A flame retardant polypropylene material and its preparation method and application

By adding ultraviolet absorbers, light stabilizers and metal oxides of specific particle sizes to polypropylene materials, the problems of decreased flame retardancy and yellowing after photoaging are solved, achieving excellent light aging resistance and flame retardant performance.

CN114213749BActive Publication Date: 2024-11-26KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111398296.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-11-26
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing polypropylene materials exhibit decreased flame retardancy and severe yellowing after photoaging, and traditional additives cannot effectively improve their resistance to photoaging.

Method used

The material uses a combination of ultraviolet absorbers, light stabilizers, and metal oxides with specific particle sizes as photoaging resistant components. Through the synergistic effect of these three components, the material's photoaging resistance is improved, and by optimizing the ratio and component selection, the material is guaranteed not to discolor.

Benefits of technology

It achieves a color difference of less than 4 after light aging test of polypropylene material, maintains good flame retardant properties, and is suitable for parts with strict requirements for flame retardancy and light resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003369098920000051
    Figure BDA0003369098920000051
  • Figure BDA0003369098920000061
    Figure BDA0003369098920000061
  • Figure BDA0003369098920000062
    Figure BDA0003369098920000062
Patent Text Reader

Abstract

The present invention discloses a flame-retardant polypropylene material and a preparation method and application thereof, belonging to the field of plastic materials. The flame-retardant polypropylene material of the present invention uses a combination of ultraviolet absorber, light stabilizer and metal oxide as light-resistant aging components, and the light-resistant aging ability of the material is improved through the synergistic effect of the three; at the same time, under the preferred formula, the flame-retardant polypropylene material has good flame-retardant properties and can be effectively and practically applied to the preparation of various flame-retardant parts with strict requirements on flame retardancy and light resistance. The present invention also discloses a preparation method and application of the flame-retardant polypropylene material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plastic materials, and in particular to a flame retardant polypropylene material and a preparation method thereof. Background Art

[0002] As one of the five general-purpose plastics, polypropylene (PP) has the advantages of being non-toxic, odorless, light, easy to process, good electrical insulation, and resistant to chemical solvents. It is widely used in the fields of automobiles, household appliances, packaging materials, wires and cables, etc. As the application areas and demand for PP increase, higher requirements are placed on the performance of PP. For example, most PP materials today are required to have flame retardant properties, so it is generally necessary to add flame retardant components to polypropylene materials.

[0003] Brominated flame retardants are effective flame retardant additives for PP, but they are prone to generate a large number of bromine free radicals after exposure to light. These free radicals react with unstable tertiary hydrogen in PP to generate a large number of alkyl free radicals, which ultimately lead to accelerated aging of PP in a xenon lamp aging box during aging tests, and reduced flame retardant properties of the material after xenon lamp aging. On the other hand, most of the light stabilizers and ultraviolet absorbers added to existing PP products cannot fully exert their effects and cannot cope with large-scale rapid light aging of PP products. After aging, the yellowing of PP materials is very obvious, and their practicality is significantly reduced. Summary of the invention

[0004] Based on the defects of the prior art, the purpose of the present invention is to provide a flame retardant polypropylene material, which has better light aging resistance and good flame retardant performance than traditional bromide-based flame retardant polypropylene materials.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A flame retardant polypropylene material comprises the following components in parts by weight:

[0007] 45-55 parts of polypropylene resin, 12-25 parts of talc, 18-25 parts of brominated flame retardant, 6-9 parts of antimony trioxide and 0.6-4 parts of light aging agent; the light aging agent includes ultraviolet absorber, light stabilizer and metal oxide; the metal oxide is at least one of ZnO, TiO2, Al2O3, MgO, and has an average particle size of 10-60nm.

[0008] Although certain functional components such as ultraviolet absorbers or antioxidants are added to the components of traditional flame-retardant polypropylene materials to improve the light aging resistance of the product, the improvement effect is limited and the product application range is narrow; the flame-retardant polypropylene material of the present invention uses ultraviolet absorbers, light stabilizers and metal oxides as light aging resistance components. Through the synergistic effect of the three, the light aging resistance of the material is improved, and the flame retardant performance is good.

