Sm-Fe-N system magnetic material and its manufacturing method

By adjusting the lattice volume and density of Sm-Fe-N magnetic materials, replacing Fe with Co and/or Ni, and optionally replacing Sm with La and/or Ce, the problem of decreased saturation magnetization of Sm-Fe-N magnetic materials in molded bodies was solved, and high-density and high-magnetic molded bodies were achieved.

CN114255948BActive Publication Date: 2024-11-05TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111111030.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-24
Filing Date
2021-09-23
Publication Date
2024-11-05
Estimated Expiration
2041-09-23

AI Technical Summary

Technical Problem

Sm-Fe-N magnetic materials contain nitrogen, making it impossible to process them at nitrogen removal temperatures during the manufacturing process. This makes it difficult to sinter them without the use of binders, resulting in a decrease in the saturation magnetization of the molded material.

Method used

By adjusting the lattice volume and density of the main phase within a specific range, replacing Fe with a small amount of Co and/or Ni, and optionally replacing Sm with La and/or Ce, Sm-Fe-N type magnetic materials with Th2Zn17 and Th2Ni17 type crystal structures are formed, avoiding the use of binders.

Benefits of technology

This improved the saturation magnetization of the main phase of the Sm-Fe-N magnetic material, thereby enhancing the density and magnetic properties of the molded body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114255948B_ABST
    Figure CN114255948B_ABST
Patent Text Reader

Abstract

The present invention relates to a Sm-Fe-N based magnetic material and a method for manufacturing the same. The magnetic material disclosed herein has a main phase having a predetermined crystal structure. The main phase has (Sm (1‑x‑y‑z) La x Ce y R 1 z )2(Fe (1‑p‑q‑s) Co p Ni q M s ) 17 N h (R 1 is a specified rare earth element etc., M is a specified element, and the composition is represented by 0≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10, 0≤s≤0.10 and 2.9≤h≤3.1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a Sm-Fe-N based magnetic material and a method for manufacturing the same. The present disclosure particularly relates to a material having Th2Zn 17 Type and Th2Ni 17 A Sm-Fe-N based magnetic material having a main phase of at least any one type of crystal structure and a method for producing the same. Background Art

[0002] As high-performance magnetic materials, Sm-Co and Nd-Fe-B magnetic materials have been put into practical use. In recent years, magnetic materials other than these have been studied. For example, magnetic materials with Th2Zn 17 Type and Th2Ni 17 A Sm-Fe-N based magnetic material having a main phase of at least any one type of crystal structure of the Sm-Fe-N based magnetic material (hereinafter sometimes referred to as “Sm-Fe-N based magnetic material”).

[0003] Sm-Fe-N magnetic materials have Th2Zn 17 Type and Th2Ni 17 The main phase is considered to be a crystal phase in which nitrogen is introduced into the Sm-Fe system in an intrusive manner.

[0004] Japanese Patent Publication No. 2017-117937 discloses a method for producing a Sm-Fe-N magnetic material, wherein an oxide containing Sm, Fe, La and W is reduced, and the reduced product is nitrided to obtain the Sm-Fe-N magnetic material. Summary of the invention

[0005] Compared with Sm-Co magnetic materials and Nd-Fe-B magnetic materials, Sm-Fe-N magnetic materials have very high coercive force. However, since Sm-Fe-N magnetic materials contain nitrogen (N), it is not possible to process intermediate products at a temperature at which nitrogen (N) is separated during their manufacture. In particular, when a molded body is obtained from a powdered Sm-Fe-N magnetic material (hereinafter sometimes referred to as "Sm-Fe-N magnetic material powder"), it is difficult to obtain the molded body without using a binder.

[0006] As a method for obtaining a molded body from powder, there is a sintering method. The sintering method is a method of heating the powder at a high temperature for a long time to calcine the powder. Even if the powder is heated to a high temperature, if the powder does not decompose, the powder can be calcined (sintered) even without using a binder. In this way, when the powder is calcined (sintered), since no binder is used, the density of the sintered body can be improved.

[0007] In the case of obtaining a molded body from magnetic material powder, if the magnetic material powder can be calcined (sintered) without using a binder, the density of the molded body (sintered body) is improved, and the saturation magnetization of the molded body can be improved. However, the Sm-Fe-N magnetic material contains nitrogen (N), so the powder of the Sm-Fe-N magnetic material cannot be heated to a temperature above the temperature at which nitrogen (N) is separated when obtaining the molded body. Therefore, in order to obtain a molded body of the Sm-Fe-N magnetic material powder, a resin binder or a low-melting-point metal or alloy binder is usually used. Therefore, the saturation magnetization of the molded body of the Sm-Fe-N magnetic material powder decreases according to the content of the binder.

[0008] When obtaining a molded body from Sm-Fe-N magnetic material powder, attempts have been made to reduce the content of the binder to improve the saturation magnetization of the molded body. Although some results have been achieved, this alone may not be sufficient. Based on this, the inventors have discovered the following problem: it is desirable to improve the saturation magnetization of the main phase itself that exhibits magnetism in the Sm-Fe-N magnetic material. It should be noted that in this specification, unless otherwise specified, "saturation magnetization" refers to the saturation magnetization at room temperature.

[0009] The present disclosure has been made to solve the above-mentioned problems. That is, an object of the present disclosure is to provide a Sm-Fe-N-based magnetic material having improved saturation magnetization of a main phase itself exhibiting magnetism compared with the conventional ones, and a method for producing the same.

[0010] The present inventors have conducted intensive research to achieve the above-mentioned object and have completed the Sm-Fe-N system magnetic material and the method for producing the same disclosed in the present invention. The Sm-Fe-N system magnetic material and the method for producing the same disclosed in the present invention include the following aspects.

[0011] <1> Sm-Fe-N magnetic material having Th2Zn 17 Type and Th2Ni 17 A Sm-Fe-N based magnetic material having a main phase of at least any one of the crystal structures of the type, wherein

[0012] The above main phase has a formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h Represents the composition, where

[0013] R 1is one or more rare earth elements other than Sm, La and Ce and Zr, M is one or more elements other than Fe, Co, Ni and rare earth elements and unavoidable impurity elements, and satisfies 0≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10, 0≤s≤0.10 and 2.9≤h≤3.1,

[0014] The lattice volume of the above main phase is 0.830~0.840nm 3 ,

[0015] The density of the main phase is 7.70-8.00 g / cm 3 .

[0016] <2> The Sm—Fe—N-based magnetic material according to <1>, wherein the volume fraction of the main phase is 95 to 100%.

[0017] <3> The Sm-Fe-N magnetic material according to <1> or <2>, wherein the lattice volume of the main phase is 0.833 to 0.835 nm 3 .

[0018] <4> The Sm—Fe—N-based magnetic material according to any one of <1> to <3>, wherein the density of the main phase is 7.70 to 7.90 g / cm 3 .

[0019] <5> A method for producing a Sm-Fe-N magnetic material, which is the method for producing a Sm-Fe-N magnetic material as described in <1>, comprising:

[0020] Prepare a magnetic material precursor, the magnetic material precursor having a formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 represents the composition of the crystalline phase, where R 1 is one or more rare earth elements other than Sm, La and Ce and Zr, M is one or more elements other than Fe, Co, Ni and rare earth elements and unavoidable impurity elements, and satisfies 0≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10 and 0≤s≤0.10; and

[0021] The magnetic material precursor is nitrided.

