even when a polarizing plate with a low moisture permeability resin film attached to the surface of the polarizer is exposed to a high humidity environment for a long time, the change in optical properties is small, and there is a tendency to be excellent in durability.

[0005] On the other hand, films formed of resin materials such as acrylic, polyester, polycarbonate, and cyclic polyolefin tend to have lower adhesion to PVA-based polarizers than cellulose-based films. Therefore, a method of providing an easy-adhesion layer on the surface of a transparent film used as a polarizer protective film to improve adhesion to the polarizer has been proposed.

[0006] For example, Patent Document 1 records that an easy-adhesive film obtained by providing an easy-adhesive layer containing microparticles and a binder resin on the surface of an acrylic film has excellent adhesion to a polarizer and can suppress sticking when the film is wound into a roll. The embodiment of Patent Document 1 shows an example of using an easy-adhesive film having a carbamate easy-adhesive layer on the surface of an acrylic film as a polarizer protective film, wherein the carbamate easy-adhesive layer contains 1 to 7% by weight of silica particles with an average primary particle size of 35 nm and an average thickness of 400 nm (thickness range 300 to 500 nm). Patent Document 2 records that when the average primary particle size of the microparticles contained in the easy-adhesive layer is greater than 200 nm, the blocking resistance is improved.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 5354733

[0010] Patent Document 2: Japanese Patent Application Publication No. 2012-32768 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] In the process of large-scale and high-brightness image display devices, the polarizing plate constituting the image display device is required to have small changes in optical properties under more severe environments (such as higher temperature and high humidity conditions). For polarizing plates using the easy-adhesive films described in Patent Documents 1 and 2 as polarizer protective films, the polarizer and the polarizer protective film have excellent adhesion and high bonding reliability. However, the following new issues have been discovered: When polarizing plates using these easy-adhesive films as polarizer protective films are exposed to a high humidity environment for a long time, unevenness sometimes occurs, resulting in reduced display characteristics.

[0013] In view of the above problems, an object of the present invention is to provide an easy-adhesion film which has excellent adhesion to polarizers and the like, is less likely to cause blocking, and is less likely to cause uneven optical defects even when exposed to a high temperature and high humidity environment for a long time.

[0014] Solutions for solving problems

[0015] In view of the above problems, the inventors of the present invention have found that the residual alkali components such as ammonia and amines added to the easy-adhesion composition for the purpose of improving the dispersibility of the microparticles in the easy-adhesion layer is one of the reasons for the reduction in durability in a humidified environment. The above problems can be solved by setting the residual alkali amount in the easy-adhesion layer to a specified range.

[0016] The present invention relates to an easy-adhesive film having an easy-adhesive layer on the surface of a transparent film substrate and a method for producing the same. The easy-adhesive layer contains a binder resin and microparticles. The thickness of the easy-adhesive layer is preferably 120 to 260 nm. The average primary particle size of the microparticles contained in the easy-adhesive layer is preferably 0.1 to 0.9 times the thickness of the easy-adhesive layer. The average primary particle size of the microparticles is 10 nm or more, preferably 100 to 200 nm. The content of the alkali component in the easy-adhesive layer is preferably 200 ppm or less, and the total content of amine and ammonia is preferably 200 ppm or less.

[0017] As the transparent film substrate, an acrylic film or the like can be used. As the binder resin of the easy-adhesion layer, a urethane resin or the like can be used. The content of the microparticles in the easy-adhesion layer is preferably about 8 to 50% by weight. The microparticles of the easy-adhesion layer can be embedded in the transparent film substrate.

[0018] An easy-adhesive layer can be formed by applying an easy-adhesive composition on the surface of a transparent film substrate and heating it. The easy-adhesive composition comprises a binder resin or a precursor thereof, particles, an alkali component and a solvent. By making the easy-adhesive composition include an alkali component, the dispersibility of the particles is improved, and an easy-adhesive film with excellent sliding properties can be obtained. In addition, the alkali component can also act as a catalyst for promoting the reaction of the binder resin (precursor). From the viewpoint of promoting the volatilization of the alkali component based on heating, the boiling point of the alkali component is preferably below 150°C. As the alkali component, amines, ammonia, etc. can be listed.

[0019] By increasing the heating temperature after applying the easy-adhesive composition, the volatilization of the alkali component can be promoted, and an easy-adhesive layer with less residual alkali component can be formed. The easy-adhesive composition can also be heated at a temperature that is 10°C higher than the glass transition temperature of the transparent film substrate. By increasing the heating temperature, a region where particles of the easy-adhesive layer are buried in the transparent film substrate is easily formed, and there is a tendency for the adhesion between the transparent film substrate and the easy-adhesive layer to be improved.

[0020] After coating the easy-adhesion composition on the transparent film substrate, the transparent film substrate may be stretched while being heated. In particular, by stretching the transparent film substrate while heating the easy-adhesion composition at a temperature 10° C. or higher than the glass transition temperature of the transparent film substrate, there is a tendency for the adhesion between the transparent film substrate and the easy-adhesion layer to be improved.

[0021] The above-mentioned easy-adhesion film has excellent adhesion to other films, glass substrates, etc. The easy-adhesion film can be used as a polarizer protective film, for example. For example, by laminating the easy-adhesion film on the surface of a polyvinyl alcohol-based polarizer via an adhesive layer, a polarizing plate can be obtained. By configuring a polarizing plate on the surface of an image display unit such as a liquid crystal display unit and an organic EL unit, an image display device can be formed.

[0022] Effects of the Invention

[0023] The easy-adhesion film of the present invention is unlikely to cause blocking and is unlikely to cause optical defects even when exposed to a high-humidity environment for a long period of time, and therefore can be suitably used as a film for display devices such as a polarizer protective film. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a cross-sectional view showing a configuration example of the easy-adhesion film.

[0025] Figure 2 It is a cross-sectional view showing a configuration example of a polarizing plate. DETAILED DESCRIPTION

[0026] Figure 1 Schematic cross-sectional view showing a configuration example of an easy-adhesive film according to an embodiment of the present invention. The easy-adhesive film 1 is provided with an easy-adhesive layer 15 on at least one surface of a film substrate 11. Easy-adhesive layers may also be provided on both surfaces of the film substrate. The easy-adhesive film is used by laminating with other films, glass substrates, etc.

[0027] As a usage form of the easy-adhesion film, a polarizer protective film can be mentioned. Figure 2 1 is a cross-sectional view showing a configuration example of a polarizing plate including an easy-adhesion film 1 as a polarizer protective film. The polarizing plate 100 includes the easy-adhesion film 1 bonded to one surface (first main surface) of a polarizer 5 via an adhesive layer 6 . Figure 2 In the polarizing plate 100 shown, the easy-adhesion film 1 has an easy-adhesion layer 15 on the surface of the film substrate 11 to be bonded to the polarizer 5. The easy-adhesion layer may be provided on the surface not bonded to the polarizer 5. Figure 2 In the polarizing plate 100 shown, a transparent protective film 2 is bonded to the other surface (second main surface) of the polarizer 5 via an adhesive layer 7 .

[0028] [Easy Adhesion Film]

[0029] The easy-adhesion film 1 includes an easy-adhesion layer 15 on at least one surface of a film substrate 11 .

[0030] <Film substrate>

[0031] The film substrate 11 is preferably a transparent film. The total light transmittance of the transparent film substrate is preferably 80% or more, more preferably 85% or more, and further preferably 90% or more. The resin material constituting the film substrate 11 includes acrylic resins, polyester resins, polycarbonate resins, polyolefin resins, cyclic polyolefin resins, polystyrene resins, polyamide resins, polyimide resins, and the like. When the easy-adhesion film is used as an optically isotropic polarizer protective film, the resin material of the film substrate 11 is preferably an acrylic resin or a cyclic polyolefin resin, and particularly preferably an acrylic resin, from the perspective of small birefringence.

[0032] Examples of cyclic polyolefin resins include polynorbornene. Examples of commercially available cyclic polyolefin resins include ZEONOR and ZEONEX manufactured by Zeon Corporation, ARTON manufactured by JSR, APEL manufactured by Mitsui Chemicals, and TOPAS manufactured by TOPAS ADVANCED POLYMERS. The cyclic polyolefin film preferably contains 50% by weight or more of the cyclic olefin resin.

[0033] Examples of acrylic resins include poly(meth)acrylates such as polymethyl methacrylate, methyl methacrylate-(meth)acrylic acid copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-acrylate-(meth)acrylic acid copolymers, methyl (meth)acrylate-styrene copolymers (MS resins, etc.), and polymers having an alicyclic hydrocarbon group (e.g., methyl methacrylate-cyclohexyl methacrylate copolymers, methyl methacrylate-norbornyl (meth)acrylate copolymers, etc.).

[0034] In the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid. Acrylic resins include those containing acrylic acid or its derivatives as monomer components and those containing methacrylic acid or its derivatives as monomer components.

