Non-volatile memory structure and manufacturing method thereof

By arranging multi-layer insulating blocks and fluid material concave steps in the non-volatile memory, a highly consistent air gap is formed, which solves the electrical instability problem caused by uneven air gaps in the existing technology and improves the memory stability and reliability.

CN114256252BActive Publication Date: 2024-10-29WINBOND ELECTRONICS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202011000067.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-22
Publication Date
2024-10-29
Estimated Expiration
2040-09-22

AI Technical Summary

Technical Problem

In existing non-volatile memories, the height and contour of the air gaps between adjacent control gates are uneven, resulting in unstable electrical performance and leakage current problems.

Method used

By arranging multi-layer insulating blocks in the non-volatile memory structure, the mobile material in the trench is used to perform a concave step with a consistent depth to form a highly consistent air gap to ensure that the dielectric layer does not fill the trench. This improves the height and profile consistency of the air gap, reduces the presence of dielectric layers, and enhances electrical isolation.

Benefits of technology

It improves the stability of non-volatile memory, reduces leakage current, and improves electrical performance and product reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114256252B_ABST
    Figure CN114256252B_ABST
Patent Text Reader

Abstract

The present invention provides a non-volatile memory structure and a manufacturing method thereof, wherein the non-volatile memory comprises: a substrate and a tunneling dielectric layer on the substrate; a plurality of gate structures located in an array region of the substrate and arranged at a distance from each other, each gate structure comprising a floating gate and a control gate located above the floating gate; a first dielectric layer located above the tunneling dielectric layer and covering the gate structure, the first dielectric layer being formed above the substrate and covering the top surface of the tunneling dielectric layer and covering the side and top surfaces of each gate structure, wherein the space between the first dielectric layers on the side surfaces of adjacent gate structures is filled with air gaps; a plurality of insulating blocks and a second dielectric layer, wherein the insulating blocks are located on the first dielectric layer and correspond to each gate structure respectively, and the second dielectric layer is located on the insulating block and covers the insulating block and the air gap. The present invention can reduce leakage current and reduce coupling capacitance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a non-volatile memory structure and a manufacturing method thereof, and in particular to a non-volatile memory structure with an air gap of uniform height and a manufacturing method thereof. Background Art

[0002] In non-volatile memory, there are two major categories of products, namely read-only memory (ROM) and flash memory, depending on whether the data in the memory can be rewritten at any time when the computer is used. Among them, flash memory has gradually become the mainstream technology of non-volatile memory due to its low cost.

[0003] Generally speaking, a flash memory contains two gates, the first gate is a floating gate that stores data, and the second gate is a control gate that performs data input and output. The floating gate is located below the control gate and is in a "floating" state. The so-called floating means that the floating gate is surrounded and isolated by insulating material to prevent charge loss. The control gate is connected to the word line to control the device. One of the advantages of flash memory is that it can erase data block-by-block (block-by-block erasing). Flash memory is widely used in enterprise servers, storage and network technology, as well as a wide range of consumer electronic products, such as flash drives, mobile phones, digital cameras, tablets, personal computer plug-ins for notebook computers and embedded controllers, etc.

[0004] In the conventional non-volatile memory, the air gap between adjacent control gates is not uniform in height and profile, which affects the stability of the electrical performance of the memory. Furthermore, in the conventional non-volatile memory, the height of the air gap is lower than the control gate, so the dielectric layer (such as an oxide layer) deposited above the control gate will also fill in between the adjacent control gates. In other words, in addition to the air gap, there will also be a dielectric layer (such as an oxide layer) between the adjacent control gates, which will cause leakage current problems, reducing the electrical performance and reliability of the memory.

[0005] Therefore, although the existing methods of forming non-volatile memories are sufficient to cope with their originally intended uses, they still do not fully meet the requirements in all aspects, so the technology of non-volatile memories still has problems to overcome. Summary of the invention

[0006] In non-volatile memory, there are two major categories of products, namely read-only memory (ROM) and flash memory, depending on whether the data in the memory can be rewritten at any time when the computer is used. Among them, flash memory has gradually become the mainstream technology of non-volatile memory due to its low cost.

