A preparation method and application of nano-thin film composite film based on molybdenum disulfide oil phase doping
By doping molybdenum disulfide nanosheets on the nanofiltration membrane to form modified membrane materials, the problem of mutual constraints on the permeability and retention of traditional nanofiltration membranes is solved, efficient desalination of bitter and salty water is achieved, and water resources are significantly improved Utilization and stability of membrane material.
Patent Information
- Application Number
- CN202111403223.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-24
AI Technical Summary
Traditional nanofiltration membranes have problems of mutual constraints on permeability and retention during the desalination of bitter and salty water, resulting in low operating efficiency and increased energy consumption, making it difficult to effectively solve the problem of shortage of freshwater resources.
Using the nano-thin film composite membrane preparation method based on molybdenum disulfide oil phase doping, molybdenum disulfide nanosheets are doped onto the polyethersulfone ultrafiltration membrane through interfacial polymerization to form a modified membrane material to improve the permeability of the membrane and Interceptibility.
Under extremely low molybdenum disulfide usage, the flux and retention rate of the nanofiltration membrane are significantly improved, including the removal rates of chloride ions, sulfate, nitrate, sodium ions and magnesium ions, reducing preparation cost and energy consumption. More efficient desalination of bitter and salty water is achieved.
Smart Images

Figure CN114210215B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of membrane material preparation, and in particular relates to a preparation method and application of a nano-thin film composite membrane based on molybdenum disulfide oil phase doping. Background Art
[0002] In recent years, with the rapid development of industry and agriculture and the acceleration of urbanization, people have higher requirements for water quality and quantity. The shortage of freshwater resources and drinking water safety have become one of the obstacles to the sustainable development of society and economy in some regions. Brackish water accounts for 1% of the total water on the earth. On the premise of ensuring ecological and economic feasibility, realizing its resource utilization through desalination of brackish water is an effective way to cope with the shortage of freshwater resources and improve the safety of water for life and production.
[0003] Nanofiltration membrane separation water purification technology has low operating costs, is environmentally friendly, has strong stability and excellent treatment effects, and is widely used in the field of brackish water desalination. However, traditional thin film composite nanofiltration membranes (TFC) are affected by the "trade-off" effect, where interception and permeability restrict each other and are difficult to break through; and during long-term operation, the decrease in permeability and the increase in operating energy consumption caused by concentration polarization also restrict the promotion and application of nanofiltration membrane technology. Summary of the invention
[0004] The present invention provides a preparation method and application of a nano-thin film composite membrane based on molybdenum disulfide oil phase doping in order to solve the technical problem of mutual restriction between permeability and interception of existing nanofiltration membranes.
[0005] The preparation method of a nano-thin film composite film based on molybdenum disulfide oil phase doping of the present invention is carried out according to the following steps:
[0006] Step 1: Soak the polyethersulfone ultrafiltration membrane in an isopropanol solution, take it out after soaking, wash it with deionized water, and then soak it in deionized water at 4°C overnight;
[0007] Step 2: Prepare a piperazine aqueous solution at room temperature;
[0008] Step 3: preparing a n-hexane solution of trimesoyl chloride at room temperature, and then ultrasonically dispersing the molybdenum disulfide nanosheet powder in the n-hexane solution of trimesoyl chloride to obtain a molybdenum disulfide nanosheet-doped oil phase solution;
[0009] Step 4: fix the polyethersulfone ultrafiltration membrane treated in step 1 on an interfacial polymerization reactor, add the piperazine aqueous solution of step 2, pour off the excess piperazine aqueous solution after the piperazine aqueous solution is fully in contact with the polyethersulfone ultrafiltration membrane, and then place it at room temperature until the membrane surface is dry, and then add the molybdenum disulfide nanosheet doped oil phase solution of step 3, pour off the excess molybdenum disulfide nanosheet doped oil phase solution after the molybdenum disulfide nanosheet doped oil phase solution is fully in contact with the membrane, and obtain a modified membrane material;
[0010] Step 5, placing the modified membrane material obtained in step 4 in an oven for drying and solidification to obtain a nano-thin film composite membrane doped with molybdenum disulfide oil phase.