[0022] <6> The method according to <5>, wherein the volume fraction of the crystal phase is 95 to 100%.

[0023] <7> The method according to <5> or <6>, wherein after the magnetic material precursor is pulverized to obtain magnetic material precursor powder, the magnetic material precursor powder is nitrided.

[0024] <8> The method according to any one of <5> to <7>, wherein the magnetic material precursor is obtained by melting and solidifying a raw material containing an element constituting the magnetic material precursor.

[0025] According to the present disclosure, by setting the lattice volume and density of the main phase within predetermined ranges, it is possible to provide a Sm—Fe—N based magnetic material in which the saturation magnetization of the main phase itself is improved compared to the related art.

[0026] In addition, according to the present disclosure, by nitriding the magnetic material precursor so that the lattice volume and density of the main phase are within predetermined ranges, a method for producing a Sm-Fe-N based magnetic material in which the saturation magnetization of the main phase itself is improved compared with the conventional method can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will be described below with reference to the accompanying drawings, in which like reference numerals represent like elements, and in which:

[0028] Figure 1 It is a graph showing the relationship between the lattice volume and the saturation magnetization Ms (300K).

[0029] Figure 2 is a graph showing the relationship between lattice volume and density. DETAILED DESCRIPTION

[0030] Hereinafter, embodiments of the Sm-Fe-N system magnetic material and the method for producing the same according to the present disclosure will be described in detail. However, the embodiments described below do not limit the Sm-Fe-N system magnetic material and the method for producing the same according to the present disclosure.

[0031] Without being bound by theory, the reason why the saturation magnetization of the main phase itself is improved in the Sm—Fe—N based magnetic material disclosed herein is described below.

[0032] Depending on the type of rare earth element, a magnetic material (hard magnetic material) containing a rare earth element may exhibit strong magnetic force mainly in combination with Fe or in combination with Co. Regarding Sm, there may be a case where it exhibits strong magnetic force mainly in combination with Fe or in combination with Co.

[0033] In the case where Sm is mainly combined with Co to exhibit strong magnetic force, the main phase that exhibits strong magnetic force has a CaCo5 type crystal structure. The main phase having a CaCo5 type crystal structure is typically a SmCo5 phase. The SmCo5 phase exhibits strong magnetic force due to magnetization. On the other hand, in the case where Sm is mainly combined with Fe to exhibit strong magnetic force, the main phase that exhibits strong magnetic force has Th2Zn 17 Type and Th2Ni 17 At least one of the crystal structures of the Th2Zn type. 17 Type and Th2Ni 17 The main phase of at least one of the crystal structures of the type is typically Sm2Fe 17 N3 phase. Sm2Fe 17 The N3 phase is the N introduced into Sm2Fe 17 Phase. Sm2Fe 17 Even if the phase is magnetized, it does not exhibit strong magnetic force. 17 Phase nitridation to form Sm2Fe 17 In the N3 phase, a strong magnetic force is exhibited through magnetization.

[0034] So far, the research on Sm2Fe 17 Part of the Sm in the N3 phase is replaced with cheap light rare earth elements such as La and Ce, and / or part of the Fe is replaced with Co. However, it is believed that in order to replace part of the Sm with cheap light rare earth elements to improve economic efficiency, the replacement rate of light rare earth elements needs to be above a certain level, and the saturation magnetization of the main phase cannot be avoided. In addition, it is believed that when a part of the Fe is replaced with Co, the Curie temperature of the main phase rises, thereby suppressing the decrease in saturation magnetization at high temperatures (403-473K), but its effect requires the replacement rate of Ce to be about 0.1-0.4 mol.

[0035] Under this situation, the inventors focused on the lattice volume and density of the main phase to improve the Sm2Fe 17 N3 phase, and obtain a main phase with excellent saturation magnetization at room temperature. Moreover, in the past, it was believed that the lattice volume and density of the main phase had an inversely proportional relationship, but the inventors found that within the specified lattice volume range, when the density is higher than the above-mentioned inversely proportional relationship, the saturation magnetization of the main phase is improved. In addition, the inventors found that in order to obtain a lattice volume and density with improved saturation magnetization of the main phase, a part of Fe can be replaced with a small amount of Co and / or Ni, and a part of Sm can be optionally replaced with a small amount of La and / or Ce. Here, the so-called "small amount" refers to an amount less than the amount of light rare earth elements replaced when a part of Sm is replaced with light rare earth elements in order to improve economy, and also refers to an amount less than the amount of Co replaced when a part of Fe is replaced with Co in order to increase the Curie temperature.

[0036] Next, the constituent elements of the Sm—Fe—N-based magnetic material and the method for producing the same according to the present disclosure, which have been completed based on the findings described so far, will be described.

[0037] 《Sm-Fe-N Magnetic Materials》

[0038] The Sm-Fe-N system magnetic material disclosed in the present invention has Th2Zn 17 Type and Th2Ni 17 The main phase is a crystal structure of at least one type. The Sm-Fe-N system magnetic material disclosed in the present invention exhibits magnetism due to the main phase. The main phase is described below.

[0039] <Crystal Structure of Main Phase>

[0040] The main phase has Th2Zn 17 Type and Th2Ni 17 The crystal structure of the main phase may include at least one of the crystal structures of the Sm-Fe-N type. In addition to the above structure, the crystal structure of the main phase may also include a TbCu7 type crystal structure. It should be noted that Th is thorium, Zn is zinc, Ni is nickel, Tb is terbium, and Cu is copper. The crystal structure of the main phase can be identified by performing, for example, X-ray diffraction analysis on the Sm-Fe-N magnetic material.

[0041] The phase having the above-mentioned crystal structure can be realized by various combinations (compositions) of elements, but the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention is realized by the following combination (composition) of elements. The composition of the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention is described below.

[0042] <Composition of the main phase>

[0043] The main phase has the formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h In the above composition formula, Sm is samarium, La is lanthanum, Ce is cerium, Fe is iron, Co is cobalt, and Ni is nickel. 1 is one or more rare earth elements other than Sm, La and Ce and Zr, and M is one or more elements other than Fe, Co, Ni and rare earth elements and inevitable impurity elements. It is noted that Zr is zirconium. In the above formula, Sm is sometimes replaced by (1-x-y) Lax Ce y R 1 z called rare earth sites, Fe (1-p-q-s) Co p Ni q M s Called the iron group site.

[0044] As can be understood from the above formula, the main phase has 2 moles of one or more elements in the rare earth site, 17 moles of one or more elements in the iron group site, and h moles of nitrogen (N). That is, a phase having the above crystal structure is composed of one or more elements in the rare earth site and one or more elements in the iron group site, and h moles of nitrogen (N) are introduced into the phase in an intrusive manner. If the amount of nitrogen (N) introduced is h moles (where h is 2.9 to 3.1), the above crystal structure can be maintained. The details of nitrogen (N) in the main phase will be described later.

[0045] The rare earth sites are composed of Sm, La, Ce and R 1 Composition, Sm, La, Ce and R 1 Each is present in a ratio of (1-xyz):x:y:z in terms of molar ratio. Since (1-xyz)+x+y+z=1, it means that a portion of Sm is selected from La, Ce and R 1 Replace more than one element in .

[0046] The iron site is composed of Fe, Co, Ni and M, and each of Fe, Co, Ni and M is present in a ratio of (1-pqs):p:q:s in terms of molar ratio. Since (1-pqs)+p+q+s=1, it means that a portion of Fe is replaced by one or more elements selected from Co, Ni and M.