[0035] As the acrylic resin, there can be used an acrylic resin having a glutaric anhydride structure as described in Japanese Patent Laid-Open No. 2006-283013, Japanese Patent Laid-Open No. 2006-335902, Japanese Patent Laid-Open No. 2006-274118, etc.; and / or an acrylic resin having a lactone ring structure as described in Japanese Patent Laid-Open No. 2000-230016, Japanese Patent Laid-Open No. 2001-151814, Japanese Patent Laid-Open No. 2002-120326, Japanese Patent Laid-Open No. 2002-254544, Japanese Patent Laid-Open No. 2005-146084, etc. The acrylic resin having a glutaric anhydride structure and the acrylic resin having a lactone ring structure have high heat resistance, high transparency, and high mechanical strength, and are therefore suitable for the manufacture of polarizing plates having high polarization degree and excellent durability.

[0036] When the film substrate 11 is an acrylic film, the content of the acrylic resin in the film substrate is preferably 50% by weight or more, more preferably 60 to 98% by weight, and further preferably 70 to 97% by weight. The acrylic film may contain a thermoplastic resin other than the acrylic resin. For example, by blending other thermoplastic resins to eliminate the birefringence of the acrylic resin, an acrylic film with excellent optical isotropy can be obtained. In addition, for the purpose of improving the mechanical strength of the film, a thermoplastic resin other than the acrylic resin may also be blended.

[0037] Examples of thermoplastic resins other than acrylic resins include olefin polymers, halogenated vinyl polymers, polystyrene, copolymers of styrene and acrylic monomers, polyesters, polyamides, polyacetals, polycarbonates, polyphenylene ethers, polyphenylene sulfides, polyetheretherketones, polysulfones, polyethersulfones, polyoxybenzyl esters, polyamideimides, and rubber polymers.

[0038] The film substrate 11 may contain additives such as antioxidants, stabilizers, reinforcing materials, ultraviolet absorbers, flame retardants, antistatic agents, colorants, fillers, plasticizers, lubricants, and fillers. The resin material and the additives may be mixed and pre-formed into a thermoplastic resin composition such as pellets before being formed into a film.

[0039] The thickness of the film substrate 11 is about 5 to 200 μm. From the viewpoint of mechanical strength, transparency, and handling properties, the thickness of the film substrate 11 is preferably 10 to 100 μm, and more preferably 15 to 60 μm.

[0040] The glass transition temperature Tg of the film substrate 11 is preferably 100° C. or higher, more preferably 110° C. or higher. When the film substrate 11 is an acrylic film, as described above, by using an acrylic resin having a glutaric anhydride structure or an acrylic resin having a lactone ring structure as the acrylic resin, the Tg of the acrylic film can be increased, thereby improving heat resistance. The upper limit of the Tg of the film substrate 11 is not particularly limited, but is preferably 170° C. or lower from the viewpoint of formability.

[0041] As a method for producing the film substrate 11, a solution casting method, a melt extrusion method, a calendaring method, a compression molding method, etc. can be cited. The film substrate 11 can be either an unstretched film or a stretched film. When the film substrate 11 is an acrylic film, from the viewpoint of improving mechanical strength, the acrylic film is preferably a stretched film stretched in at least one direction, and is particularly preferably a biaxially stretched film. By compounding other thermoplastic resins to eliminate the birefringence of the acrylic resin, an acrylic film with low retardation and excellent optical isotropy can be obtained even when stretched.

[0042] <Easy Adhesion Layer>

[0043] The easy-adhesion layer 15 provided on the surface of the film substrate 11 includes a binder resin and particles. By providing the easy-adhesion layer 15, the adhesion to films such as polarizers, glass substrates, etc. can be improved. By making the easy-adhesion layer 15 include particles, fine concavo-convex patterns are formed on the surface of the easy-adhesion layer 15, and the sliding property of the film is improved. Therefore, it is helpful to reduce the damage of the easy-adhesion film 1 during roller conveyance and suppress adhesion when it is wound into a roll.

[0044] (Binder resin)

[0045] As binder resin, from the aspect of excellent adhesion with film substrates such as acrylic film, resins (polymers) with reactive groups such as polyurethane resin, epoxy resin, isocyanate resin, polyester resin, polymers containing amino groups in the molecule, acrylic resins with crosslinking functional groups such as oxazoline groups can be used. As the binder resin of easy bonding layer 15, polyurethane resin is particularly preferred. The adhesion of the easy bonding layer 15 comprising polyurethane resin binder and film substrate 11 is high. In addition, the easy bonding film 1 comprising polyurethane resin binder has a tendency to show high adhesion when films such as polarizers are laminated by means of adhesive layer.

[0046] The urethane resin is typically a reaction product of a polyol and a polyisocyanate. As the polyol component, preferably used are high molecular weight polyols such as polyacrylic polyols, polyester polyols, and polyether polyols.

[0047] Polyacrylic acid polyols can be obtained by polymerization of (meth)acrylates and hydroxyl-containing monomers. Examples of (meth)acrylates include methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypentyl (meth)acrylate; (meth)acrylate monoesters of polyols such as glycerol and trimethylolpropane; and N-methylol (meth)acrylamide.

[0048] Polyacrylic acid polyols may contain monomer components other than those mentioned above. Other monomer components include: unsaturated monocarboxylic acids such as (meth) acrylic acid; unsaturated dicarboxylic acids such as maleic acid and their anhydrides and diesters; unsaturated nitriles such as (meth) acrylonitrile; unsaturated amides such as (meth) acrylamide and N-hydroxymethyl (meth) acrylamide; vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether; α-olefins such as ethylene and propylene; halogenated α,β-unsaturated aliphatic monomers such as vinyl chloride and vinylidene chloride; α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene, etc.

[0049] Polyester polyols can be obtained by reacting polybasic acids and polyols. Examples of polybasic acids include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, and tetrahydrophthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedioic acid, dodecanedioic acid, octadecanedioic acid, tartaric acid, alkyl succinic acid, linolenic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, tetrahydrophthalic acid, 1,3-cyclohexane dicarboxylic acid, and 1,4-cyclohexane dicarboxylic acid; or reactive derivatives thereof such as anhydrides, alkyl esters, and acyl halides.

[0050] Examples of the polyol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, 1-methyl-1,3-butanediol, 2-methyl-1,3-butanediol, 1-methyl-1,4-pentanediol, 2-methyl-1,4-pentanediol, 1,2-dimethyl-neopentyl glycol, 2,3-dimethyl- Neopentyl glycol, 1-methyl-1,5-pentanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,2-dimethylbutanediol, 1,3-dimethylbutanediol, 2,3-dimethylbutanediol, 1,4-dimethylbutanediol, diethylene glycol, triethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, bisphenol A, bisphenol F, hydrogenated bisphenol A, hydrogenated bisphenol F, etc.

[0051] The polyether polyol can be obtained by ring-opening polymerization of alkylene oxide and adding it to a polyol. Examples of the polyol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol, trimethylolpropane, etc. Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, tetrahydrofuran, etc.

[0052] Examples of the polyisocyanate include aliphatic diisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, 1,4-butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate; and isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4′-cyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexane diisocyanate, 1,3-bis(isocyanato)isocyanate. alicyclic diisocyanates such as toluene diisocyanate, 2,2′-diphenylmethane diisocyanate, 2,4′-diphenylmethane diisocyanate, 4,4′-diphenylmethane diisocyanate, 4,4′-diphenyldimethylmethane diisocyanate, 4,4′-dibenzyl diisocyanate, 1,5-naphthalene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate; aromatic aliphatic diisocyanates such as dialkyl diphenylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanate, α,α,α,α-tetramethylxylylene diisocyanate, etc.

[0053] The carbamate resin constituting the easy-adhesive layer 15 preferably has a carboxyl group. By making the carbamate resin have a carboxyl group, a cross-linked structure can be introduced, and there is a tendency to improve the bonding durability of the easy-adhesive film 1 and the polarizer, etc. The carbamate resin having a carboxyl group can be obtained, for example, by reacting a chain extender having a free carboxyl group on the basis of a polyol and a polyisocyanate. As chain extenders having free carboxyl groups, dihydroxycarboxylic acids, dihydroxysuccinic acid, etc. can be listed. As dihydroxycarboxylic acids, dihydroxyalkyl alkanoic acids such as dimethylol alkanoic acid (for example, dimethylol acetic acid, dimethylol butyric acid, dimethylol propionic acid, dimethylol butyric acid, dimethylol valeric acid) can be listed.

[0054] The method for producing the carbamate resin is not particularly limited, and may be any one of a one-step method in which the monomer components are reacted at once and a multi-stage method in which the monomer components are reacted in stages. When a chain extender having a free carboxyl group is used to introduce a carboxyl group into the carbamate resin, a multi-stage method is preferred. When producing the carbamate resin, a carbamate reaction catalyst may be used as needed.

[0055] The number average molecular weight of the urethane resin is preferably 5000 to 600000, more preferably 10000 to 400000. The acid value of the urethane resin is preferably 10 to 50, more preferably 20 to 45.