[0011] It is further defined that in step 1, the polyethersulfone ultrafiltration membrane is immersed in an isopropanol solution for 8 to 12 minutes.
[0012] It is further defined that the volume fraction of the isopropanol solution in step 1 is 20% to 30%.
[0013] It is further defined that the method for preparing the piperazine aqueous phase solution in step 2 is as follows: dissolving piperazine in deionized water at room temperature, and then adjusting the pH of the solution to 11.0 to obtain the piperazine aqueous phase solution.
[0014] It is further defined that the mass ratio of piperazine to deionized water is 1:(80-120).
[0015] Further defined, the method for preparing the n-hexane solution of trimesoyl chloride in step 3 is as follows: dissolving trimesoyl chloride in n-hexane at room temperature to obtain a n-hexane oil solution of trimesoyl chloride.
[0016] It is further defined that the ratio of the mass of trimesoyl chloride to the volume of n-hexane is 0.1 g: (80-120) mL.
[0017] It is further defined that the ratio of the mass of the molybdenum disulfide nanosheet powder to the volume of the trimesoyl chloride n-hexane oil solution in step 3 is (0.2-1.0) mg:100 mL.
[0018] Further defined, the amount of piperazine aqueous solution used in step 4 is (0.45-0.65) mL / cm 2 .
[0019] It is further defined that the contact time between the piperazine aqueous solution and the polyethersulfone ultrafiltration membrane in step 4 is 1.5 min to 2.5 min.
[0020] It is further defined that in step 4, after the excess piperazine aqueous solution is poured off, the mixture is left to stand at room temperature for 10 to 20 minutes.
[0021] It is further defined that the amount of the molybdenum disulfide nanosheet-doped oil phase solution in step 4 is (0.45-0.65) mL / cm 2 .
[0022] It is further defined that in step 4, the contact time between the molybdenum disulfide nanosheet-doped oil phase solution and the polyethersulfone ultrafiltration membrane is 25s to 35s.
[0023] It is further defined that the interfacial polymerization reactor in step 4 is an organic glass interfacial polymerization reactor.
[0024] It is further defined that the drying and curing temperature in step 5 is 50-70° C. and the time is 5 min to 7 min.
[0025] The nano-thin film composite membrane based on molybdenum disulfide oil phase doping of the present invention is applied to the field of brackish water desalination.
[0026] Compared with the prior art, the present invention has the following significant effects:
[0027] The present invention provides a method for modifying the polyamide layer of a nanocomposite membrane. By doping molybdenum disulfide nanosheets in the oil phase, a polyamide nanofiltration membrane doped with two-dimensional nanomaterials is constructed on the basis of an ultrafiltration membrane by interfacial polymerization. Under the conditions of extremely low loading and stable retention, the nanofiltration membrane flux is greatly improved. The specific advantages are as follows
[0028] 1) The present invention is based on the principle of conventional interfacial polymerization reaction, with simple experimental equipment, mild reaction conditions, controllable reaction process, and a good basis for promotion and application;
[0029] 2) The present invention uses organic phase doping to take advantage of the good dispersibility of molybdenum disulfide in the organic phase and the good volatility of n-hexane, thereby reducing the process of preparing the molybdenum disulfide dispersion during the membrane preparation process, reducing the consumption of reagents, shortening the drying time, and having a more "low-carbon" experimental process;
[0030] 3) The present invention creatively distributes molybdenum disulfide nanosheets directly on the membrane surface through organic phase doping, so that it protects the polyamide active layer with separation ability, achieves an increase in cross-linking degree, and improves the stability of the membrane material; at the same time, it gives full play to the advantages of its two-dimensional material, such as high hydrophilicity and electronegativity;
[0031] 4) The present invention breaks through the influence of the "trade-off" effect of traditional nanofiltration membranes, and with the help of extremely low molybdenum disulfide doping at the milligram level, simultaneously improves the permeability, divalent salt retention, and monovalent salt retention of the nanofiltration membrane;