[0007] Generally speaking, a flash memory contains two gates, the first gate is a floating gate that stores data, and the second gate is a control gate that performs data input and output. The floating gate is located below the control gate and is in a "floating" state. The so-called floating means that the floating gate is surrounded and isolated by insulating material to prevent charge loss. The control gate is connected to the word line to control the device. One of the advantages of flash memory is that it can erase data block-by-block. Flash memory is widely used in enterprise servers, storage and network technology, as well as a wide range of consumer electronic products, such as flash drives, mobile phones, digital cameras, tablets, notebook personal computer plug-ins and embedded controllers, etc.

[0008] In the conventional non-volatile memory, the air gap between adjacent control gates is not uniform in height and profile, which affects the stability of the electrical performance of the memory. Furthermore, in the conventional non-volatile memory, the height of the air gap is lower than the control gate, so the dielectric layer (such as an oxide layer) deposited above the control gate will also fill in between the adjacent control gates. In other words, in addition to the air gap, there will also be a dielectric layer (such as an oxide layer) between the adjacent control gates, which will cause leakage current problems, reducing the electrical performance and reliability of the memory.

[0009] Therefore, although the existing methods of forming non-volatile memories are sufficient to cope with their originally intended uses, they still do not fully meet the requirements in all aspects, so the technology of non-volatile memories still has problems to overcome. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] FIG. 1A to FIG. 1I 2 are cross-sectional schematic diagrams corresponding to different intermediate stages of manufacturing a non-volatile memory structure according to some embodiments of the present invention.

[0011] FIG. 2A to FIG. 2F 1 is a cross-sectional schematic diagram corresponding to different intermediate stages of manufacturing a non-volatile memory structure according to another embodiment of the present invention, which shows the steps of Figure 1G Another manufacturing process after step.

[0012]

Explanation of symbols

[0013] 10: Substrate

[0014] 12: Tunneling dielectric layer

[0015] 14: Gate structure

[0016] 141: floating gate

[0017] 142: Inter-gate dielectric layer

[0018] 144: Polysilicon gate

[0019] 144a, 145a, 182a, 191a, 211a, 214a, 291a: top surface

[0020] 145:Metal gate

[0021] 16, 23: Dielectric layer

[0022] 161, 211, 311: Part I

[0023] 162, 212s, 212b, 312s, 312b: Part II

[0024] 162s, 211s, 311s: Side

[0025] 163, 213, 313: Part 3

[0026] 164, 214, 314: Part 4

[0027] 171: First groove

[0028] 1710, 2710: Depression

[0029] 172: Second groove

[0030] 18, 182: Oxide layer

[0031] 19, 191, 29, 291: Flowable materials

[0032] 21, 31: Insulation material layer

[0033] 211', 214': insulation block (first insulation layer)

[0034] 311', 314': second insulating layer

[0035] 23b: Bottom

[0036] 25, 35: air gap

[0037] 25a, 35a: Top

[0038] A1: First Area

[0039] A2: Second Area

[0040] CG: Control Gate

[0041] D1, D2, D3: Direction

[0042] H1, H2: Height

[0043] IL1, IL2: Insulation block

[0044] S1, S2: stacked structure

[0045] T S0 、T S1 、T S2 :thickness

[0046] W1, W Air :width DETAILED DESCRIPTION

[0047] The present invention is more fully described with reference to the drawings of the embodiments of the present invention. However, the present invention may be embodied in various forms and should not be limited to the embodiments described herein. The thickness of the layers and regions in the drawings are exaggerated for clarity. The same or similar element numbers represent the same or similar elements, and the following paragraphs will not be repeated one by one.