[0056] The carbamate resin may have a cross-linked structure. By introducing a cross-linked structure into the carbamate resin, there is a tendency that the bonding durability of the easy-to-bond film 1 and the polarizer etc. is improved. As a cross-linking agent, a cross-linking agent that can react with the cross-linking functional group of the carbamate resin can be used without particular restriction. In the case where the carbamate resin has a carboxyl group, a cross-linking agent comprising an amino group, an oxazoline group, an epoxy group, a carbodiimide group etc. can be used. Among these, a cross-linking agent having an oxazoline group is preferably used. Oxazoline groups have a low reactivity with carboxyl groups at room temperature, so the pot life when mixed with the carbamate resin is long, and the lead time (lead time) of the process can be flexibly dealt with.

[0057] The cross-linking agent can be a low molecular compound or a polymer. From the perspective of high solubility in water-based compositions and excellent compatibility with urethane resins, as a cross-linking agent, an acrylic acid polymer is preferred. When an acrylic acid polymer with an oxazoline group is particularly used as a cross-linking agent, there is a tendency that the adhesion of the film 1 to films such as polarizers is improved.

[0058] The amount of the cross-linking agent used is preferably 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, based on 100 parts by weight of the urethane resin.

[0059] (particle)

[0060] By making the easy bonding layer 15 include particles, thus forming a fine concavo-convex shape on the surface of the easy bonding layer, the slidability of the easy bonding film 1 is improved, and adhesion can be suppressed. From the viewpoint of forming the concavo-convex that helps to improve slidability and suppress adhesion, the particle size (average primary particle size) of the particles is preferably more than 0.1 times, more preferably more than 0.2 times, and more preferably more than 0.3 times of the thickness of the easy bonding layer. On the other hand, when the particle size of the particles is too large, sometimes the particles will fall off from the easy bonding layer and become the cause of poor appearance and adhesion. In addition, the particles that fall off sometimes adhere to conveyor rollers etc. and become the cause of scratches and damage. Therefore, the average primary particle size of the particles is preferably less than 0.9 times, more preferably less than 0.8 times, of the thickness of the easy bonding layer.

[0061] There is a tendency that the smaller the average particle size of the microparticles, the less scattering of visible light and the higher the transparency. The haze of the easy-adhesion film is preferably less than 2%, preferably less than 1.5%. From the viewpoint of suppressing the increase in haze caused by the microparticles, the average particle size of the microparticles is preferably less than 250nm, more preferably less than 200nm. When forming an easy-adhesion layer with a small thickness, from the viewpoint of suppressing the falling of the microparticles from the surface of the easy-adhesion layer, the average particle size of the microparticles is also preferably within the above range.

[0062] From the viewpoint of improving the dispersibility of the particles in the easy-adhesion layer and uniformly forming unevenness in the surface, the average particle size of the particles is preferably 10 nm or more, more preferably 15 nm or more, and further preferably 20 nm or more. In particular, from the viewpoint of ensuring dispersibility even at a low alkali content and suppressing unevenness in the polarizing plate caused by residual alkali, the average particle size of the particles is preferably 50 nm or more, and particularly preferably greater than 100 nm.

[0063] The particles of the easy-adhesion layer 15 may be inorganic particles or organic particles. From the perspective of excellent dispersibility and uniformity of particle size, inorganic particles are preferred as particles. As inorganic particles, inorganic oxides such as titanium oxide, aluminum oxide, and zirconium oxide can be listed; calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate, magnesium silicate, calcium phosphate, etc. can be listed. Among these, inorganic oxides are preferred. As organic particles, silicone resins, fluorine resins, acrylic resins, etc. can be listed. In order to suppress light scattering caused by particles, it is preferred that the refractive index difference between the binder resin (usually with a refractive index of about 1.5) and the particles is small. From the perspective of a small refractive index difference with the binder resin and excellent dispersibility, the particles of the easy-adhesion layer 15 are preferably silica particles.

[0064] When the easy-adhesion layer 15 is formed from an aqueous composition, it is preferred to use fine particles with high water dispersibility. An aqueous dispersion of fine particles may also be mixed into the composition. In order to improve the dispersibility of the fine particles, it is preferred to add an alkali component such as amine or ammonia to make the easy-adhesion composition weakly alkaline.

[0065] As water-dispersible silica particles, colloidal silica is preferably used. As colloidal silica, commercially available products such as Quartron.PL series manufactured by Fuso Chemical Industry Co., Ltd., SnowTex series manufactured by Nissan Chemical Industry Co., Ltd., AERODISP series and AEROSIL series manufactured by NIPPON AEROSIL Co., Ltd., and SEAHOSTAR KE series manufactured by Nippon Shokubai Co., Ltd. can be used.

[0066] From the viewpoint of improving the sliding property and blocking resistance of the easy-adhesion film 1 by forming the concavo-convex on the surface of the easy-adhesion layer 15, the content of the fine particles in the easy-adhesion layer 15 is preferably 3 wt% or more, more preferably 4 wt% or more. When the thickness of the easy-adhesion layer 15 is small (for example, when it is 260 nm or less), the sliding property and blocking resistance tend to be improved by increasing the content of fine particles to increase the amount of fine particles per unit area (number density) or by increasing the particle size of fine particles to increase the size of each concavo-convex (protrusion).

[0067] When the content of the particles in the easy-adhesion layer 15 is too large, it may sometimes lead to a decrease in optical properties caused by increased light scattering at the interface between the binder resin and the particles. In addition, when the content of the particles increases, it may sometimes become the cause of poor appearance caused by the aggregation of the particles and reduced adhesion caused by the relative content of the binder resin. Therefore, the content of the particles in the easy-adhesion layer 15 is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 30% by weight or less. The content of the particles in the easy-adhesion layer 15 may also be 20% by weight or less, 15% by weight or less, or 10% by weight or less.

[0068] (Residual alkali content)

[0069] When using alkali components such as amine and ammonia to improve the dispersibility of particles, the alkali components will inevitably remain in the easy bonding layer. When the easy bonding film 1 is used as a polarizer protective film, when the residual alkali amount of the easy bonding layer is too large, the penetration of the adhesive into the easy bonding layer is promoted, and it is difficult to form an adhesive layer at the interface with the polarizer, so sometimes the bonding force of the polarizer and the easy bonding film is reduced. In addition, when the residual alkali components of the easy bonding layer 15 are dissolved by water, the polarizer is sometimes degraded, resulting in optical defects such as reduced polarization degree and unevenness of the polarizer.

[0070] From the viewpoint of increasing the adhesive force of the easy-adhesive film and improving the humidification durability of the polarizing plate, the residual alkali content of the easy-adhesive layer 15 is preferably 200 ppm or less, more preferably 150 ppm or less. In particular, from the viewpoint of improving the humidification durability of the polarizing plate, the less the residual alkali content in the easy-adhesive layer 15, the more preferred it is, and the residual alkali content is preferably 100 ppm or less, more preferably 75 ppm or less. The residual alkali content may also be 70 ppm or less, 60 ppm or less, or 55 ppm or less.

[0071] On the other hand, when the residual alkali amount of the easy-adhesion layer 15 is too small, the dispersibility of the particles is impaired, and sometimes the appearance such as white turbidity caused by the aggregation of particles is produced. In addition, due to the aggregation of particles and the falling off of particles from the easy-adhesion layer caused by the reduction of dispersibility, appropriate concavo-convex is not formed on the surface of the easy-adhesion layer, and there is a tendency that the slip of the easy-adhesion film is reduced. Therefore, the residual alkali amount of the easy-adhesion layer 15 is preferably more than 3ppm, more preferably more than 5ppm, and further preferably more than 10ppm. The residual alkali amount can also be more than 15ppm, more than 20ppm, or more than 25ppm.

[0072] As the specific example of the residual alkali component in the easy-adhesion layer, amine and ammonia can be listed, and the total content of amine and ammonia in the preferred easy-adhesion layer is within the above range. The amount of alkali in the easy-adhesion layer can be quantitatively determined by liquid chromatography, ion chromatography, etc. according to the type of the alkali component. It is also possible to quantitatively determine the alkali component by combining chromatography with a mass spectrometry (MS) analysis method (such as LC / MS). In the case where the easy-adhesion layer includes a variety of alkali components, the total of each component is used as the alkali component content (residual amount) of the easy-adhesion layer.

[0073] As described above, within the range of not damaging the dispersibility of the particles, by increasing the content of the particles or increasing the particle size of the particles, the slip and adhesion resistance of the easy-adhesive film can be improved. From the viewpoint of suppressing the aggregation of the particles, it is preferred to use a method of using particles with large particle diameter within a range not exceeding 0.9 times or 0.8 times the thickness of the easy-adhesive layer. In the case of increasing the amount of particles with a small particle size, it is also possible to maintain dispersibility by increasing the amount of alkali added, but when increasing the amount of alkali added in order to improve the dispersibility of the particles, sometimes residual alkali will become the cause of the deterioration of the polarizer. In addition, if the time of heat treatment is extended in order to reduce the amount of residual alkali, sometimes productivity will be reduced.