[0047] Hereinafter, each element constituting the above formula and its content ratio (molar ratio) will be described.

[0048] <sm>

[0049] Sm is a main element constituting the above-mentioned crystal structure together with Fe and N. A part of Sm is selected from La, Ce and R 1 In the following, La, Ce and R 1 Provide explanation.

[0050] <la>

[0051] The substitution of La for a portion of Sm contributes to the change in the lattice volume and density of the main phase, especially the lattice volume. The ionic radius of La is much larger than that of Sm, so when a portion of Sm is substituted with La, the lattice volume of the main phase is basically increased. However, when a small amount of La is substituted because the degree of intrusion of nitrogen (N) introduced into the main phase in an intrusive manner during nitridation fluctuates, the lattice volume of the main phase may also decrease.

[0052] As mentioned above, the ionic radius of La is much larger than that of Sm. Therefore, when a part of Sm is replaced by La, the change in the lattice volume of the main phase is greatly affected. When the lattice volume of the main phase exceeds the specified range, the above-mentioned crystal structure cannot be maintained, or even if the above-mentioned crystal structure can be maintained, the magnetic properties, especially the saturation magnetization, are deteriorated. In order to prevent this problem, when a part of Sm is replaced by La, it is necessary not to make the substitution rate of La too high.

[0053] La is a so-called light rare earth element and has a larger reserve (resource amount) and is cheaper than Sm. Therefore, by replacing a part of Sm with La, the amount of Sm used is reduced and the economic efficiency is improved, which is suitable.

[0054] <ce>

[0055] The substitution of Ce for a portion of Sm contributes to the change in the lattice volume and density of the main phase, especially the lattice volume. The ionic radius of Ce is slightly larger than the ionic radius of Sm, so when a portion of Sm is substituted with Ce, the lattice volume of the main phase is basically increased. However, since Ce ions can have trivalent and tetravalent valences, and the degree of intrusion of nitrogen (N) introduced into the main phase in an intrusive manner during nitridation fluctuates, when a portion of Sm is substituted with Ce, the lattice volume of the main phase may increase or decrease.

[0056] As described above, the ionic radius of Ce is slightly larger than that of Sm. Therefore, even if a part of Sm is replaced by Ce, the effect on the change of the lattice volume of the main phase is small. Accordingly, when the lattice volume of the main phase is changed, when a part of Sm is replaced by Ce, the amount of substitution by Ce becomes higher than when a part of Sm is replaced by La.

[0057] Ce belongs to the so-called light rare earth elements and has a larger reserve (resource amount) and is cheaper than Sm. Therefore, by replacing a part of Sm with Ce, the amount of Sm used is reduced and the economic efficiency is improved, which is suitable.

[0058] <R 1 >

[0059] R 1 It is one or more rare earth elements other than Sm, La and Ce, and Zr. 1 It is one or more elements that can be contained within a range that does not impair the magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention. 1 Typically, it is one or more rare earth elements other than Sm, La and Ce which are difficult to be completely separated from each of them when the raw material containing Sm, La and Ce is purified and a small amount of them remain in the raw material. 1 Zr may be contained. Zr is not a rare earth element, but sometimes a part of Sm is substituted with Zr. Even if a part of Sm is substituted with Zr, if the substitution amount is small, the magnetic properties of the Sm-Fe-N system magnetic material will not be significantly impaired.

[0060] In this specification, rare earth elements include 17 elements: Sc (scandium), Y (yttrium), La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium) and Lu (lutetium).

[0061] <fe>

[0062] Fe is a main element constituting the above-mentioned crystal structure together with Sm and N. A part of Fe may be substituted with one or more elements selected from Co, Ni and M. Hereinafter, Co, Ni and M will be described.

[0063] <co>

[0064] Co replaces part of Fe, which contributes to the change of the lattice volume and density of the main phase. The ionic radius of Co is smaller than that of Fe, so when a part of Fe is replaced by Co, the lattice volume of the main phase is basically reduced. However, due to the fluctuation of the intrusion degree of nitrogen (N) introduced into the main phase in an intrusive manner during nitridation, when a part of Fe is replaced by Co, the lattice volume of the main phase sometimes increases and sometimes decreases.

[0065] When a part of Fe is substituted with Co, the Curie temperature of the main phase rises, and the decrease in saturation magnetization at high temperature (403 to 473 K) can be suppressed, which is suitable.

[0066] <ni>

[0067] Ni replaces part of Fe, which contributes to the change of the lattice volume and density of the main phase. The ionic radius of Ni is smaller than that of Fe, so when part of Fe is replaced by Ni, the lattice volume of the main phase is basically reduced. However, due to the fluctuation of the intrusion degree of nitrogen (N) introduced into the main phase in an intrusive manner during nitridation, when part of Fe is replaced by Ni, the lattice volume of the main phase sometimes increases and sometimes decreases.

[0068] Compared with Fe, Ni contributes less to the presentation of magnetization. Therefore, it was previously believed that when a portion of Fe in the main phase was replaced with Ni, there was a concern that the magnetic properties would decrease. However, the ionic radius of Ni is smaller than the ionic radius of Co, so compared with the case where a portion of Fe is replaced with Co, when a portion of Fe is replaced with Ni, even if the substitution rate of Ni is not so high, the lattice volume of the main phase is significantly reduced. As a result, compared with the decrease in magnetic properties caused by replacing a portion of Fe with Ni, it was confirmed that the magnetic properties, especially the saturation magnetization, were improved due to the significant change in the lattice volume of the main phase.

[0069] <m>

[0070] M is one or more elements other than Fe, Co, Ni and rare earth elements and unavoidable impurity elements. M is one or more elements and unavoidable impurity elements that are allowed to be contained within the range that does not damage the magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention. The so-called unavoidable impurity elements refer to impurity elements that cannot be avoided when manufacturing the Sm-Fe-N system magnetic material disclosed in the present invention, or impurity elements that will cause a significant increase in manufacturing costs in order to avoid their inclusion. As such unavoidable impurity elements, there can be cited impurity elements in raw materials, or elements such as Cu (copper), Zn (zinc), Ga (gallium), Al (aluminum) and B (boron), which diffuse and / or invade the surface of the main phase when forming a bonded molded body. In addition, there can be cited elements contained in lubricants used during molding, and elements that diffuse and / or invade the surface of the main phase. It should be noted that the bonded molded body will be described later.

[0071] Examples of M other than the inevitable impurity elements include one or more elements selected from the group consisting of Ti (titanium), Cr (chromium), Mn (manganese), V (vanadium), Mo (molybdenum), W (tungsten) and C (carbon). These elements, for example, form nuclei when the main phase is generated, and contribute to promoting refinement of the main phase and / or suppressing grain growth of the main phase.

[0072] In addition, Zr may be included as M. As described above, Zr is not a rare earth element, but Zr may be used to replace a portion of Sm, and Zr may be used to replace a portion of Fe. In either case, if the amount of substitution is small, the magnetic properties of the Sm-Fe-N system magnetic material are not significantly impaired.

[0073] <n>

[0074] N is introduced into the main phase having the above-mentioned crystal structure in an intrusive manner. By introducing N to such an extent that N does not destroy the phase having the above-mentioned crystal structure, a magnetic moment is expressed in the main phase.