[0048] The non-volatile memory structure proposed in the embodiment can be a non-volatile memory structure of different types, wherein the memory structure including a floating gate can be applied to the embodiment of the present invention. A non-volatile memory structure can include multiple stacked structures. In the example, multiple first stacked structures and multiple second stacked structures are arranged in a first region (e.g., an array region, or an active region) and a second region (e.g., a peripheral region) of a substrate, and a dielectric layer covers the top surface and the side surface of the aforementioned stacked structure. Each stacked structure at least includes a floating gate, a control gate, and an inter-gate dielectric layer between the floating gate and the control gate above the substrate, wherein there is a highly consistent air gap between the dielectric layers on the side surfaces of adjacent first stacked structures. According to some embodiments of the present invention, these air gaps fill the space between the first dielectric layers on the side surfaces of adjacent first stacked structures. The aforementioned air gap has a sufficient width to expose all dielectric layers covering the side surfaces of the first stacked structure, and the details of its manufacturing method and the obtained structure will be described later. To simplify the description, the accompanying drawings of the embodiment depict three first stack structures and one second stack structure above the substrate and air gaps extending between the first stack structures to illustrate an example of a non-volatile memory structure.

[0049] FIG. 1A to FIG. 1I 1 is a cross-sectional view corresponding to different intermediate stages of manufacturing a non-volatile memory structure according to some embodiments of the present invention. Figure 1A, a substrate 10 is provided, and a tunnel dielectric layer 12 is formed on the substrate 10. In some embodiments, the substrate 10 includes a first region (e.g., an array region) A1 and a second region (e.g., a peripheral region) A2. The material of the substrate 10 may include silicon, gallium arsenide, gallium nitride, silicon germanium, silicon on insulator (SOI), other suitable materials, or a combination of the foregoing. In some embodiments, the material of the tunnel dielectric layer 12 is, for example, silicon oxide or a high dielectric constant material (the dielectric constant is, for example, greater than 4). The high dielectric constant material may, for example, include hafnium oxide, hafnium silicon oxide, hafnium aluminum oxide, or hafnium tantalum oxide. In one embodiment, the thickness of the tunnel dielectric layer 12 may range from about 3 nm to about 10 nm.

[0050] Refer to Figure 1A , forming a plurality of stacked structures on the tunnel dielectric layer 12, for example, forming a stacked structure S1 and a stacked structure S2 respectively located in the first area A1 and the second area A2, and the aforementioned stacked structures are arranged at a distance from each other in the direction D1 (such as the X direction). Furthermore, each stacked structure includes two or more material layers vertically stacked in the direction D2 (such as the Z direction) and extending in the direction D3 (such as the Y direction).

[0051] In one embodiment, the stacked structure S1 is a plurality of gate structures 14 located in an array region, each gate structure comprising a floating gate 141, an inter-gate dielectric layer 142, and a control gate CG, wherein the floating gate 141 is located on the tunneling dielectric layer 12, the control gate CG is located above the floating gate 141, and the inter-gate dielectric layer 142 is located between the floating gate 141 and the control gate CG.

[0052] In some embodiments, the floating gate 141 includes polysilicon. In one embodiment, the inter-gate dielectric layer 142 may be a single-layer structure or a multi-layer structure, and the material of the inter-gate dielectric layer 142 may include silicon oxide, silicon nitride, or a combination thereof. For example, the inter-gate dielectric layer 142 may be a structure of silicon oxide / silicon nitride / silicon oxide (ONO structure), or a NONON structure. Furthermore, the control gate CG may be a single-layer or multi-layer structure. In some embodiments, the material of the control gate CG includes polysilicon, metal, metal silicide, or other conductive material. For example, the metal may include titanium, tantalum, tungsten, aluminum, or zirconium. The metal silicide may include nickel silicide, titanium silicide, tungsten silicide, or cobalt silicide. In this example, the control gate CG includes a polysilicon gate 144 and a metal gate 145 located on the polysilicon gate 144, and the metal gate 145 includes, for example, a metal silicide, such as cobalt silicide. In addition, in this example, the stacked structure S2 includes the same material layer stack as the stacked structure S1, which is not repeated here.