[0074] Microparticles having a particle size greater than 100 nm also show good dispersibility at low alkali content, and are therefore advantageous from the perspective of improving both the sliding property and the anti-blocking property, as well as the durability of the polarizing plate. From the perspective of ensuring the dispersibility of the microparticles and maintaining the fixation of the microparticles to the easy-adhesion layer, the average primary particle size of the microparticles contained in the easy-adhesion layer is particularly preferably greater than 100 nm and less than 200 nm.

[0075] <Formation of Easy Adhesion Layer>

[0076] There is no particular limitation on the method for forming the easy-adhesion layer 15 on the surface of the film substrate 11. The easy-adhesion layer 15 is preferably formed by applying an easy-adhesion composition (coating liquid) containing a binder resin and fine particles onto the film substrate 11 and heating it.

[0077] (Easy-adhesive composition)

[0078] The easy-adhesion composition is preferably an aqueous composition using water as a solvent (and a dispersion medium for the fine particles). The concentration of the solid content (non-volatile content) in the easy-adhesion composition is preferably 1 to 30% by weight, more preferably 2 to 20% by weight, and further preferably 3 to 15% by weight.

[0079] The aqueous easy-adhesive composition comprises water as a solvent (and a dispersion medium), a binder resin or a precursor thereof, and microparticles. The easy-adhesive composition preferably further comprises an alkali component. As mentioned above, the alkali component has the function of promoting the dispersion of microparticles.

[0080] On the other hand, when the alkali contained in the easy-adhesion composition remains in the easy-adhesion layer, it may be the cause of reducing the moisture and heat resistance of the polarizer. In particular, even a small amount of strong alkali such as caustic soda may be the cause of polarizer degradation. Therefore, as the alkali component contained in the easy-adhesion composition, a weak base component such as ammonia and amine is preferred. From the viewpoint of improving the dispersibility of the particles and preventing the polarizer from deteriorating, the pH of the easy-adhesion composition (coating solution) is preferably about 7.5 to 9.

[0081] From the viewpoint of improving the dispersibility of the particles, the amount of the alkali component contained in the easy-adhesion composition is preferably 100 ppm or more, more preferably 300 ppm or more, and further preferably 500 ppm or more relative to the solid content of the easy-adhesion composition. On the other hand, when the content of the alkali component is too large, it is sometimes difficult to reduce the amount of residual alkali, so the amount of the alkali component contained in the easy-adhesion composition is preferably 50000 ppm or less, more preferably 10000 ppm or less, and further preferably 5000 ppm or less relative to the solid content of the easy-adhesion composition. The amount of the alkali component contained in the easy-adhesion composition can also be 4000 ppm or less or 3500 ppm or less relative to the solid content of the easy-adhesion composition. As mentioned above, as specific examples of the alkali components contained in the easy-adhesion composition, amines and ammonia can be listed, and the total content of these alkali components is preferably within the above range.

[0082] The alkali component contained in the easy-adhesion composition may be a substance having a catalytic effect in addition to improving the dispersibility of the particles. For example, when the binder resin is a carbamate resin, the easy-adhesion composition may contain a tertiary amine such as triethylamine as a urethanization catalyst for a polyurethane precursor (polyol, isocyanate, etc.).

[0083] By applying the easy-adhesive composition on the film substrate and then heating it, the alkali component can be volatilized and removed to reduce the residual alkali component of the easy-adhesive layer 15. From the viewpoint of promoting the volatilization of the alkali component based on heating, the alkali component contained in the easy-adhesive composition preferably has a boiling point of 150°C or less. The boiling point of the alkali component is more preferably below 130°C, further preferably below 120°C, and particularly preferably below 110°C. The boiling point of the alkali component may also be below 100°C or below 90°C. When the easy-adhesive composition contains a plurality of alkali components, it is preferred that the boiling point of at least one alkali component is within the above range, and it is preferred that the boiling points of two or more alkali components are within the above range. Relative to the total amount of alkali contained in the easy-adhesive layer, the boiling point of the alkali component of preferably 50% by weight or more is within the above range. It is ideal that the boiling points of all alkali components contained in the easy-adhesive composition are within the above range. For example, when the alkali component is amine and ammonia, it is preferred that the boiling point of the amine is within the above range.

[0084] The easy-adhesive composition may contain a crosslinking agent in addition to the binder resin (or its precursor), microparticles and an alkali component. The easy-adhesive composition may contain catalysts such as a crosslinking accelerator, antioxidants, ultraviolet absorbers, leveling agents, anti-blocking agents, antistatic agents, dispersion stabilizers, defoamers, thickeners, dispersants, surfactants, lubricants and other additives.

[0085] (Formation of an easy-adhesion layer on a film substrate)

[0086] Before applying the easy-adhesive composition on the film substrate 11, the film substrate may also be subjected to a surface treatment. By performing the surface treatment, the wetting tension of the film substrate can be adjusted to improve the adhesion with the easy-adhesive layer 15. As the surface treatment, corona treatment, plasma treatment, ozone blowing, ultraviolet irradiation, flame treatment, chemical treatment, etc. can be listed. Among these, corona treatment or plasma treatment is preferred.

[0087] As the coating method of the easy bonding composition, rod coating, roller coating, gravure coating, rod coating, slot coating, curtain coating, injection coating etc. can be listed. The easy bonding layer 15 is formed by removing the solvent from the easy bonding composition after heating the coating. It is also possible to react the precursor material of the binder resin and solidify it by heating. For example, when the easy bonding composition includes a crosslinking agent, the crosslinking reaction can be promoted by heating.

[0088] The heating temperature during the formation of the easy-adhesion layer is, for example, about 50 to 200° C. From the viewpoint of promoting the curing reaction of the resin component in the easy-adhesion composition and efficiently volatilizing and removing the alkali component contained in the easy-adhesion composition, the heating temperature is preferably 100° C. or higher, more preferably 120° C. or higher, further preferably 130° C. or higher, and particularly preferably 135° C. or higher. In addition, the heating temperature is preferably higher than the boiling point of the alkali component contained in the easy-adhesion composition.

[0089] The heating temperature when forming the easy-adhesion layer is preferably a temperature higher than the glass transition temperature (Tg) of the film substrate. By heating at a high temperature, the curing reaction of the resin component in the easy-adhesion composition can be promoted, and the alkali component contained in the easy-adhesion composition can be volatilized and removed efficiently. The heating temperature is preferably a temperature higher than the Tg of the film substrate by 10°C or more.

[0090] It is believed that by heating at a temperature higher than the Tg of the film substrate, the volatilization removal efficiency of the alkali in the easy-adhesion composition can be improved, and the easy-adhesion composition becomes easy to penetrate into the surface of the film substrate, thereby improving the adhesion between the film substrate 11 and the easy-adhesion layer 15. From the viewpoint of improving the adhesion of the easy-adhesion layer, the heating temperature is preferably Tg of the film substrate + 10°C or more, more preferably Tg + 15°C or more, and further preferably Tg + 20°C or more.

[0091] When heated at a temperature higher than Tg+10°C of the film substrate, the film substrate changes from a glass state to a rubber state, and the surface becomes easily deformed, so an interface layer in which the resin component of the film substrate and the constituent components of the easy adhesion layer are mixed is easily formed at the interface between the film substrate 11 and the easy adhesion layer 15. By forming the interface layer, there is a tendency for the adhesion between the film substrate 11 and the easy adhesion layer 15 to be improved.

[0092] In particular, when there is a region on the surface of the film substrate 11 where the particles of the easy-adhesion layer 15 are embedded and buried, an easy-adhesion film having high adhesion between the film substrate 11 and the easy-adhesion layer 15 can be obtained. It is considered that when the film substrate is heated to a rubber state formed at a temperature higher than Tg, the particles are embedded in the film substrate, and when the film substrate is subsequently restored to a glass state, the particles embedded in the surface of the film substrate and the binder resin existing around them are fixed to the surface of the film substrate, thereby improving the adhesion between the film substrate 11 and the easy-adhesion layer 15.

[0093] The easy-adhesive layer can also be formed in the manufacturing process of the film substrate. In addition, the easy-adhesive layer can also be formed by heating when the film substrate is formed. For example, in the case where the film substrate is a stretched film, the easy-adhesive composition can be applied to the surface of the film before stretching or the film after longitudinal stretching, and the solvent can be dried and the resin can be cured by heating during transverse stretching or simultaneous biaxial stretching based on a tenter.

[0094] In the case of stretching the film substrate after applying the easy-adhesive composition, from the viewpoint of suppressing the undesirable conditions such as cracks in the easy-adhesive layer, the stretching ratio is preferably less than 5 times, more preferably less than 4 times, further preferably less than 3 times, and particularly preferably less than 2.5 times. The lower limit of the stretching ratio is not particularly limited, but from the viewpoint of improving film strength, the stretching ratio is preferably more than 1.3 times, more preferably more than 1.5 times. When the film substrate is an acrylic film, from the viewpoint of improving film strength, it is preferably stretched along the conveying direction (MD) and the width direction (TD) respectively with the above-mentioned stretching ratio.