[0075] The Sm-Fe-N-based magnetic material disclosed herein has a main phase composed of the elements described above, and a desired saturation magnetization is obtained when the lattice volume and density of the main phase are within a predetermined range. The lattice volume and density are described below.

[0076] <Lattice Volume>

[0077] The lattice volume of the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention is 0.830 to 0.840 nm 3 When the lattice volume of the main phase is within the above range and the density of the main phase is within the range described below, a desired saturation magnetization is obtained.

[0078] Without being bound by theory, the reason why the lattice volume of the main phase needs to be within the above range in order to obtain desired saturation magnetization is considered to be as follows.

[0079] As described above, the saturation magnetization of Sm-Fe-N magnetic materials originates from the intrusion of N into the main phase, thereby presenting a magnetic moment in the main phase. As a result, the saturation magnetization is greatly affected by the Fe-N spacing in the lattice of the main phase (hereinafter sometimes referred to as "Fe-N spacing"). Fe and N are arranged in three dimensions in the lattice of the main phase, so the lattice volume of the main phase is suitable for grasping the Fe-N spacing.

[0080] In the Sm-Fe-N system magnetic material disclosed in the present invention, part of Fe is replaced by Co and / or Ni, and optionally part of Sm is replaced by La and / or Ce, thereby making Sm2Fe 17 The lattice volume of the N3 phase changes. At this time, it is believed that the Fe-N spacing in the main phase can be made close to that of Sm2Fe 17 Fe-N spacing in the lattice of N3 phase. Sm2Fe 17 The lattice volume of the N3 phase is about 0.838 nm 3 Therefore, it is believed that the lattice volume of the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention can be close to 0.838nm 3 From this point of view, the lattice volume of the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention can be 0.830nm 3 Above, 0.831nm 3 Above, 0.832nm 3 Above, 0.833nm 3 Above or 0.834nm 3 Above, it can be 0.840nm 3 Below, 0.839nm 3 Below, 0.838nm 3 Below, 0.837nm 3 Below, 0.836nm 3 Below or 0.835nm 3 the following.

[0081] The lattice volume of the main phase can be calculated by the following points. X-ray diffraction analysis is performed on the Sm-Fe-N magnetic material, and the a-axis length and the c-axis length are calculated from the X-ray diffraction pattern based on the relationship between the crystal plane index and the lattice plane spacing value (d value). When calculating the a-axis length and the c-axis length, the main phase of the Sm-Fe-N magnetic material disclosed in the present invention has the above-mentioned crystal structure, so it can be assumed that the main phase is a rhombohedral crystal. Therefore, as crystal plane indices, the (202) plane, (113) plane, (104) plane, (211) plane, (122) plane and (300) plane can be used. Then, the lattice volume is calculated according to the following formula.

[0082] (lattice volume) = {(a-axis length) / 2} 2 ×6×3 0.5 ×{(c-axis length) / 3}

[0083] <Density of main phase>

[0084] Generally, the lattice volume of the crystalline phase is inversely proportional to the density. However, in the Sm-Fe-N system magnetic material disclosed in the present invention, the lattice volume of the main phase is inversely proportional to the density. If the density is such, the saturation magnetization of the main phase is higher than that of Sm2Fe 17 Saturation magnetization of N3 phase. It was experimentally confirmed that such density is achieved when the lattice volume of the main phase is within the above range and a portion of Fe is replaced by a small amount of Co and / or Ni. Moreover, it was confirmed that a portion of Sm can be optionally replaced by La and / or Ce. Regarding "a small amount", it is as described. Specifically, x+y is greater than 0, greater than 0.01 or greater than 0.02, and is less than 0.04 or less than 0.03. In addition, the value of p+q is greater than 0.01, greater than 0.02 or greater than 0.03, and is less than 0.05 or less than 0.04.

[0085] The density of the main phase can be 7.70 g / cm 3 Above, 7.71g / cm 3 Above, 7.73g / cm 3 Above, 7.75g / cm 3 Above, 7.77g / cm 3 Above, 7.79g / cm 3 Above, 7.80g / cm 3 Above, 7.81g / cm 3 Above, 7.83g / cm 3 Above, 7.85g / cm 3 Above or 7.87g / cm 3 Above, it can be 8.00g / cm 3 Below, 7.98g / cm 3 Below, 7.96g / cm 3 Below, 7.94g / cm 3 Below, 7.92g / cm 3 Below or 7.90g / cm 3 the following.

[0086] The density of the main phase is obtained by crushing the Sm-Fe-N system magnetic material to obtain a powder and measuring the density of the powder using a pycnometer method. As described above, in the Sm-Fe-N system magnetic material disclosed in the present invention, the volume ratio of the main phase is preferably 95% or more. 17 The density of N3 phase and Sm2Fe3 phase is 7.65g / cm 3 and 8.25g / cm 3 Therefore, the density of the main phase can be approximated by the value obtained by the above-mentioned measurement method.

[0087] In the Sm-Fe-N system magnetic material disclosed herein, a portion of Fe is replaced by Co and / or Ni, and optionally a portion of Sm is replaced by La and / or Ce, so that the lattice volume and density of the main phase are within the above ranges. In this regard, the following formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h Provide explanation.

[0088] <x+y>

[0089] In the above formula representing the composition of the main phase, the value of x represents the ratio (molar ratio) of replacing a part of Sm with La, and the value of y represents the ratio (molar ratio) of replacing a part of Sm with Ce.

[0090] The lattice volume of the main phase is changed by replacing a part of Fe with Co and / or Ni, but a part of Sm may be optionally replaced with La and / or Ce to change the lattice volume of the main phase. Thus, the value of x+y may be greater than 0, greater than 0.01, or greater than 0.02. On the other hand, if the value of x+y is less than 0.04 or less than 0.03, the lattice volume of the main phase does not change excessively, especially does not increase excessively.

[0091] In addition, when the value of x+y satisfies the above range, the value of x may be greater than 0, greater than 0.01, or greater than 0.02, and may be less than 0.04 or less than 0.03. Similarly, when the value of x+y satisfies the above range, the value of y may be greater than 0, greater than 0.01, or greater than 0.02, and may be less than 0.04 or less than 0.03.

[0092] <z>

[0093] In the above formula representing the composition of the main phase, z represents R 1 The ratio (molar ratio) of replacing a part of Sm. As mentioned above, R 1 It is one or more rare earth elements and Zr that are allowed to be contained within the range that does not damage the magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention. Therefore, z can be less than 0.10, less than 0.08, less than 0.06, less than 0.04 or less than 0.02. On the other hand, the Sm-Fe-N system magnetic material disclosed in the present invention may not contain R 1 , that is, z can be 0, but when manufacturing the Sm-Fe-N system magnetic material disclosed in the present invention, it is difficult to completely eliminate R from the raw materials. 1 From this viewpoint, z may be 0.01 or more.

[0094] <p+q>

[0095] In the above formula representing the composition of the main phase, the value of p represents the ratio (molar ratio) of replacing a part of Fe with Co, and the value of q represents the ratio (molar ratio) of replacing a part of Fe with Ni.

[0096] As described above, a portion of Fe is replaced with Co and / or Ni to change the lattice volume of the main phase. If the value of p+q exceeds 0, the lattice volume of the main phase changes. From this viewpoint, the value of p+q can be greater than 0.01, greater than 0.02, or greater than 0.03. On the other hand, if the value of p+q is less than 0.10, the lattice volume of the main phase does not change excessively. From this viewpoint, the value of p+q can be less than 0.09, less than 0.08, less than 0.07, less than 0.06, less than 0.05, or less than 0.04.