[0053] Reference Figure 1B , a dielectric layer 16 is formed above the substrate 10, and the dielectric layer 16 covers the top surface of the tunnel dielectric layer 12 and covers the top and side surfaces of the stacked structure S1 and the stacked structure S2. In this example, the dielectric layer 16 includes a first portion 161 located on the top surface of the stacked structure S1 (for example, the top surface 145a of the metal gate 145), a second portion 162 located between adjacent stacked structures S1, a third portion 163 located between adjacent stacked structures S2, and a fourth portion 164 located on the top surface of the stacked structure S2. The second portion 162 and the third portion 163 are respectively formed like liners between adjacent stacked structures S1 and between adjacent stacked structures S2. Figure 1B As shown, the second portion 162 covers the side of the floating gate 141, the side of the inter-gate dielectric layer 142 and the side of the control gate CG (eg including the polysilicon gate 144 and the metal gate 145). Furthermore, in one embodiment, the dielectric layer 16 is a nitride layer, such as silicon nitride.

[0054] like Figure 1B As shown, after the dielectric layer 16 is formed, there is a first groove 171 between adjacent stacked structures S1, and there is a second groove 172 between adjacent stacked structures S1 and stacked structures S2. In one example, the stacked structure S1 is located in the array region of the substrate 10 (i.e., the aforementioned first region A1), and the stacked structure S2 is located in the peripheral region of the substrate 10 (i.e., the aforementioned second region A2). Compared with the stacked structure S2, the stacked structure S1 is more densely arranged, and there is a wider spacing between the stacked structure S1 in the array region and the stacked structure S2 in the peripheral region, so the width of the second groove 172 in the direction D1 is greater than the width of the first groove 171 in the direction D1.

[0055] Next, a plurality of insulating blocks (such as Figure 1H The insulating blocks 211' and 214' shown in the figure are on the dielectric layer 16, and these insulating blocks correspond to the top surfaces of the stacking structure S1 and the stacking structure S2 respectively. Figure 1C to Figure 1H A cross-sectional schematic diagram corresponding to a method for manufacturing an insulating block according to an embodiment of the present invention is described.

[0056] Reference Figure 1C , forming an oxide layer 18 on the dielectric layer 16. For example, the oxide layer 18 is deposited on the dielectric layer 16 by a non-conformal deposition method. Since the stack structure S1 is more densely arranged than the stack structure S2, the width of the first trench 171 is smaller and the width of the second trench 172 is larger. Therefore, after deposition, the oxide layer 18 does not fill the first trench 171 (i.e., is located above the first trench 171), but can fill the larger second trench 172.

[0057] Reference Figure 1D Then, a portion of the oxide layer 18 is removed to expose the dielectric layer 16 and the first trench 171, and the remaining portion 182 of the oxide layer fills the second trench 172. Specifically, for example, a portion of the oxide layer 18 is removed by chemical mechanical polishing (CMP), and after removal, the first trench 171 and the dielectric layer 16 covering the stacked structure S1 are exposed, and the top surface 182a of the portion 182 of the oxide layer remaining in the second trench 172 is substantially coplanar with the top surface of the fourth portion 164 of the adjacent dielectric layer 16 (located above the stacked structure S2). In this example, when removing a portion of the oxide layer 18, the dielectric layer 16 can be used as a polishing stop layer.

[0058] Reference Figure 1E Then, a fluid material 19 is deposited on the dielectric layer 16 and on the remaining portion 182 of the oxide layer, wherein the fluid material 19 fills the first trench 171. The fluid material 19 is, for example, a material containing carbon and oxygen and having a flowable property. In some embodiments, the fluid material 19 includes an organic dielectric layer (ODL), spin-on carbon, a photoresist layer, a bottom anti-reflective coating (BARC), a deep UV light absorbing oxide (DUO), or other suitable materials. In this example, the fluid material 19 is an organic dielectric layer.