[0032] 5) The prepared membrane material is used in actual brackish water desalination application experiments, with chloride ion removal rates of 29.53%, sulfate ion removal rates of 98.0%, nitrate ion removal rates of 96.10%, sodium ion removal rates of 92.96%, and magnesium ion removal rates of 98.53%, which are greatly improved compared with traditional nanofiltration membranes. In addition, the amount of molybdenum disulfide used is extremely low, and the cost is controllable, showing good application prospects in the field of brackish water desalination. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1a is a scanning electron microscope photo of the thin film composite membrane TFC of comparative example 1, Figure 1 f is an atomic force microscope photograph of the thin film composite membrane TFC of Comparative Example 1;
[0034] Figure 1 b is a scanning electron microscope photo of the thin film nanocomposite membrane TFN-O-0.0002 of Example 1, Figure 1 g is an atomic force microscope photograph of the thin film nanocomposite film TFN-O-0.0002 of Example 1;
[0035] Figure 1 c is a scanning electron microscope photo of the thin film nanocomposite membrane TFN-O-0.0006 of Example 2, Figure 1 h is an atomic force microscope photograph of the thin film nanocomposite film TFN-O-0.0006 of Example 2;
[0036] Figure 1 d is a scanning electron microscope photograph of the thin film nanocomposite membrane TFN-O-0.0008 of Example 3; Figure 1 i is an atomic force microscope photograph of the thin film nanocomposite film TFN-O-0.0008 of Example 3;
[0037] Figure 1 e is a scanning electron microscope photograph of the thin film nanocomposite membrane TFN-O-0.001 of Example 4, Figure 1 j is an atomic force microscope photograph of the thin film nanocomposite film TFN-O-0.001 of Example 4;
[0038] Figure 2 A bar graph comparing the water contact angles of the nanocomposite films of Examples 1-4 and the composite films of Comparative Examples 1-2;
[0039] Figure 3 a is the O1s spectrum of the TFC composite membrane of Comparative Example 1;
[0040] Figure 3 b is the O1s spectrum of the nanocomposite film TFN-O-0.001 of Example 4;
[0041] Figure 4 It is a line graph of the interception rate of PEG by the composite membrane of Comparative Example 1-2 and the nanocomposite membrane of Example 1-4;
[0042] Figure 5 The pure water flux bar graph of the composite membrane of Comparative Example 1-2 and the nanocomposite membrane of Example 1-4;
[0043] Figure 6 It is a bar graph of the rejection rate of the composite membrane of Comparative Example 1-2 and the nano-composite membrane of Example 1-4 for sodium sulfate;
[0044] Figure 7 It is a bar graph of the sodium chloride rejection rate of the composite membrane of Comparative Example 1-2 and the nano-composite membrane of Examples 1-4. DETAILED DESCRIPTION
[0045] Embodiment 1: The preparation method of a nano-thin film composite film based on molybdenum disulfide oil phase doping of this embodiment is carried out according to the following steps:
[0046] Step 1: Place a polyethersulfone ultrafiltration membrane (membrane area 45.34 cm 2 / diameter 76mm) was placed in a 25vol% isopropanol solution and soaked for 10min, taken out after soaking, washed with deionized water and then soaked in deionized water at 4°C for 24h;
[0047] Step 2: dissolving 4 g of piperazine in 400 mL of deionized water at room temperature, and then adjusting the pH of the solution to 11.0 with a NaOH solution to obtain a piperazine aqueous solution;
[0048] Step 3: dissolving 0.1 g of trimesoyl chloride in 100 mL of n-hexane at room temperature to obtain a trimesoyl chloride n-hexane oil solution, and then ultrasonically dispersing 0.0002 g of molybdenum disulfide nanosheet powder in 100 mL of trimesoyl chloride n-hexane solution to obtain a molybdenum disulfide nanosheet-doped oil phase solution;
[0049] Step 4: fix the polyethersulfone ultrafiltration membrane treated in step 1 on an interfacial polymerization reactor, add 25 mL of the piperazine aqueous solution of step 2, pour off the excess piperazine aqueous solution after the piperazine aqueous solution is in contact with the polyethersulfone ultrafiltration membrane for 2 minutes, and then place it at room temperature for 15 minutes until the membrane surface is dry, and then add 25 mL of the molybdenum disulfide nanosheet-doped oil phase solution of step 3, pour off the excess molybdenum disulfide nanosheet-doped oil phase solution after the molybdenum disulfide nanosheet-doped oil phase solution is in contact with the membrane for 30 seconds, to obtain a modified membrane material;
[0050] Step 5, placing the modified membrane material obtained in step 4 in an oven at 60° C. for drying and curing for 6 minutes to obtain a nano-thin film composite membrane doped with molybdenum disulfide oil phase (denoted as TFN-O-0.0002).