[0097] In addition, when the value of p+q satisfies the above range, the value of p may exceed 0, be 0.01 or more, 0.02 or more, or 0.03 or less, 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less. Similarly, when the value of p+q satisfies the above range, the value of q may exceed 0, be 0.01 or more, 0.02 or more, or 0.03 or less, 0.10 or less, 0.09 or less, 0.08 or less, 0.07 or less, 0.06 or less, 0.05 or less, or 0.04 or less.

[0098] <s>

[0099] In the above formula representing the composition of the main phase, s represents the ratio (molar ratio) of replacing a part of Fe with M. As described above, M is one or more elements and inevitable impurity elements that can be contained within a range that does not impair the magnetic properties of the Sm-Fe-N-based magnetic material of the present disclosure. Thus, s can be 0.10 or less, 0.08 or less, 0.06 or less, 0.04 or less, or 0.02 or less. On the other hand, the Sm-Fe-N-based magnetic material of the present disclosure may contain no M at all, that is, s can be 0, but it is difficult to completely eliminate the inevitable impurity elements in M. From this perspective, s can be 0.01 or more.

[0100] <Relationships among x, y, z, p, q, and s>

[0101] x, y, z, p, q, and s respectively satisfy the conditions regarding x, y, z, p, q, and s described so far, and can be appropriately determined such that the lattice volume and density of the main phase are within the above ranges. At this time, x, y, p, and q preferably satisfy the relationship of the following formula (1).

[0102] 830 ≤ 16.267x + 3.927y - 26.279p - 56.5327q + 836 ≤ 840... Formula (1)

[0103] The reason why x, y, p, and q preferably satisfy Formula (1) will be described below.

[0104] In Formula (1), the relational expression represented by "16.267x + 3.927y - 26.279p - 56.5327q + 836" between the inequality signs represents the lattice volume of the main phase in terms of x, y, p, and q. This relational expression represents the calculation result of the lattice volume of the main phase when replacing a part of Sm with La and / or Ce and replacing a part of Fe with Co and / or Ni for the Sm2Fe 17 N3 phase using machine learning. Hereinafter, "16.267x + 3.927y - 26.279p - 56.5327q + 836" between the inequality signs in Formula (1) will sometimes be referred to as "the relational expression representing the lattice volume of the main phase".

[0105] Then, Formula (1) means that "the relational expression representing the lattice volume of the main phase" is in the range of 830 to 840 cubic angstroms (0.830 to 0.840 nm 3 ). As described above, the lattice volume of the main phase of the Sm-Fe-N-based magnetic material of the present disclosure is in the range of 0.830 to 0.840 nm 3 range. Thus, it means that the composition of the main phase of the Sm-Fe-N-based magnetic material of the present disclosure preferably has s, y, p, and q satisfying Formula (1).

[0106] The "relationship expressing the lattice volume of the main phase" does not include R related to z. 1 The reasons for s being related to M are as follows.

[0107] R 1 and M are one or more elements that are allowed to be contained within the range that does not damage the magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention. The magnetic properties are closely related to the lattice volume of the main phase. Therefore, as long as it is within the range that does not damage the magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention, the influence on the lattice volume of the main phase is also small, and the necessity of considering z and s is low. Therefore, in the "relationship formula representing the lattice volume of the main phase", z and s are not considered.

[0108] As described above, the “relationship expression representing the lattice volume of the main phase” is obtained through machine learning, but it represents the following technical significance and is considered to be highly reliable.

[0109] First, when x=y=p=q=0, it means that part of Sm is not replaced by La and / or Ce, and part of Fe is not replaced by Co and / or Ni. 17 The lattice volume of the N3 phase is 836 cubic angstroms (0.836 nm 3 ). It is known that the actual Sm2Fe 17 The lattice volume of the N3 phase is about 0.838 nm 3 Therefore, it can be understood that Sm2Fe 17 The value of the lattice volume of the N3 phase is very close to the actual value.

[0110] The ratio of the coefficients of x and y (16.267:3.927) is close to the ratio of the ionic radius of La to the ionic radius of Ce. The ratio of the absolute values ​​of the coefficients of p and q (26.279:56.5327) is close to the ratio of the ionic radius of Co to the ionic radius of Ni.

[0111] Each of the above coefficients indicates the magnitude of the effect on the change in the lattice volume of the main phase when a part of Sm is substituted with La and / or Ce, or a part of Fe is substituted with Co and / or Ni.

[0112] The coefficients of x and y are positive, which means that when a part of Sm is replaced by La and / or Ce, the lattice volume of the main phase is basically increased. The coefficient of x is larger than the coefficient of y, which means that since the ionic radius of La is larger than the ionic radius of Ce, replacing a part of Sm with La has a greater effect on the change in the lattice volume of the main phase than replacing a part of Sm with Ce.

[0113] The coefficients of p and q are negative, which means that when a part of Fe is replaced by Co and / or Ni, the lattice volume of the main phase is basically reduced. The absolute value of the coefficient of q is greater than the absolute value of the coefficient of p, which means that since the ionic radius of Ni is larger than the ionic radius of Co, replacing a part of Fe with Ni has a greater effect on the change in the lattice volume of the main phase than replacing a part of Fe with Co.

[0114] The reason why the wording "basically" is used in the expressions related to the coefficients of the "relationship expression representing the lattice volume of the main phase" described so far is explained.

[0115] The "relationship formula representing the lattice volume of the main phase" in formula (1) is related to Sm2Fe 17 The results are related to the N3 phase and are obtained by using machine learning by assuming that part of Sm is replaced by La and / or Ce and part of Fe is replaced by Co and / or Ni. 17 When the phase is nitrided, not only Sm2Fe 17 N3 phase, and Sm2Fe 17 N h (h is 2.9 to 3.1) The details of h will be described later.

[0116] Depending on the degree of nitridation, the coefficients of x, y, p and q change. The smaller the absolute value of the coefficient, the more easily it is affected by the degree of nitridation. For example, the absolute value of the coefficient of y is the smallest among the coefficients of x, y, p and q, so y is easily affected by the degree of nitridation. Specifically, when a part of Sm is replaced by Ce, basically, the lattice volume of the main phase increases. Therefore, basically, the coefficient of y is positive. However, depending on the degree of nitridation, the coefficient of y sometimes decreases. In this case, since the absolute value of the coefficient of y is small, the coefficient of y can become negative by reducing the coefficient of y. The coefficient of y becomes negative, which means that even when a part of Sm is replaced by Ce, the lattice volume of the main phase is reduced. This is because the ionic radius of Ce is large compared to the ionic radius of Sm, but the difference is small, so the absolute value of the coefficient of y is small. In addition, this is also because Ce ions have trivalent and tetravalent valences, and the coefficient of y is easy to change.

[0117] On the other hand, the ionic radius of La is very large compared to the ionic radius of Sm, and therefore, it is not easily affected by the degree of nitridation. Specifically, when a portion of Sm is replaced by La, basically, the lattice volume of the main phase increases. Therefore, basically, the coefficient of x is positive. However, depending on the degree of nitridation, the coefficient of x sometimes decreases. Even in this case, the absolute value of the coefficient of x is relatively large, so even if the coefficient of x decreases, it is difficult for the coefficient of x to become negative. As a case where the coefficient of x decreases until the coefficient of x becomes negative according to the degree of nitridation, a case where a small amount of La is used as a substitution amount can be cited.