[0009] In addition, the inventor of the present application has also studied the type and particle size of metal oxides: the addition of metal oxides as light aging resistant components in traditional flame retardant polypropylene materials is because metal oxides can adjust the pH value of the entire material and neutralize the peroxy radicals generated by bromine flame retardants. However, the inventors found that such light aging resistant effect is not ideal, and its effect has a saturation value, and once the saturation value is reached, the metal oxide fails and the process of the maximum color difference of the product is accelerated; in addition, although the introduction of some metal oxides can improve the light aging resistant effect of the material, it has a certain bright color system, which has a great influence on the color of the material and cannot improve the use value. The flame retardant polypropylene material of the present invention is white or grayish white without adding color powder. If the color system is deepened, the degree of discoloration after light aging will be deepened. Only by selecting nano-scale metal oxide particles of specific types, specific sizes and specific colors to match with ultraviolet absorbers and light stabilizers, metal oxides can effectively shield, absorb and refract external light sources, and inhibit the generation of bromine radicals by bromine flame retardants from the source by physical means, can a long-term light aging resistant effect be achieved without affecting the color system of the material itself.

[0010] Preferably, the weight portion of the light aging resistance agent is 1 to 2 parts;

[0011] The more the content of the light aging agent, the better. When the content reaches a certain level, the light aging resistance of the flame retardant polypropylene material is not significantly improved, and the production cost becomes high, which is not conducive to large-scale production.

[0012] Preferably, the mass ratio of the ultraviolet absorber, the light stabilizer and the metal oxide is ultraviolet absorber:light stabilizer:metal oxide=(1-3):(1-3):(8-12).

[0013] The ratio of the three also has a certain impact on the performance of the product. If the metal oxide content is too much (too little UV absorber or light stabilizer), it will not be able to effectively reduce the concentration of bromine free radicals and peroxyl free radicals already contained in the product. If there are too many UV absorbers or light stabilizers, it will not be able to effectively shield the influence of external light sources on brominated flame retardants. Both situations will lead to a reduction in the product's light aging resistance.

[0014] Under the preferred addition amount and ratio, the ultraviolet absorber, light stabilizer and metal oxide can fully work synergistically, and the maximum color difference of the obtained product in the xenon lamp aging test is lower.

[0015] Preferably, the talc D 90 8~13μm, D 50 3~6μm.

[0016] The talc powder with the particle size described above has better dispersibility during the processing of the flame-retardant polypropylene material and is not likely to generate a large shear force to damage the ultraviolet absorber, the light stabilizer and the metal oxide.

[0017] Preferably, the polypropylene resin is at least one of homopolypropylene and copolymer polypropylene.

[0018] Preferably, the brominated flame retardant is at least one of decabromodiphenylethane, brominated epoxy, brominated triazine, tetrabromobisphenol A, and ethylenebis(tetrabromophthalamide).

[0019] Preferably, the ultraviolet absorber is at least one of a benzotriazole ultraviolet absorber and a benzophenone ultraviolet absorber; and the light stabilizer is a hindered amine N-OR type light stabilizer.

[0020] Preferably, the flame retardant polypropylene material also includes 0 to 0.5 parts of a mixture of an antioxidant and a lubricant.

[0021] More preferably, the antioxidant is at least one of a phenolic antioxidant and a phosphite antioxidant; and the lubricant is at least one of zinc stearate, magnesium stearate, calcium stearate and barium stearate.

[0022] Another object of the present invention is to provide a method for preparing the flame retardant polypropylene material, comprising the following steps:

[0023] After the components are uniformly mixed according to a certain proportion, they are placed in a twin-screw extruder for melt mixing and extrusion granulation in sequence to obtain the flame-retardant polypropylene material.

[0024] The preparation method of the flame-retardant polypropylene material of the present invention has simple operation steps and can realize industrial large-scale production.

[0025] Preferably, the screw length-to-diameter ratio of the twin-screw extruder is 40-48:1, the barrel temperature is 180-200° C., and the screw speed is 200-550 r / min.

[0026] Another object of the present invention is to use the flame-retardant polypropylene material in preparing flame-retardant parts for automobiles or household appliances.

[0027] The beneficial effect of the present invention is that the present invention provides a flame-retardant polypropylene material, which uses a combination of ultraviolet absorber, light stabilizer and metal oxide as light-resistant aging components, and improves the light-resistant aging ability of the material through the synergistic effect of the three; at the same time, under the preferred ratio of the formula, the flame-retardant polypropylene material has good flame-retardant properties and can be effectively and practically applied to the preparation of various flame-retardant parts with strict requirements on flame retardancy and light resistance. The present invention also provides a preparation method and application of the flame-retardant polypropylene material. DETAILED DESCRIPTION

[0028] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments designed by the present invention and comparative examples are all commonly used ordinary reagents and instruments unless otherwise specified.