[0051] Example 2: The difference between this example and Example 1 is that the amount of molybdenum disulfide nanosheet powder used in step 3 is 0.0006 g, and the resulting composite film is recorded as TFN-O-0.0006. Other steps and parameters are the same as those in Example 1.
[0052] Example 3: The difference between this example and Example 1 is that the amount of molybdenum disulfide nanosheet powder used in step 3 is 0.0008 g, and the resulting composite film is recorded as TFN-O-0.0008. Other steps and parameters are the same as those in Example 1.
[0053] Example 4: The difference between this example and Example 1 is that the amount of molybdenum disulfide nanosheet powder used in step 3 is 0.001 g, and the resulting composite film is denoted as TFN-O-0.001. Other steps and parameters are the same as those in Example 1.
[0054] Comparative Example 1 (TFC composite membrane): The difference between this example and Example 1 is that no molybdenum disulfide nanosheet powder is added in step 3. Other steps and parameters are the same as those in Example 1.
[0055] Comparative Example 2 (TFN-W-0.0025): The difference between this example and Example 1 is that:
[0056] Step 2: using deionized water to prepare a 0.0025% molybdenum disulfide nanosheet dispersion by ultrasonic dispersion, then dissolving 1 g of piperazine in 100 mL of the 0.0025% molybdenum disulfide nanosheet dispersion at room temperature, and adjusting the pH of the solution to 11.0 with a NaOH solution to obtain a molybdenum disulfide nanosheet-doped aqueous solution;
[0057] Step 3: No molybdenum disulfide nanosheet powder is added. Other steps and parameters are the same as those in Example 1.
[0058] Detection test
[0059] Experiment 1: The water contact angles of the nanocomposite membranes of Examples 1-4 and the TFC composite membrane of Comparative Example 1 were tested, and the results were as follows: Figure 2 The water contact angle comparison bar graph of the nanocomposite membranes of Examples 1-4 and the TFC composite membrane of Comparative Example 1 is shown. Figure 2 It can be seen that the water contact angle of the control TFC nanofiltration membrane without molybdenum disulfide is 38.3°, and the water contact angle of the TFN-W-0.0025 composite membrane doped with molybdenum disulfide in the water phase in comparative example 2 is 35.9°. The water contact angles of the nanofiltration membranes TFN-O-0.0002, TFN-O-0.0006, TFN-O-0.0008, and TFN-O-0.001 doped with molybdenum disulfide are 37.5°, 35.7°, 34.6°, and 32.6°, respectively. Compared with the control membrane, the water contact angle of the TFN nanofiltration membrane prepared by oil phase doping with molybdenum disulfide decreases with the increase of doping amount, and the hydrophilicity is improved.
[0060] Experiment 2: X-ray photoelectron spectroscopy was used to further analyze Example 4 and Comparative Example 1, and the O1s spectra of Example 4 (TFN-O-0.001) and Comparative Example 1 (TFC) were obtained. Figure 3It can be seen that since the oil phase doped with molybdenum disulfide nanosheets promotes the further formation of amide, the content of OC=O generated by hydrolysis of unreacted acyl chloride groups in the TFN membrane doped with molybdenum disulfide nanosheets in the oil phase is reduced compared with the TFC membrane in the comparative example.