[0118] When a part of Fe is replaced by Co and / or Ni, the lattice volume of the main phase is basically reduced. Therefore, basically, the coefficients of p and q are negative. However, sometimes the coefficients of p and q increase due to the degree of nitridation. Even in this case, since the absolute values ​​of the coefficients of p and q are greater than the absolute values ​​of the coefficients of x and y, even if the coefficients of p and q increase, the coefficients of p and q are difficult to become positive.

[0119] As explained so far, the "relationship formula representing the lattice volume of the main phase" in formula (1) has the above-mentioned technical significance even if it is obtained through machine learning. In addition, it has been confirmed through experiments that if the lattice volume of the main phase is 0.830 to 0.840 nm 3 The density of the main phase is 7.70-8.00 g / cm 3 , the desired saturation magnetization is obtained. Therefore, regarding x, y, p and q, it is preferred that the equation (1) is satisfied first.

[0120] In addition, the density of the main phase is 7.70 to 8.00 g / cm 3 The x, y, p and q can be obtained by machine learning using the following formula (2) as a reference.

[0121] 0.0619≤-0.817x-0.5669y+0.499p+2.606q≤0.16194…Formula (2)

[0122] <h>

[0123] Next, h, which indicates the degree of nitridation, is described. 17 During nitridation, basically, Sm2Fe is formed 17 N h phase (where h = 3). Nitriding is typically accomplished by converting the Sm2Fe 17 The Sm-Fe-N system magnetic material precursor (hereinafter sometimes referred to as "precursor") of the phase is exposed to a nitrogen atmosphere at high temperature. Therefore, due to the different degrees of nitridation on the surface and inside of the precursor, h can vary in the range of 2.9 to 3.1. The same is true when a part of Sm is replaced by La and / or Ce, and a part of Fe is replaced by Co and / or Ni in the precursor. That is, (Sm,La,Ce)2(Fe,Co,Ni) 17 When the phase is nitrided, (Sm,La,Ce)2(Fe,Co,Ni) is formed 17 N h phase (where h is 2.9 to 3.1).

[0124] <Volume Ratio of Main Phase>

[0125] The Sm-Fe-N system magnetic material disclosed in the present invention has a main phase represented by the above-mentioned composition formula. The magnetic properties of the Sm-Fe-N system magnetic material disclosed in the present invention are presented by the main phase. Therefore, the volume ratio of the main phase is preferably higher relative to the entire Sm-Fe-N system magnetic material disclosed in the present invention. Specifically, the volume ratio of the main phase can be 95% or more, 96% or more, or 97% or more relative to the entire Sm-Fe-N system magnetic material disclosed in the present invention. On the other hand, when manufacturing the Sm-Fe-N system magnetic material disclosed in the present invention, there are the following situations: there is a process in which a phase other than the main phase represented by the above-mentioned composition formula is in a stable temperature region. In addition, it is sometimes difficult to completely eliminate the inevitable impurity elements that do not constitute the main phase. Therefore, although the volume ratio of the main phase is ideally 100%, as long as the volume ratio of the above-mentioned main phase is ensured, there is no problem in practical use even if the volume ratio of the main phase is 99% or less or 98% or less.

[0126] Phases other than the main phase typically exist at the grain boundaries between the main phases, particularly at triple points. Typical examples of phases other than the main phase include SmFe3 phases and their nitrided phases. The SmFe3 phase and its nitrided phase contain: a portion of Sm is selected from La, Ce and R 1 phases in which a part of Fe is replaced by one or more elements selected from Co, Ni and M and nitrided phases thereof, and phases in which a part of Sm is replaced by one or more elements selected from La, Ce and R 1 Phases in which a portion of Fe is substituted with one or more elements selected from Co, Ni and M, and their nitrided phases.

[0127] The volume fraction of the main phase was determined by using high-frequency inductively coupled plasma atomic emission spectrometry (ICP-AES) to measure the overall composition of the precursor before nitridation. Based on the measured values, it was assumed that the precursor before nitridation was divided into (Sm, La, Ce, R 1 )2(Fe,Co,Ni,M) 17 Phase and (Sm, La, Ce, R 1 Specifically, after obtaining the mass concentration (mass ratio) of each element from the ICP measurement results, Sm2Fe 17 The mass ratio of the SmFe3 phase and the SmFe3 phase is calculated from the density of each phase. 1 )2(Fe,Co,Ni,M) 17 Phase representation Sm2Fe 17 Phase, Sm2Fe 17 A portion of the Sm phase is selected from Sm, La, Ce and R 1 Phases in which one or more elements are substituted, Sm2Fe 17 A phase in which a portion of Fe is replaced by one or more elements selected from Co, Ni and M, and a phase in which Sm2Fe 17 A portion of the Sm phase is selected from Sm, La, Ce and R 1 More than one element in Sm2Fe 17 A phase in which part of Fe is replaced by one or more elements selected from Co, Ni and M. In addition, (Sm, La, Ce, R 1 )(Fe,Co,Ni,M)3 phase means SmFe3 phase, a part of Sm in SmFe3 phase is selected from Sm, La, Ce and R 1 phase in which a portion of Fe in the SmFe3 phase is replaced by one or more elements selected from Co, Ni and M, and a portion of Sm in the SmFe3 phase is replaced by one or more elements selected from Sm, La, Ce and R 1 A phase in which a portion of Fe in the SmFe3 phase is replaced by one or more elements selected from Co, Ni and M.

[0128] From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase and its nitrided phase during the manufacture of the Sm-Fe-N system magnetic material disclosed in the present invention, the overall composition (the sum of the main phase and phases other than the main phase) of the Sm-Fe-N system magnetic material disclosed in the present invention can be set to Sm, La, Ce and R in the main phase. 1 That is, the overall composition of the Sm-Fe-N based magnetic material disclosed in the present invention can be (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 N h (wherein w is 2.00 to 3.00). In this case, x, y, z, p, q, s and h may be the same as x, y, z, p, q, s and h in the formula representing the composition of the above-mentioned main phase. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more or 2.50 or more. On the other hand, from the viewpoint of reducing the above-mentioned (Sm, La, Ce, R 1 From the viewpoint of the volume ratio of the (Fe, Co, Ni, M)3 phase, w is preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.

[0129] 《Manufacturing method》

[0130] Next, a method for producing a Sm-Fe-N-based magnetic material of the present disclosure (hereinafter sometimes referred to as “the production method of the present disclosure”) is described.

[0131] The manufacturing method disclosed in the present invention includes a magnetic material precursor preparation step and a nitridation step. Each step will be described below.

[0132] <Magnetic material precursor preparation step>

[0133] In the production method disclosed in the present invention, a compound having a formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 Represents the composition of the crystalline phase of the magnetic material precursor.

[0134] In the formula representing the composition of the crystal phase, Sm, La, Ce, R 1 , Fe, Co, Ni and M as well as x, y, z, p, q and s, as described in "Sm-Fe-N Magnetic Materials".

[0135] The crystal phase of the magnetic material precursor has Th2Zn 17 Type and Th2Ni 17 When the magnetic material precursor is nitrided, the crystal phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention. The main phase of the Sm-Fe-N system magnetic material disclosed in the present invention has Th2Zn 17 Type and Th2Ni 17 Thus, nitridation is performed to maintain the Th2Zn 17 Type and Th2Ni 17 The degree of crystal structure of at least one type.