[0095] When biaxial stretching of the film substrate is performed, the biaxial stretching can be successive biaxial stretching or simultaneous biaxial stretching. In addition, oblique stretching can also be performed. When biaxial stretching is performed successively, it is also possible to apply the easy bonding composition on the film after stretching the film along 1 direction (MD) by roller stretching as described above, and heating the easy bonding composition when stretching based on a tenter.

[0096] As described above as the heating temperature of the easy-adhesion layer, the stretching temperature is preferably a temperature higher than the Tg of the film substrate, preferably Tg+10°C or more, more preferably Tg+15°C or more, and further preferably Tg+20°C or more. It is particularly preferred that the film is stretched in at least one direction at the above temperature after the easy-adhesion composition is applied. When the film substrate is stretched in a rubber state at a temperature higher than the Tg of the film substrate, a region in which the particles in the easy-adhesion composition are buried is easily formed on the surface of the film substrate, and there is a tendency for the adhesion between the film substrate 11 and the easy-adhesion layer 15 to be improved. As a reason for easily burying particles in the film substrate by stretching at high temperature, it can be cited that when the film substrate is stretched in a rubber state, the easy-adhesion composition is easily wetted and diffused when the film substrate is deformed, and it is easy to form a state in which the particles are embedded in the concave part of the surface concave and convex formed when the film substrate is deformed. In addition, it can be considered that if the stress is released and the film substrate is cooled after stretching, the particles embedded in the surface of the film substrate are fixed when the film substrate shrinks, so it is easy to form a region in which the particles are buried in the film substrate.

[0097] By adjusting the solid content concentration and coating thickness of the adhesive composition, the thickness of the adhesive layer 15 can be adjusted. When the film substrate is stretched after coating the adhesive composition, the thickness of the adhesive layer 15 can also be adjusted by the stretching ratio.

[0098] The thickness of easy bonding layer 15 is not particularly limited, but from the viewpoint of promoting the removal of alkali components based on heating, it is preferably below 260nm, more preferably below 250nm. The thickness of easy bonding layer can also be below 240nm, below 230nm or below 220nm. When easy bonding film 1 is used as polarizer protective film, the thickness of easy bonding layer 15 is smaller, the humidification durability of polarizer is improved, the occurrence of optical bad spots such as striped unevenness is reduced. In addition, the thickness of easy bonding layer 15 is smaller, and the degree of polarization when polarizer is exposed to humidification environment is reduced, which is more suppressed.

[0099] When the easy-adhesive composition is heated and dried, if the alkali component is excessively removed, the dispersibility of the particles in the binder resin is reduced, and it is easy to produce the aggregation of particles and the resulting particles from the easy-adhesive layer surface. When the aggregation and fall of particles are produced, the sliding property of the easy-adhesive film is reduced, and it is easy to produce damage during transportation and adhesion during winding. In addition, it may become the cause of pollution of the process caused by the particles that fall off, damage caused by the particles attached to the conveying roller, and scratches. Therefore, the thickness of the easy-adhesive layer 15 is preferably more than 100nm. In addition, the greater the thickness of the easy-adhesive layer, the more the adhesion to the film, glass, etc. such as the polarizer is improved. From the viewpoint of improving adhesion, the thickness of the easy-adhesive layer 15 is preferably more than 120nm. The thickness of the easy-adhesive layer can also be more than 130nm, more than 140nm, more than 150nm, or more than 160nm.

[0100] [Polarizing plate]

[0101] The polarizing plate may have a transparent protective film on only one side of the polarizer, or Figure 2 As shown in FIG. 1 , a polarizer 5 is provided with a transparent protective film on both sides. By laminating the above-mentioned easy-adhesion film as a polarizer protective film on one side of the polarizer, a polarizing plate having a transparent protective film only on one side of the polarizer can be formed. Regarding a polarizing plate having a polarizer protective film on both sides of the polarizer, the above-mentioned easy-adhesion film can be laminating on at least one side of the polarizer. The polarizing plate can also have the above-mentioned easy-adhesion film laminating on both sides of the polarizer. The polarizer 5 and the easy-adhesion film 1 are laminating with the aid of an adhesive layer 6.

[0102] <Polarizer>

[0103] As the polarizer 5, a polyvinyl alcohol (PVA) polarizer can be used, in which a polyvinyl alcohol film such as polyvinyl alcohol or partially methylated polyvinyl alcohol is adsorbed with a dichroic substance such as iodine or a dichroic dye and oriented in one direction. For example, a PVA polarizer can be obtained by dyeing a polyvinyl alcohol film with iodine and stretching it.

[0104] In the manufacturing process of the polarizer 5, water washing, swelling, cross-linking and other treatments may be performed as needed. Stretching may be performed before or after iodine dyeing, or while dyeing. Stretching may be performed by stretching in the air (dry stretching), or in water or in an aqueous solution containing boric acid, potassium iodide, etc. (wet stretching), or a combination of these may be used. The film thickness of the polarizer 5 is not particularly limited, and is usually about 1 to 50 μm.

[0105] As the polarizer 5, a thin PVA-based polarizer with a thickness of less than 10 μm can also be used. As a thin polarizer, for example, thin polarizers recorded in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, WO2010 / 100917, Japanese Patent No. 4691205 Specification, Japanese Patent No. 4751481 Specification, etc. can be cited. These thin polarizers can be obtained by a method comprising a process of stretching a PVA-based resin layer and a stretching resin substrate in a laminate state and an iodine dyeing process. If it is this method, even if the PVA-based resin layer is thin, it will be supported by the stretching resin substrate, so it can be stretched without undesirable conditions such as breakage caused by stretching.

[0106] <Adhesive>

[0107] As long as the adhesive layer 6 for bonding the polarizer 5 and the easy-bonding film 1 is optically transparent, there is no particular restriction on the material thereof, and examples thereof include epoxy resins, silicone resins, acrylic resins, polyurethanes, polyamides, polyethers, polyvinyl alcohol, and the like. The thickness of the adhesive layer 6 is, for example, about 0.01 to 20 μm, and can be appropriately set according to the type of adherend, the material of the adhesive, and the like. When a curing adhesive that exhibits adhesion through a cross-linking reaction after coating is used, the thickness of the adhesive layer 6 is preferably 0.01 to 5 μm, and more preferably 0.03 to 3 μm.

[0108] As the adhesive, various adhesives can be used, such as water-based adhesives, solvent-based adhesives, hot melt adhesives, active energy ray-curable adhesives, etc. Among these, water-based adhesives or active energy ray-curable adhesives are preferred because they can reduce the thickness of the adhesive layer.

[0109] As the polymer component of the water-based adhesive, vinyl polymer, gelatin, vinyl latex, polyurethane, polyester, epoxy, etc. can be exemplified. Among these, vinyl polymer is preferred from the aspect of excellent adhesion between the easy-to-bond film and the polarizer, and polyvinyl alcohol resin is particularly preferred. Among the polyvinyl alcohol resins, polyvinyl alcohol containing acetoacetyl groups is preferred.

[0110] From the viewpoint of adhesiveness, the average degree of polymerization of the polyvinyl alcohol-based resin is preferably about 100 to 5000, and more preferably 1000 to 4000. The average degree of saponification of the polyvinyl alcohol-based resin is preferably 85 mol % or more, and more preferably 90 mol % or more.

[0111] In addition to polymers such as polyvinyl alcohol resins, aqueous adhesive compositions (solutions) may also contain crosslinking agents. As crosslinking agents, compounds having at least two functional groups reactive with the polymers constituting the adhesive in one molecule may be used. Examples of crosslinking agents for polyvinyl alcohol resins include: alkylenediamines; isocyanates; epoxies; aldehydes; amino-formaldehydes such as methylol urea and methylol melamine. Among these, amino-formaldehyde is preferred. As amino-formaldehyde resins, compounds having methylol groups are preferred, and methylol melamine is particularly preferred. The amount of the crosslinking agent in the adhesive composition is preferably about 10 to 60 parts by weight, and more preferably 20 to 50 parts by weight, relative to 100 parts by weight of the polyvinyl alcohol resin.

[0112] Active energy ray curing adhesives are adhesives that can be free radical polymerized, cationic polymerized, or anionic polymerized by irradiation with active energy rays such as electron beams and ultraviolet rays. Among them, from the aspect of being able to be cured with low energy, photoradical polymerizable adhesives, photocationic polymerizable adhesives, or hybrid adhesives using a combination of photocationic polymerization and photoradical polymerization are preferred.

[0113] As monomers of the radical polymerizable adhesive, compounds having a (meth)acryloyl group and compounds having a vinyl group can be cited. Among them, compounds having a (meth)acryloyl group are preferred. As compounds having a (meth)acryloyl group, (meth)acrylic acid C 1-20 Alkyl (meth)acrylates such as chain alkyl esters, alicyclic (meth)acrylates, and polycyclic (meth)acrylates; (meth)acrylates containing hydroxyl groups; (meth)acrylates containing epoxy groups such as glycidyl (meth)acrylates, etc. The radical polymerizable adhesive may contain nitrogen-containing monomers such as hydroxyethyl (meth)acrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, (meth)acrylamide, and (meth)acryloyl morpholine. The radical polymerizable adhesive may also contain polyfunctional monomers such as tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, cyclic trimethylolpropane formal acrylate, dioxanediol diacrylate, and EO-modified diglycerol tetraacrylate as crosslinking components.