[0029] Examples 1 to 13

[0030] The flame retardant polypropylene material of the present invention and the method for preparing the product comprise the following steps:

[0031] After premixing the raw materials in a high-speed mixer in proportion, the raw materials are placed in a twin-screw extruder for melt mixing and extrusion granulation in sequence to obtain the flame-retardant polypropylene material; the twin-screw extruder has a screw length-to-diameter ratio of 45:1, a barrel temperature of 180-200°C, and a screw speed of 400r / min.

[0032] The raw materials used in each example are as follows, and the proportions of the raw materials are shown in Table 1.

[0033] Polypropylene resin 1: copolymer polypropylene EP300M, produced by CNOOC Shell Petrochemical Co., Ltd.;

[0034] Polypropylene resin 2: homopolymer polypropylene HP 500N, produced by CNOOC Shell Petrochemical Co., Ltd.;

[0035] Talc 1: Commercially available talc, the talc D 90 8~10μm, D 50 3~4μm;

[0036] Talc 2: Commercially available talc, the talc has a 90 20~25μm, D 50 10~11μm;

[0037] Brominated flame retardant 1: decabromodiphenylethane, SAYTEX 4010, produced by Albemarle Corporation, USA;

[0038] Brominated flame retardant 2: Bromotriazine, FR245, Dead Sea, Israel;

[0039] Metal oxide 1: ZnO, average particle size 30 nm, commercially available;

[0040] Metal oxide 2: TiO2, average particle size 25 nm, commercially available;

[0041] UV absorber 1: benzotriazole UV absorber UV-P (2-(2'-hydroxy-5'-methylphenyl)benzotriazole), produced by Qitai (Shanghai) Chemical Technology Co., Ltd.;

[0042] UV absorber 2: Pentaerythritol tetraacrylate UV absorber UV-3030 (pentaerythritol tetra(2-cyano-3,3-diphenylacrylate)), produced by Xiangyang Jindacheng Fine Chemical Co., Ltd.;

[0043] Light stabilizer 1: hindered amine N-OR type N-OR116, produced by BASF;

[0044] Light stabilizer 2: hindered amine NH type NH UV-770, produced by Guangzhou Xinyouwei Chemical Co., Ltd.;

[0045] Antioxidant: Antioxidant 3114, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, commercially available;

[0046] Lubricant: Magnesium stearate, commercially available.

[0047] Comparative Examples 1 to 6

[0048] The difference between the products described in Comparative Examples 1 to 6 and the products described in Examples 1 to 13 is only that the formulation or ratio of the component raw materials is different. The ratio of the raw materials is shown in Table 2.

[0049] The raw materials used that are different from the raw materials of the embodiment are as follows:

[0050] Metal oxide 3: The metal oxide is Fe2O3, with an average particle size of 20 nm, commercially available;

[0051] Metal oxide 4: The metal oxide is TiO2, with an average particle size of 5 nm, commercially available;

[0052] Metal oxide 5: The metal oxide is ZnO, with an average particle size of 1000 nm, commercially available;

[0053] Except for the above specific instructions, the raw materials used in other embodiments and comparative examples are all the same commercially available products.

[0054] Table 1

[0055]

[0056]

[0057] Table 2

[0058]

[0059] In order to verify the performance of the products obtained in the examples of the present invention, the products of each example and comparative example were baked at 120° C. for 3 h, and then injection molded into standard color plates and 1.5 mm vertical combustion specimens (prepared by injection molding according to the requirements of the corresponding test method), and the color difference test before and after xenon lamp aging was performed, and then the samples after xenon lamp aging were subjected to a combustion test. The results are shown in Tables 3 and 4, respectively. The specific test method is as follows:

[0060] (1) Xenon lamp aging test: According to ISO 4892-2:2013 standard test method condition 1, the test duration is 1008 hours, and each example and comparative example product is injection molded into a standard color plate with a size of 83mm*54mm*2mm at 200°C, and the color difference change value ΔE of the product color plate before and after xenon lamp aging is measured by an X-Rite 7000A colorimeter; the smaller the maximum value of the color difference change value ΔE appearing during the test, the better the light aging effect of the product;

[0061] (2) Combustion performance test: vertical combustion performance test according to GB / T 2408-2008;

[0062] (3) Appearance color inspection: Use a commercially available standard whiteness calibration color card to test the sample's apparent color.