[0136] As described above, the crystalline phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention, so it can be considered that the volume ratio of the crystalline phase in the magnetic material precursor is the same as the volume ratio of the main phase in the Sm-Fe-N system magnetic material disclosed in the present invention. Therefore, the volume ratio of the crystalline phase of the magnetic material precursor can be 95% or more, 96% or more, or 97% or more relative to the entire magnetic material precursor. When manufacturing a magnetic material precursor, there are the following situations: there is a process in which a phase other than the crystalline phase represented by the above-mentioned composition formula is in a stable temperature region. In addition, it is sometimes difficult to completely eliminate the inevitable impurity elements that do not constitute the crystalline phase. The volume ratio of the crystalline phase is ideally 100%, but as long as the volume ratio of the above-mentioned crystalline phase is ensured, there is no problem in practical use even if the volume ratio of the main phase is less than 99% or less than 98%.

[0137] Phases other than the crystalline phase typically exist at the grain boundaries between the crystalline phases, particularly at triple points. Typical examples of phases other than the crystalline phase include the SmFe3 phase. The SmFe3 phase contains: a portion of Sm selected from La, Ce, and R 1 phase in which a part of Fe is replaced by one or more elements selected from Co, Ni and M, and a part of Sm is replaced by one or more elements selected from La, Ce and R 1 A phase in which a portion of Fe is substituted by one or more elements selected from Co, Ni and M.

[0138] The volume fraction of the crystalline phase was determined by using high-frequency inductively coupled plasma atomic emission spectrometry (ICP-AES) to measure the overall composition of the precursor before nitridation. Based on the measured values, it was assumed that the precursor before nitridation was divided into (Sm, La, Ce, R 1 )2(Fe,Co,Ni,M) 17 Phase and (Sm, La, Ce, R 1 Specifically, after obtaining the weight concentration (weight ratio) of each element from the ICP measurement results, Sm2Fe 17 The weight ratio of the SmFe3 phase and the SmFe3 phase is calculated from the density of each phase. 1 )2(Fe,Co,Ni,M) 17 Phase representation Sm2Fe 17 Phase, Sm2Fe 17 A portion of the Sm phase is selected from Sm, La, Ce and R 1 Phases in which one or more elements are substituted, Sm2Fe 17 A phase in which a portion of Fe is replaced by one or more elements selected from Co, Ni and M, and a phase in which Sm2Fe 17 A portion of the Sm phase is selected from Sm, La, Ce and R 1 More than one element in Sm2Fe 17 A phase in which part of Fe is replaced by one or more elements selected from Co, Ni and M. In addition, (Sm, La, Ce, R 1 )(Fe,Co,Ni,M)3 phase means SmFe3 phase, a part of Sm in SmFe3 phase is selected from Sm, La, Ce and R 1 phase in which a portion of Fe in the SmFe3 phase is replaced by one or more elements selected from Co, Ni and M, and a portion of Sm in the SmFe3 phase is replaced by one or more elements selected from Sm, La, Ce and R 1 A phase in which a portion of Fe in the SmFe3 phase is replaced by one or more elements selected from Co, Ni and M.

[0139] From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase during the manufacture of the magnetic material precursor, the overall composition of the magnetic material precursor (the sum of the crystalline phase and the phases other than the crystalline phase) can be set to Sm, La, Ce and R in the crystalline phase. 1 That is, the overall composition of the magnetic material precursor can be (Sm (1-x-y-z) La x Ce y R 1 z ) w (Fe (1-p-q-s) Co p Ni q M s ) 17 (wherein w is 2.00 to 3.00). In this case, x, y, z, p, q and s may be the same as x, y, z, p, q and s in the formula representing the composition of the above-mentioned crystalline phase. From the viewpoint of suppressing the appearance of the α-(Fe, Co, Ni, M) phase, w is preferably 2.02 or more, 2.04 or more, 2.06 or more, 2.08 or more, 2.10 or more, 2.20 or more, 2.30 or more, 2.40 or more or 2.50 or more. On the other hand, from the viewpoint of reducing the (Sm, La, Ce, R 1 From the viewpoint of the volume ratio of the (Fe, Co, Ni, M)3 phase, w is preferably 2.90 or less, 2.80 or less, 2.70 or less, or 2.60 or less.

[0140] The magnetic material precursor can be obtained using a well-known manufacturing method. As a method for obtaining a magnetic material precursor, for example, it can be cited that the raw material containing the elements constituting the magnetic material precursor is melted and solidified. As a melting method for raw materials, for example, the following can be cited: the raw material is loaded into a container such as a crucible, the raw material is melted or high-frequency melted in the container, and after obtaining the molten metal, the molten metal is injected into a mold such as a book mold, or the molten metal is solidified in a crucible. From the perspective of suppressing the coarsening of the crystal phase in the magnetic material precursor and improving the homogenization of the crystal phase, it is preferred to increase the cooling rate of the molten metal. From this perspective, it is preferred to inject the molten metal into a mold such as a book mold. Furthermore, from the perspective of suppressing the coarsening of the crystal phase in the magnetic material precursor and improving the homogenization of the crystal phase, for example, the following method can also be used. That is, the raw material can be melted in a container by high-frequency melting or arc melting, and the ingot obtained by solidification can be melted again by high-frequency melting, etc., and the molten liquid is quenched using a strip casting method and a liquid quenching method, etc. to obtain a thin sheet, and the thin sheet is used as a magnetic material precursor.

[0141] Before the nitridation described below, in order to homogenize the grains in the magnetic material precursor, the magnetic material precursor may be heat treated (hereinafter, this heat treatment is sometimes referred to as "homogenization heat treatment"). The temperature of the homogenization heat treatment may be, for example, above 1273K, above 1323K, or above 1373K, and may be below 1523K, below 1473K, or below 1423K. The homogenization heat treatment time may be, for example, above 6 hours, above 12 hours, above 18 hours, or above 24 hours, and may be below 48 hours, below 42 hours, below 36 hours, or below 30 hours.

[0142] The homogenization heat treatment is preferably performed in a vacuum or inert gas atmosphere to suppress oxidation of the magnetic material precursor. The inert gas atmosphere does not include a nitrogen atmosphere. This is because when the homogenization heat treatment is performed in a nitrogen atmosphere, the Th2Zn 17 Type and / or Th2Ni 17 The phase with this type of crystal structure is easy to decompose.

[0143] <Nitriding process>

[0144] The magnetic material precursor is nitrided. Thus, the crystal phase in the magnetic material precursor is nitrided to form the main phase of the Sm-Fe-N system magnetic material disclosed in the present invention.

[0145] As long as the desired main phase can be obtained, there is no particular limitation on the nitriding method. Typically, for example, the following can be mentioned: while heating the magnetic material precursor, exposing it to an atmosphere containing nitrogen, or exposing it to a gas atmosphere containing nitrogen (N). As an atmosphere containing nitrogen, for example, a nitrogen atmosphere, a mixed gas atmosphere of nitrogen and an inert gas, and a mixed gas atmosphere of nitrogen and hydrogen can be mentioned. As a gas atmosphere containing nitrogen (N), for example, an ammonia atmosphere or a mixed gas atmosphere of ammonia and hydrogen can be mentioned. The atmospheres exemplified so far can also be combined. From the viewpoint of the efficiency of nitriding, an ammonia atmosphere, a mixed gas atmosphere of ammonia and hydrogen, and a mixed gas atmosphere of nitrogen and hydrogen are preferred.