[0114] As the curable component of the cationic polymerizable adhesive, compounds having an epoxy group and an oxetane group can be cited. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various generally known curable epoxy compounds can be used. As preferred epoxy compounds, compounds having at least two epoxy groups and at least one aromatic ring in the molecule (aromatic epoxy compounds) can be cited; compounds having at least two epoxy groups in the molecule, at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring, etc. (alicyclic epoxy compounds). A mixed adhesive can also be prepared by making the cationic polymerizable adhesive contain a free radical polymerizable compound such as a compound having a (meth)acryloyl group.

[0115] The photocurable adhesive preferably contains a photopolymerization initiator. The photopolymerization initiator can be appropriately selected according to the reaction species. For example, in a radical polymerizable adhesive, as a photopolymerization initiator, it is preferred to mix a photoradical generator that generates free radicals by light irradiation. In a cationic polymerizable adhesive, as a photopolymerization initiator, it is preferred to mix a photocationic polymerization initiator (photoacid generator) that generates cationic species or Lewis acids by light irradiation. In a mixed adhesive, it is preferred to mix a photocationic polymerization initiator and a photoradical generator.

[0116] The content of the polymerization initiator is generally about 0.1 to 10 parts by weight, preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the monomer. It should be noted that when the free radical polymerizable adhesive is used as an electron beam curing type, a photopolymerization initiator is not particularly required. In order to increase the curing speed and sensitivity, a photosensitizer may also be added to the active energy ray curing adhesive as needed. The amount of the photosensitizer used is generally about 0.001 to 10 parts by weight, preferably 0.01 to 3 parts by weight, relative to 100 parts by weight of the monomer.

[0117] The adhesive may contain appropriate additives as required. Examples of additives include coupling agents such as silane coupling agents and titanate coupling agents, adhesion promoters such as ethylene oxide, ultraviolet absorbers, anti-degradation agents, dyes, processing aids, ion capture agents, antioxidants, tackifiers, fillers, plasticizers, leveling agents, foaming inhibitors, antistatic agents, heat stabilizers, hydrolysis stabilizers, etc.

[0118] [Production of polarizing plate]

[0119] The polarizing plate can be manufactured by laminating the easy-adhesion film 1 to one surface (first main surface) of the polarizer 5 via the adhesive layer 6. The easy-adhesion film 1 can be laminated to the polarizer 5 via the adhesive layer on the surface where the easy-adhesion layer is formed, or laminated to the polarizer 5 via the adhesive layer on the surface where the easy-adhesion layer is not formed. Figure 2As shown, by sandwiching the adhesive layer 6 and bonding the polarizer 5 to the easy bonding layer 15 of the easy bonding film 1, a polarizing plate having high adhesion between the polarizer and the polarizer protective film (easy bonding film 1), excellent mechanical strength and durability can be obtained. In the case where the easy bonding layer is not formed on the surface and is bonded to the polarizer 5 with the help of the adhesive layer, the adhesion with other films, adhesive layers, glass substrates, etc. provided on the easy bonding film can be improved.

[0120] In the lamination of the polarizer 5 and the easy-adhesive film 1, it is preferred that: after applying the adhesive composition to either or both of the polarizer 5 and the easy-adhesive film 1, the polarizer 5 and the easy-adhesive film 1 are laminated by a roll laminator or the like, and the adhesive is cured. As a coating method of the adhesive composition to the polarizer 5 and / or the easy-adhesive film 1, a roller method, a spray method, a dipping method, etc. can be listed. Before applying the adhesive composition to the surface of the polarizer 5 and / or the easy-adhesive film 1, a surface treatment such as a corona treatment, a plasma treatment, a saponification treatment, etc. can also be performed.

[0121] After the polarizer 5 and the easy-adhesion film 1 are bonded together, the adhesive layer 6 is formed by curing the adhesive according to the type of the adhesive. When a water-based adhesive is used, the adhesive is cured by heating and drying. When an active energy ray-curable adhesive is used, the adhesive is cured by irradiation with active energy rays such as electron beams and ultraviolet rays.

[0122] <Transparent protective film>

[0123] A transparent protective film 2 may also be bonded to the second main surface of the polarizer 5 by means of an adhesive layer 7. As the transparent protective film 2, any appropriate transparent film may be used. The thickness of the transparent protective film 2 is about 5 to 200 μm. From the viewpoints of mechanical strength, transparency, and operability, the thickness of the transparent protective film 2 is preferably 10 to 100 μm, and more preferably 15 to 60 μm. The thickness of the easy-adhesion film 1 and the transparent protective film 2 may be the same or different.

[0124] Examples of materials for forming the transparent protective film 2 include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN); cellulose polymers such as diacetyl cellulose and triacetyl cellulose; styrene polymers such as polystyrene and acrylonitrile-styrene copolymer; cyclic polyolefins such as polynorbornene; and polycarbonate.

[0125] The transparent protective film 2 may include an easy-adhesion layer (not shown) on the surface to be bonded to the polarizer 5. The transparent protective film 2 may be provided with an easy-adhesion layer similar to the easy-adhesion layer 15 of the easy-adhesion film 1.

[0126] As adhesive layer 7 for bonding polarizer 5 and transparent protective film 2, various adhesives such as water-based adhesives, solvent-based adhesives, hot melt adhesives, and active energy ray-curable adhesives can be used. Adhesive layer 6 and adhesive layer 7 can use the same adhesive composition.

[0127] [Use of polarizing plate]

[0128] An adhesive layer for bonding a liquid crystal unit, an organic EL unit, etc. may be provided on the polarizing plate. As the adhesive forming the adhesive layer, an adhesive based on a polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer, etc. may be appropriately selected and used. In particular, an acrylic adhesive is preferred from the aspects of excellent optical transparency, moderate wettability and cohesion, and excellent weather resistance, heat resistance, etc.

[0129] The adhesive layer can be attached to the polarizing plate in an appropriate manner. For example, an adhesive solution having a solid content concentration of about 10 to 40% by weight is prepared by dissolving or dispersing a base polymer in a solvent such as toluene or ethyl acetate, and the adhesive solution is attached to the polarizing plate, or an adhesive layer formed on a suitable substrate is transferred to the polarizing plate.

[0130] Adhesive layers may be provided on both sides of the polarizing plate. When adhesive layers are provided on both sides of the polarizing plate, the composition and thickness of the adhesive layers on the front and back sides may be the same or different. The thickness of the adhesive layer is usually about 5 to 500 μm.

[0131] A release film may be temporarily attached to the surface of the adhesive layer for the purpose of preventing contamination of the adhesive layer, etc. As the release film, a release film obtained by coating the surface of a plastic film with a release agent such as a silicone release agent, a long-chain alkyl release agent, or a fluorine release agent is preferably used.

[0132] The polarizing plate may be a laminated polarizing plate laminated with other optical layers. Examples of the optical layer include a phase difference plate, a viewing angle compensation film, and a brightness enhancement film.

[0133] By laminating a polarizing plate to the surface of an image display unit such as a liquid crystal unit and an organic EL unit, an image display device can be formed. Regarding the formation of a liquid crystal display device, it is formed by appropriately assembling a liquid crystal unit and a polarizing plate, and components such as a lighting system as required, and incorporating a drive circuit, etc. In an organic EL display device, by laminating a circular polarizing plate composed of a combination of the polarizing plate of the present invention and a phase difference film (typically a 1 / 4 wavelength plate) on the surface of an organic EL unit, the re-emission of reflected light from external light caused by a metal electrode, etc., can be reduced, thereby improving visibility.

[0134] Example

[0135] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. The following descriptions of "%" are weight % unless otherwise specified.

[0136] [Preparation of easy-adhesion composition]

[0137] <Easy-adhesive composition A>

[0138] An easy-adhesion composition A was prepared by mixing 20.6 parts by weight of an aqueous polyurethane having a solid content of 34% ("Super Flex 210R" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) containing polyester urethane and isophorone diisocyanate as resin components, triethylamine as a curing catalyst, and methyl ethyl ketone as a dispersion medium, 5.2 parts by weight of an aqueous solution of an oxazoline-containing polymer having a solid content of 25% ("Epocros WS-700" manufactured by Nippon Shokubai Co., Ltd.), 7.5 parts by weight of a 20% aqueous dispersion of colloidal silica having an average primary particle size of 35 nm, 3.0 parts by weight of 1% ammonia water, and 63.7 parts by weight of pure water. The easy-adhesive composition contains polyurethane and oxazoline-containing polymer (cross-linking agent) as resin components in a weight ratio of 84.3:15.7, and is a 10% aqueous solution containing 15.3 weight parts of silica particles per 100 weight parts of solid content (the total of resin component and particles), and the ammonia concentration in the aqueous solution is 300 ppm (3000 ppm relative to the solid content).