[0061] Experiment 3: The retention rate of PEG (200 mg / L) of the nanocomposite membranes of Examples 1-4 and Comparative Examples 1-2 was tested, and the following results were obtained: Figure 4 The interception rate of the composite membrane of Comparative Example 1-2 and the nanocomposite membrane of Example 1-4 for PEG (200 mg / L) is shown in the line graph. Figure 4 It can be seen that the control TFC nanofiltration membrane without molybdenum disulfide doped in comparative example 1 has a molecular weight cutoff of 756Da and an average pore size of 0.67nm, the TFN-W-0.0025 composite membrane doped with molybdenum disulfide in the aqueous phase in comparative example 2 has a molecular weight cutoff of 633Da and an average pore size of 0.61nm, and the nanofiltration membrane TFN-O-0.001 doped with molybdenum disulfide has a molecular weight cutoff of 517Da and an average pore size of 0.54nm. For TFN nanofiltration membranes with different doping amounts, the molecular weight cutoff gradually decreases with the increase of the doping amount.
[0062] Experiment 4: The pure water flux of the nanocomposite membranes of Examples 1-4 and the composite membranes of Comparative Examples 1-2 was tested, and the results were as follows: Figure 5 The pure water flux bar graph of the composite membrane of Comparative Example 1-2 and the nanocomposite membrane of Example 1-4 is shown in FIG. Figure 5 It can be seen that the pure water flux of the control TFC nanofiltration membrane without molybdenum disulfide doping is 8.07LMH / bar, the pure water flux of the nanofiltration membrane TFN-W-0.0025 doped with molybdenum disulfide in the water phase is 8.96LMH / bar, and the pure water flux of the nanofiltration membranes TFN-O-0.0002, TFN-O-0.0006, TFN-O-0.0008, and TFN-O-0.001 doped with molybdenum disulfide are 8.57LMH / bar, 9.09LMH / bar, 9.27LMH / bar, and 10.45LMH / bar, respectively. With the increase of the molybdenum disulfide doping amount, the water flux of the constructed TFN nanofiltration membrane gradually increases. When the oil phase doping reaches 0.001wt%, the water flux of the nanofiltration membrane increases by 30%, which is significantly better than the water-doped composite membrane with the same doping amount.
[0063] Experiment 5: The retention rates of sodium sulfate (2 g / L) and sodium chloride (2 g / L) of the nanocomposite membranes of Examples 1-4 and the composite membranes of Comparative Examples 1-2 were tested, and the following results were obtained: Figure 6 The interception rate of the composite membrane of Comparative Example 1-2 and the nanocomposite membrane of Example 1-4 for sodium sulfate (2 g / L) is shown in the bar graph and Figure 7The bar graphs of the rejection rates of the composite membranes of Comparative Examples 1-2 and the nanocomposite membranes of Examples 1-4 for sodium chloride (2 g / L) are compared;
[0064] from Figure 6 It can be seen that the rejection rate of the control TFC nanofiltration membrane of comparative example 1 without molybdenum disulfide for sodium sulfate is 97.08%, the rejection rate of the TFN-W-0.0025 composite membrane doped with molybdenum disulfide in the water phase of comparative example 2 for sodium sulfate is 98.06%, and the rejection rates of the nanofiltration membranes TFN-O-0.0002, TFN-O-0.0006, TFN-O-0.0008, and TFN-O-0.001 doped with molybdenum disulfide for sodium sulfate are 97.56%, 97.65%, 96.94%, and 98.25%, respectively. Molybdenum disulfide doped in the oil phase maintains the high rejection rate of the nanofiltration membrane for divalent salts while improving the permeability of the nanofiltration membrane.