[0063] Table 3

[0064]

[0065] Table 4

[0066]

[0067] According to Table 3 and Table 4, it can be seen that the flame-retardant polypropylene materials obtained in the embodiments of the present invention have good light aging resistance, and the maximum color difference change value after the 1008h xenon lamp aging test is less than 4, and the combustion level above V-2 can still be maintained after the light aging test; when the number of light aging agents added in the product components is preferably 1 to 2 parts, the products of Example 1 and Example 3 obtained therefrom have better light aging resistance than Example 2 within the non-preferred range, and when the number of added parts reaches 2.1 parts as described in Example 4, the light aging resistance of the product is not improved to a high degree, and the preparation cost is significantly increased. Therefore, in general, the addition of the light aging agent to the product components is preferably 1 to 2 parts, and the light aging resistance of the product is not improved to a high degree, and the preparation cost is significantly increased. The cost performance is the highest when it is 1 to 2 parts; from the 1008h xenon lamp aging test results of the products of Examples 1, 5 to 8, it can be seen that the light aging resistance of the products is different due to the different ratios of the ultraviolet absorber, light stabilizer and metal oxide in the light aging agent. When the ratio of the three reaches (1 to 3): (1 to 3): (8 to 12), the performance of the products of Examples 1, 5 and 6 obtained is better than that of the products of Examples 7 and 8 within the non-preferred range; and according to the comparison of the light aging resistance of the product of Example 1 with that of Examples 11 to 13, it can be seen that the different types of ultraviolet absorbers and light stabilizers in the product components and the size of talcum powder will affect its final performance.

[0068] Compared with the products of the embodiments, the light aging resistance agents in the components of the products obtained in Comparative Examples 1 to 3 do not contain ultraviolet absorbers, light stabilizers or metal oxides, and the three cannot play a significant synergistic role, and the light aging resistance effect is not good; the metal oxide in Comparative Example 4 is Fe2O3, and its introduction makes the product pink, which not only greatly reduces its scope of use, but also weakens the light aging resistance of the product by the introduction of the color system, and the maximum color difference change value reaches 4.92; according to the comparison of the light aging resistance of the products of Comparative Examples 4 to 6 and Example 1, it can be seen that if the particle size of the metal oxide is not within the protection scope of the present invention, it cannot play a synergistic role with the ultraviolet absorber and the light stabilizer, and it is difficult to effectively shield, absorb, and refract external light sources, and inhibit the generation of bromine free radicals by brominated flame retardants from the source by physical means.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A flame retardant polypropylene material, characterized in that: The composition comprises the following components in parts by weight: 48-55 parts of polypropylene resin, 22-25 parts of talc, 22-25 parts of brominated flame retardant, 7-9 parts of antimony trioxide and 0.6-4 parts of light aging agent; the light aging agent comprises an ultraviolet absorber, a light stabilizer and a metal oxide; the mass ratio of the ultraviolet absorber, the light stabilizer and the metal oxide is ultraviolet absorber:light stabilizer:metal oxide=(1-3):(1-3):(8-12); the metal oxide is at least one of ZnO with an average particle size of 30nm and TiO2 with an average particle size of 25nm; the ultraviolet absorber is a benzotriazole ultraviolet absorber; the light stabilizer is a hindered amine N-OR type light stabilizer; the talc D 90 8~13μm, D 50 3~6μm.

2. The flame retardant polypropylene material according to claim 1, characterized in that: The weight proportion of the light aging resistance agent is 1 to 2 parts.

3. The flame retardant polypropylene material according to claim 1, characterized in that: The flame retardant polypropylene material also includes 0 to 0.5 parts of a mixture of an antioxidant and a lubricant.

4. The method for preparing the flame retardant polypropylene material according to any one of claims 1 to 3, characterized in that: The following steps are involved: After the components are uniformly mixed according to a certain proportion, they are placed in a twin-screw extruder for melt mixing and extrusion granulation in sequence to obtain the flame-retardant polypropylene material.

5. The method for preparing the flame retardant polypropylene material according to claim 4, characterized in that: The screw length-diameter ratio of the twin-screw extruder is 40-48:1, the barrel temperature is 180-200° C., and the screw speed is 200-550 r / min.

6. Use of the flame-retardant polypropylene material according to any one of claims 1 to 3 in the preparation of flame-retardant parts for automobiles or household appliances.