[0139] <Easy-adhesive compositions B to G>

[0140] The type (particle size) and blending amount of silica particles and the blending amount of the resin component (water-based polyurethane resin and oxazoline-containing polymer as a crosslinking agent) were changed as shown in Table 1 to prepare an easy-adhesive composition with a concentration of 10%. In any composition, the amount of ammonia water added was adjusted so that the ammonia concentration in the solution was 300 ppm. The details of the silica particles are as follows.

[0141] PL-3: 20% aqueous dispersion of spherical silica having an average primary particle size of 35 nm ("Quartron PL-3" manufactured by Fuso Chemical Industries, Ltd.)

[0142] KE-W10: 15% aqueous dispersion of spherical silica having an average primary particle size of 110 nm ("SEAHORSTAR KE-W10" manufactured by Nippon Shokubai Co., Ltd.)

[0143] TECHNO CHEMICAL: Spherical silica particles with an average primary particle size of 150 nm ("Silica Microsphere Plane 24320-15" manufactured by TECHNO CHEMICAL Corp.)

[0144] KE-W30: 20% aqueous dispersion of spherical silica having an average primary particle size of 280 nm ("SEAHORSTAR KE-W30" manufactured by Nippon Shokubai Co., Ltd.)

[0145] Table 1 shows the compositions of the easy-adhesion compositions A to G (content of each component relative to 100 parts by weight of the total solid content, and ammonia concentration in the composition (aqueous solution)).

[0146] [Table 1]

[0147]

[0148] [Production of easy-adhesion film]

[0149] <Example 1>

[0150] An easy-to-adhesive film is prepared using a film manufacturing device equipped with a melt extrusion film-making device, a gravure coater, a tenter-type simultaneous biaxial stretching device, and a winding device. As an acrylic resin, pellets of the same imidized MS resin (glass transition temperature: 120°C) as the material used in the preparation of the "transparent protective film 1A" described in the embodiment of Japanese Patent Publication No. 2017-26939 are used. The acrylic resin is melt-extruded from a T die and film-formed with a thickness of 160 μm. The above-mentioned easy-to-adhesive composition C is applied to one side of the film with a wet thickness of about 9 μm using a gravure coater. In a heating furnace at a temperature of 140°C, the film is stretched to 2 times in the length direction (MD) and the width direction (TD) using a simultaneous biaxial stretching tenter, and an easy-to-adhesive film having an easy-to-adhesive layer with a thickness of 200 nm is obtained on one side of an acrylic film with a thickness of 40 μm.

[0151] <Examples 2 to 13 and Comparative Examples 1 to 5>

[0152] An easily adhesive film was obtained in the same manner as in Example 1 except that the type of the easily adhesive composition, the coating thickness and the stretching temperature were changed as shown in Table 3. Table 3 shows the thickness of the easily adhesive layer (after stretching).

[0153] <Comparative Example 6>

[0154] Except that the easy-adhesion composition was not applied, melt extrusion and simultaneous biaxial stretching of the acrylic resin were performed in the same manner as in Example 1 to obtain an acrylic film having a thickness of 40 μm. The easy-adhesion composition D was applied to one surface of the acrylic film at a wet thickness of about 2 μm, and dried at 140° C. for 30 seconds to obtain an easy-adhesion film having an easy-adhesion layer having a thickness of 200 nm formed on one surface of the acrylic film.

[0155] [Evaluation of easy-adhesion films]

[0156] The following evaluations were performed on the easily adhesive films produced above.

[0157] <Residual Alkali Amount in Easy Adhesion Layer>

[0158] The amount of triethylamine and ammonia remaining in the easy-adhesion layer was quantified. Regarding the residual amount of triethylamine, the powder obtained by scraping off the easy-adhesion layer from the surface of the easy-adhesion film was weighed and dissolved in methanol, and the solution was quantified by gas chromatography-mass spectrometry (GC / MS). Regarding the residual amount of ammonia, the easy-adhesion film was immersed in pure water at 25°C, and then heated and extracted in a dryer at 120°C for 60 minutes, and the ammonia dissolved in the water was quantified by ion chromatography. The total amount of triethylamine and the amount of ammonia was taken as the residual alkali amount.

[0159] <Presence or absence of interface layer>

[0160] The cross section of the easy adhesion film was observed with a transmission electron microscope (TEM) to confirm whether there was a region (interface layer) where the particles in the easy adhesion layer were buried in the acrylic film at the interface between the acrylic film and the easy adhesion layer.

[0161] <Particle Dispersibility>

[0162] The surface of the easy-adhesion film was visually observed, and the presence or absence of local turbidity (increased haze) due to aggregation of silica particles was evaluated according to the following criteria.

[0163] ○: No aggregation of silica particles, good uniformity within the surface

[0164] △: Slight turbidity due to aggregation of silica particles was observed

[0165] ×: Turbidity caused by aggregation of silica particles was clearly observed

[0166] <Fixability of Particles>

[0167] The surface of the easy-to-bond film was visually observed to determine the particle fixation according to the following criteria based on the presence or absence of scratches or marks caused by the dropped particles during roller conveyance.

[0168] ○: No scratches or damage caused by particles were found

[0169] ×: Scratches and / or scratches caused by fallen particles are observed

[0170] <Haze of Easy Adhesion Film>

[0171] The haze of the easy-adhesion film was measured using a haze meter ("HM-150" manufactured by Murakami Color Research Laboratory), and a value of less than 1.5% was indicated as "0", and a value of 1.5% or more was indicated as "×".

[0172] <Blocking resistance>

[0173] After the easy-adhesive film was wound into a roll, the film was unwound from the roll to evaluate the presence of wrinkles caused by blocking. After the film was stored at room temperature for 72 hours in the wound state, the film was unwound from the roll again to evaluate the presence of wrinkles caused by blocking.

[0174] ○: No wrinkles were observed when unwinding from the roll immediately after winding and when unwinding from the roll after 72 hours of storage.

[0175] △: No wrinkles were observed when the roll was unwound immediately after winding, but wrinkles were observed when the roll was unwound after 72 hours of storage.

[0176] ×: Wrinkles were observed when unwinding the roll immediately after winding and when unwinding the roll after 72 hours of storage.

[0177] <Adhesion of the Easy Adhesion Layer>

[0178] An adhesive tape ("No. 31B" manufactured by Nitto Denko Corporation) was surface-bonded to the easy-bonding layer of the easy-bonding film at a linear pressure of 8 kg / m and a bonding speed of 0.3 m / min. After being stored at 50°C for 48 hours, a 180° peel test was performed by holding the front end of the adhesive tape and at a tensile speed of 30 m / min. The adhesion of the easy-bonding layer was determined according to the following criteria.

[0179] ○: The easy-adhesion layer was not peeled off from the acrylic film, but peeled off at the interface between the pressure-sensitive adhesive tape and the easy-adhesion layer.

[0180] ×: Peeling occurred at the interface between the acrylic film and the easy-adhesion layer

[0181] [Production of polarizing plate]

[0182] (Production of polarizer)

[0183] A long roll of a polyvinyl alcohol (PVA) resin film ("PE4500" manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm was uniaxially stretched in the longitudinal direction to 5.9 times in the longitudinal direction by a roll stretching machine, and the swelling bath, dyeing bath, crosslinking bath 1, crosslinking bath 2, and cleaning bath shown in Table 2 were sequentially conveyed and dried at 70° C. for 5 minutes to prepare a polarizer having a thickness of 18 μm. The iodine concentration and potassium iodide concentration in the dyeing bath were adjusted so that the single body transmittance of the polarizer was 43.4%.

[0184] [Table 2]

[0185] Aqueous solution composition Temperature(℃) Stretch ratio Swelling bath Pure water 20 2.2 dye bath Iodine: Potassium iodide = 1:7 (weight ratio) 30 1.4 Crosslinking bath 1 5.0% boric acid, 3.0% potassium iodide 40 1.2 Crosslinking bath 2 4.3% boric acid, 5.0% potassium iodide 65 1.6 Cleansing Bath 2.6% Potassium iodide 20 -

[0186] (Preparation of UV-curable adhesive)

[0187] An ultraviolet curable adhesive was prepared containing 40 parts by weight of N-hydroxyethylacrylamide and 60 parts by weight of acryloylmorpholine as curable components and 3 parts by weight of 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one ("Irgacure 819" manufactured by BASF Corporation) as a polymerization initiator.

[0188] (Lamination of polarizer and polarizer protective film)

[0189] As the polarizer protective film on one side, the easy-adhesive film of each embodiment and comparative example was used, and as the polarizer protective film on the other side, a biaxially stretched cyclic polyolefin film ("ZEONOR Film ZF-14" manufactured by Zeonor Co., Ltd., Japan) was used. The above-mentioned ultraviolet curing adhesive was applied to the easy-adhesive layer forming surface of the easy-adhesive film and the surface of the ZEONOR film with a thickness of about 1 μm, and after being attached to the polarizer using a roll laminator, the accumulated light amount was irradiated at 1000 / mJ / cm 2 The adhesive was cured by ultraviolet rays to obtain a polarizing plate having an acrylic film (easy-adhesive film) on one side of the polarizer and a ZEONOR film on the other side.