[0065] from Figure 7 It can be seen that the sodium chloride rejection rate of the control TFC nanofiltration membrane of comparative example 1 without molybdenum disulfide is 18.33%, the sodium chloride rejection rate of the TFN-W-0.0025 composite membrane doped with molybdenum disulfide in the water phase of comparative example 2 is 21.46%, and the sodium chloride rejection rates of the nanofiltration membranes doped with molybdenum disulfide TFN-O-0.0002, TFN-O-0.0006, TFN-O-0.0008, and TFN-O-0.001 are 21.67%, 24.17%, 26.25%, and 30.56%, respectively. Molybdenum disulfide doped in the oil phase has greatly improved the rejection capacity of the nanofiltration membrane for conventional monovalent salts. As the doping amount of molybdenum disulfide increases, the monovalent salt rejection capacity of the constructed TFN nanofiltration membrane is gradually improved. When the doping reaches 0.001wt%, the monovalent salt rejection capacity of the TFN nanofiltration membrane is increased by 40%.
Claims
1. A method for preparing a nano-thin film composite film based on molybdenum disulfide oil phase doping, characterized in that: The preparation method is carried out according to the following steps: Step 1: Soak the polyethersulfone ultrafiltration membrane in a 20% to 30% by volume isopropanol solution for 8 to 12 minutes, take it out after soaking, wash it with deionized water, and then soak it in deionized water at 4°C overnight; Step 2: dissolving piperazine in deionized water at room temperature, and then adjusting the pH of the solution to 11.0 to obtain a piperazine aqueous phase solution; the mass ratio of piperazine to deionized water is 1:(80-120); Step 3: dissolving trimesoyl chloride in n-hexane at room temperature to obtain a trimesoyl chloride n-hexane oil solution, and then ultrasonically dispersing molybdenum disulfide nanosheet powder in the trimesoyl chloride n-hexane solution to obtain a molybdenum disulfide nanosheet-doped oil phase solution; the ratio of the mass of trimesoyl chloride to the volume of n-hexane is 0.1 g: (80-120) mL, and the ratio of the mass of the molybdenum disulfide nanosheet powder to the volume of the trimesoyl chloride n-hexane oil solution is (0.2-1.0) mg: 100 mL; Step 4: fix the polyethersulfone ultrafiltration membrane treated in step 1 on an interfacial polymerization reactor, add the piperazine aqueous solution of step 2, pour off the excess piperazine aqueous solution after the piperazine aqueous solution is fully in contact with the polyethersulfone ultrafiltration membrane, and then place it at room temperature until the membrane surface is dry, and then add the molybdenum disulfide nanosheet doped oil phase solution of step 3, pour off the excess molybdenum disulfide nanosheet doped oil phase solution after the molybdenum disulfide nanosheet doped oil phase solution is fully in contact with the membrane, and obtain a modified membrane material; The amount of piperazine aqueous solution used is (0.45~0.65)mL / cm 2 The contact time between the piperazine aqueous solution and the polyethersulfone ultrafiltration membrane is 1.5 min to 2.5 min. After the excess piperazine aqueous solution is poured off, the solution is placed at room temperature for 10 min to 20 min. The amount of the MoS2 nanosheet-doped oil phase solution is (0.45 to 0.65) mL / cm 2 , the contact time between the MoS2 nanosheet-doped oil phase solution and the polyethersulfone ultrafiltration membrane is 25s to 35s; Step 5, placing the modified membrane material obtained in step 4 in an oven for drying and solidification to obtain a nano-thin film composite membrane doped with molybdenum disulfide oil phase.
2. The method for preparing a nano-thin film composite film based on molybdenum disulfide oil phase doping according to claim 1, characterized in that: The interfacial polymerization reactor in step 4 is an organic glass interfacial polymerization reactor.
3. The method for preparing a nano-thin film composite film based on molybdenum disulfide oil phase doping according to claim 1, characterized in that: The drying and curing temperature in step 5 is 50-70° C. and the time is 5-7 minutes.
4. The use of a nano-thin film composite membrane based on molybdenum disulfide oil phase doping obtained by the preparation method according to any one of claims 1 to 3, characterized in that: The nano-thin film composite membrane based on molybdenum disulfide oil phase doping is applied in the field of brackish water desalination.