[0146] The magnetic material precursor may be crushed before nitriding to obtain the magnetic material precursor powder, and then the magnetic material precursor powder may be nitrided. By nitriding after crushing the magnetic material precursor, the crystal phase present in the magnetic material precursor can be fully nitrided. The crushing of the magnetic material precursor is preferably carried out in an inert gas atmosphere. The inert gas atmosphere may include a nitrogen atmosphere. Thus, oxidation of the magnetic material precursor during crushing can be suppressed. As the particle size of the magnetic material precursor powder, D 50 The thickness may be 5 μm or more, 10 μm or more, or 15 μm or more, and may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less.

[0147] The nitriding temperature may be, for example, 673 K or more, 698 K or more, 723 K or more, or 748 K or more, and may be 823 K or less, 798 K or less, or 773 K or less. In addition, the nitriding time may be, for example, 4 hours or more, 8 hours or more, 12 hours or more, or 16 hours or more, and may be 48 hours or less, 36 hours or less, 24 hours or less, 20 hours or less, or 18 hours or less.

[0148] Metamorphosis

[0149] The Sm-Fe-N system magnetic material and its manufacturing method disclosed in the present invention are not limited to the embodiments described so far, and can be appropriately modified within the scope described in the claims. For example, the Sm-Fe-N system magnetic material disclosed in the present invention can be a powder or a molded body of the powder. The molded body can be a bonded molded body or a sintered molded body. In the case of a molded body, a bonded molded body is preferred from the viewpoint of easily avoiding the temperature at which nitrogen (N) in the main phase is separated (decomposed) during the molding process. As an adhesive, for example, resins and low-melting-point metal adhesives can be mentioned. As a low-melting-point metal adhesive, for example, metallic zinc, or zinc alloys and combinations thereof can be mentioned.

[0150] The Sm-Fe-N system magnetic material and the method for producing the same are further described in detail below by way of examples and comparative examples. It should be noted that the Sm-Fe-N system magnetic material and the method for producing the same are not limited to the conditions used in the following examples.

[0151] 《Sample Preparation》

[0152] Samples of Sm-Fe-N based magnetic materials were prepared in the following manner.

[0153] Metal Sm, metal La, Ce-Fe alloy, metal Fe, metal Co and metal Ni are combined so that the main phase has the composition described in Table 1-1, and the mixture is subjected to high-frequency melting and solidification at 1673K (1400°C) to obtain a magnetic material precursor. When combined, the total molar number of Sm, La and Ce is greater than the total molar number of Sm, La and Ce in the main phase, so that the volume ratio of the main phase is 95 to 100%. It should be noted that in this specification, for example, the so-called "metal Sm" refers to unalloyed Sm. Metal Sm may of course contain inevitable impurities.

[0154] The magnetic material precursor was homogenized and heat-treated at 1373 K in an argon atmosphere for 24 hours.

[0155] The magnetic material precursor after homogenization heat treatment was placed in a glove box and crushed using a cutter mill in a nitrogen atmosphere. The particle size of the crushed magnetic material precursor powder was 1.37 mm / s. 50 The thickness is calculated to be less than 20 μm.

[0156] The magnetic material precursor powder was heated to 748 K in a nitrogen atmosphere and nitrided for 16 hours. The nitridation amount was determined by the change in mass of the magnetic material precursor powder before and after nitridation.

[0157] "evaluate"

[0158] For each sample, the composition, volume fraction, density and lattice volume of the main phase were obtained by the above-mentioned measurement method. In addition, for each sample, the magnetic properties were measured using the physical property measurement system PPMS (registered trademark)-VSM with a maximum load magnetic field of 9T. For the measurement of magnetic properties, the powders of each sample after nitridation were solidified in an ethylene oxide resin while being oriented in a magnetic field, and the magnetic properties of each solidified sample were measured at 300-453K in the direction of the easy magnetization axis and the direction of the difficult magnetization axis. The saturation magnetization Ms was calculated using the law of approach to saturation from the measured values ​​in the direction of the easy magnetization axis. In addition, the anisotropic magnetic field Ha was obtained from the intersection of the hysteresis curve in the direction of the easy magnetization axis and the hysteresis curve in the direction of the difficult magnetization axis.

[0159] The results are shown in Table 1-2. Figure 1 It is a graph showing the relationship between the lattice volume and the saturation magnetization Ms (300K). Figure 2 is a graph showing the relationship between lattice volume and density.

[0160]

[0161]

[0162] According to Table 1-1 and Table 1-2 and Figure 1 and Figure 2 For the samples of Examples 1 to 5, the lattice volume of the main phase is 0.830 to 0.840 nm. 3 , and the density of the main phase is 7.70~8.00g / cm 3 , so it can be understood that the saturation magnetization is improved. In addition, according to Figure 2 It can be understood that in the samples of Comparative Examples 1 to 14, the lattice volume and the density are inversely proportional to each other, and regarding the samples of Examples 1 to 5, the density becomes higher than this relationship.

[0163] From the above results, the effects of the Sm—Fe—N-based magnetic material and the method for producing the same according to the present disclosure can be confirmed.< / h> < / s> < / z> < / n> < / m> < / ni> < / co> < / fe> < / ce> < / la> < / sm>

Claims

1. Sm-Fe-N magnetic material, which has Th2Zn 17 Type and Th2Ni 17 A Sm-Fe-N based magnetic material having a main phase of at least any one of the crystal structures of the type, wherein The above main phase has a formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 N h Represents the composition, where R 1 is one or more rare earth elements other than Sm, La and Ce and Zr, M is one or more elements other than Fe, Co, Ni and rare earth elements and unavoidable impurity elements, and satisfies 0.01≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10, 0≤s≤0.10 and 2.9≤h≤3.1, The volume ratio of the main phase is 95 to 100%. The lattice volume of the above main phase is 0.830~0.840nm 3 ,and The density of the main phase is 7.70-8.00 g / cm 3 .

2. The Sm-Fe-N based magnetic material according to claim 1, wherein: The lattice volume of the above main phase is 0.833~0.835nm 3 .

3. The Sm-Fe-N based magnetic material according to claim 1 or 2, wherein: The density of the main phase is 7.70-7.90 g / cm 3 .

4. A method for producing a Sm-Fe-N magnetic material, which is the method for producing a Sm-Fe-N magnetic material according to claim 1, comprising: Prepare a magnetic material precursor, the magnetic material precursor having a formula (Sm (1-x-y-z) La x Ce y R 1 z )2(Fe (1-p-q-s) Co p Ni q M s ) 17 represents the composition of the crystalline phase, where R 1 is one or more rare earth elements other than Sm, La and Ce and Zr, M is one or more elements other than Fe, Co, Ni and rare earth elements and unavoidable impurity elements, and satisfies 0.01≤x+y<0.04, 0≤z≤0.10, 0<p+q≤0.10 and 0≤s≤0.10; and The magnetic material precursor is nitrided. The volume ratio of the above-mentioned crystal phase is 95 to 100%.

5. The method according to claim 4, wherein: After the magnetic material precursor is crushed to obtain magnetic material precursor powder, the magnetic material precursor powder is nitrided.

6. The method according to claim 4 or 5, wherein: The magnetic material precursor is obtained by melting and solidifying a raw material containing elements constituting the magnetic material precursor.