[0190] [Evaluation of polarizing plates]

[0191] The following evaluations were performed on the easily adhesive films produced above.

[0192] <Measurement of Adhesive Strength>

[0193] The polarizing plate is cut into a size of 200mm in the direction parallel to the tensile direction of the polarizer (absorption axis direction) and 20mm in the orthogonal direction (transmission axis direction), and a cutter is used to cut a notch between the easy-bonding film and the polarizer, and the polarizing plate is attached to the glass plate. Using a tensile compression tester (MINEBEA "TG-1kN"), a peeling test is performed with a peeling angle of 90 ° and a peeling speed of 1000mm / minute to measure the adhesive force. The case where the adhesive force is more than 2.4N / 20mm is recorded as "0", the case where the adhesive force is more than 1.6N / 20mm and less than 2.4N / 20mm is recorded as "△", and the case where the adhesive force is less than 1.6N / 20mm is recorded as "×".

[0194] <Humidification durability of polarizing plate>

[0195] The polarizing plate was cut into a size of 320 mm × 240 mm, and the surface of the cyclic polyolefin film side was bonded to the glass with a 20 μm thick acrylic adhesive. The sample was placed in a constant temperature and humidity chamber at a temperature of 60°C and a relative humidity of 90% for 500 hours, and a heating / humidification durability test was performed. Another polarizing plate was configured with a cross prism on the polarizing plate after the durability test, and the presence or absence of streaky unevenness and the overall uniformity of the surface (whether there is surface unevenness) were confirmed by visual observation, and the evaluation was performed according to the following criteria.

[0196] (Uneven stripes)

[0197] ○: No streak-like unevenness was observed

[0198] △: Slight streak-like unevenness is detected

[0199] ×: Stripe-like unevenness is clearly recognized

[0200] (Uneven surface)

[0201] ○: Uniform in the surface, no unevenness was observed

[0202] △: Slight unevenness is visible on the surface

[0203] ×: Unevenness is visible throughout the surface

[0204] Table 3 shows the production conditions of the easy-adhesive films of the embodiments and comparative examples (type of easy-adhesive composition, stretching timing (stretching before or after coating of the easy-adhesive composition), stretching temperature, thickness of the easy-adhesive layer), evaluation results of the easy-adhesive films (residual alkali content, presence or absence of an interface layer, dispersion and fixation of particles, haze, blocking resistance, and adhesion), and evaluation results of the polarizing plate (adhesion between the polarizer and the easy-adhesive film, and presence or absence of unevenness after a durability test).

[0205] [Table 3]

[0206]

[0207] In Comparative Examples 1 to 3 in which the thickness of the easy-adhesive layer is 300 nm, stripe-like unevenness was confirmed after the durability test of any polarizing plate. In Comparative Example 6 in which the easy-adhesive layer is formed by coating the stretched film with an easy-adhesive composition, the amount of residual alkali is large, and the adhesion between the easy-adhesive film and the polarizer is insufficient. In addition, in Comparative Example 6, in addition to the stripe-like unevenness visible in the polarizing plate after the durability test, the entire surface also has unevenness. It is believed that the reduced adhesion in Comparative Example 6 and the unevenness after the durability test are caused by the residual alkali component in the easy-adhesive layer.

[0208] In Comparative Example 4, which used particles having a particle size equal to the thickness of the easy-adhesion layer, scratches with a spacing equal to the circumference of the conveying roller were confirmed in the easy-adhesion film. It is believed that this is caused by process contamination caused by the particles that fall off. In Comparative Example 5, which used particles having a particle size larger than the thickness of the easy-adhesion layer, scratches with spacing were confirmed in the same manner as in Comparative Example 4.

[0209] In Example 13 and Comparative Example 4, where the thickness of the easy-adhesion layer was 150 nm, the adhesion between the polarizer and the easy-adhesion film was smaller than that of the other examples. These results show that the thicker the easy-adhesion layer, the higher the adhesion tends to be.

[0210] The easily adhesive films of Examples 1 to 12 had no defect in appearance due to the falling of particles. In addition, no unevenness was observed in the polarizing plate after the durability test, and the polarizing plate had a good appearance.

[0211] In the embodiment 9 provided with the easy-adhesive layer containing 5 weight % of particles with an average particle size of 35nm, the blocking resistance is reduced compared with other embodiments. On the other hand, the embodiments 2, 3, 11, 13 containing 5 weight % of particles with an average particle size of 150nm and the embodiments 5 and 6 containing 5 weight % of particles with an average particle size of 110nm show excellent blocking resistance. In addition, the embodiments 7 and 8 containing 15 weight % of particles with an average particle size of 35nm also show excellent blocking resistance. According to these results, it can be seen that increasing the particle size of the particles of the easy-adhesive layer and increasing the content of the particles are useful for improving the blocking resistance.

[0212] In Example 8, which contains 15% particles with an average particle size of 35 nm, a decrease in the dispersibility of the particles can be observed. It is believed that the reason is that since the dispersibility of particles with a small particle size is low, they tend to aggregate when the content increases. In Example 7, in which the residual alkali amount is increased by making the stretching temperature lower than that of Example 8, the dispersibility of the particles is good. However, as mentioned above, when the residual alkali amount is large, there is a concern that it may become a cause of poor appearance such as reduced adhesion and unevenness after a durability test. In addition, in order to ensure the dispersibility of the particles, the residual alkali amount needs to be maintained above the specified value, and the process window may become narrower.

[0213] For Examples 1 to 3 and Examples 10 to 12 using particles with an average particle size of 150 nm, and Examples 4 to 6 using particles with an average particle size of 110 nm, the particles had good dispersibility and blocking resistance. From these results, it can be seen that by using fine particles with a particle size greater than 100 nm, the blocking resistance can be improved even with a small amount of particles, and an easy-adhesion film with excellent dispersibility of particles in the easy-adhesion layer can be obtained even when the amount of residual alkali is small.

[0214] Description of Reference Numerals

[0215] 1 Easy-to-bond film

[0216] 11 Film substrate

[0217] 15 Easy bonding layer

[0218] 2 Transparent film

[0219] 5 polarizers

[0220] 6, 7 Adhesive layer

[0221] 100 polarizing plate

Claims

1. An easy-adhesive film comprising an easy-adhesive layer on the surface of a transparent film substrate, The easy-adhesion layer contains a binder resin and inorganic fine particles. The thickness of the easy-adhesion layer is 120 to 260 nm. The average primary particle size of the inorganic fine particles is 0.3 to 0.9 times the thickness of the easy-adhesion layer. The easy-adhesion layer has an alkali component content of 25 to 200 ppm having a boiling point of 150° C. or less.

2. The easy-adhesion film according to claim 1, wherein The average primary particle size of the inorganic fine particles is greater than 100 nm and less than 200 nm.

3. The easy-adhesion film according to claim 1 or 2, wherein The content of the inorganic fine particles in the easy-adhesion layer is 3 to 50% by weight.

4. The easy-adhesion film according to claim 1 or 2, wherein The transparent film substrate is an acrylic film.

5. The easy-adhesion film according to claim 1 or 2, wherein The binder resin of the easy-adhesion layer is a urethane resin.

6. The easy-adhesion film according to claim 1 or 2, wherein At the interface between the transparent film substrate and the easy-adhesion layer, there is a region where the inorganic fine particles are buried in the transparent film substrate.

7. A method for producing an easily adhesive film, the method for producing the easily adhesive film according to any one of claims 1 to 6, wherein: The surface of the transparent film substrate is coated with an easy-adhesion composition containing a binder resin or a precursor thereof, inorganic fine particles, an alkali component and a solvent. The easy-adhesion composition is heated at a temperature higher than the glass transition temperature of the transparent film substrate by 10° C. or more to volatilize the solvent and the alkali component.

8. The method for producing an easily adhesive film according to claim 7, wherein: The easy-adhesion composition contains, as the base component, one or more selected from the group consisting of amines and ammonia.

9. The method for producing an easily adhesive film according to claim 8, wherein: The easy-adhesion composition contains an amine having a boiling point of 150° C. or less as the base component.

10. The method for producing an easily adhesive film according to any one of claims 7 to 9, wherein The alkaline component has a function of promoting dispersion of the inorganic fine particles.

11. The method for producing an easily adhesive film according to any one of claims 7 to 9, wherein: The easy-adhesion composition contains a polyurethane precursor as a precursor of the binder resin and contains a tertiary amine as the base component.

12. The method for producing an easily adhesive film according to any one of claims 7 to 9, wherein: The transparent film substrate coated with the easy-adhesive composition is stretched in at least one direction while heating the easy-adhesive composition at a temperature 10° C. or higher than the glass transition temperature of the transparent film substrate.

13. A polarizing plate comprising: A polyvinyl alcohol-based polarizer having a first main surface and a second main surface; and a transparent film attached to the first main surface of the polarizer via an adhesive layer, The transparent film is the easy-adhesion film according to any one of claims 1 to 6. 14 . An image display device comprising an image display unit and the polarizing plate according to claim 13 .