[0059] Reference Figure 1F Then, a portion of the fluid material 19 is removed to expose the dielectric layer 16 and the remaining portion 182 of the oxide layer, so that the fluid material corresponding to the first trench 171 is recessed. Figure 1F As shown, after removing part of the fluid material 19, recessed portions 1710 are formed above the fluid material 191 remaining in the first trench 171. In this example, these recessed portions 1710 expose at least a portion of the dielectric layer 16 covering the side surface of the stacked structure S1.

[0060] Furthermore, according to the present invention, the depth of the depression of the fluid material 19 (i.e., the height of the recessed portion 1710 in the direction D2) should not be too deep, so as to avoid closing the recessed portion 1710 when the insulating material layer is subsequently deposited. The depth of the depression of the fluid material 19 should not be too shallow, so as to avoid the thickness difference between the insulating material layer subsequently deposited above the stacked structure and the insulating material layer deposited in the recessed portion being too small. If the aforementioned thickness difference is too small, after the process of removing the material layer filled in the first groove, an insulating block with sufficient thickness will not be left above the stacked structure, thereby affecting the height of the air gap finally formed. As for the value of the depression depth of the fluid material 19, it can be appropriately adjusted depending on the size of the groove (including depth and width) in actual application.

[0061] In some embodiments, after removing a portion of the fluid material 191, the top surface 191a of the fluid material 191 remaining in the first trench 171 is lower than the top surface of the stacked structure S1. Figure 1F As shown, in this example, the top surface 191a of the fluid material 191 left in the first trench 171 is lower than the top surface 145a of the metal gate 145 in the stacked structure S1, but not lower than the top surface 144a of the polysilicon gate 144 in the stacked structure S1. However, the present invention is not limited to the aforementioned position for the top surface of the fluid material 191 left in the first trench 171 after the fluid material 19 is recessed.

[0062] Reference Figure 1G Then, D1 forms an insulating material layer 21 on the dielectric layer 16, the remaining oxide layer portion 182, and the remaining fluid material 191. An insulating material layer 21 is deposited on the dielectric layer 16 in a conformal manner. In this example, the insulating material layer 21 includes a first portion 211 located on the top surface of the stacked structure S1 (e.g., the top surface 145a of the metal gate 145), a second portion 212s and 212b deposited on the sidewalls and bottom surface of the recess 1710, a third portion 213 located on the remaining oxide layer 182, and a fourth portion 214 located on the top surface of the stacked structure S2. In addition, the insulating material layer 21 is, for example, an oxide layer.

[0063] Furthermore, since the stacked structure S1 is more densely arranged, the width of the first trench 171 is smaller, so the thickness of the second portion 212s and 212b of the insulating material layer 21 deposited on the sidewall and bottom surface of the recessed portion 1710 is less than the thickness deposited on the top surface of the stacked structure S1. That is, the thickness T of the first portion 211 (in the direction D2) of the insulating material layer 21 is S0 Greater than the thickness T of the second portion 212b (in the direction D2) S1 .

[0064] Reference Figure 1H Then, the insulating material layer and the fluid material at the first groove 171 are removed. Specifically, a portion of the insulating material layer 21 is removed (for example, the second portion 212s and 212b deposited on the sidewall and bottom surface of the recessed portion 1710 are removed in this example), and the remaining fluid material 191 corresponding to the first groove 171 is removed, so that the first groove 171 is exposed, and a plurality of insulating blocks 211' and 214' are formed, respectively corresponding to the stacked structure S1 and the upper portion S2 of the second stacked structure, as shown in FIG. Figure 1H shown.

[0065] In some embodiments, the insulating material layer and the fluid material 191 are removed by dry etching. Figure 1G The thickness T of the first portion 211 of the deposited insulating material layer 21 is shown as S0 is much larger than the thickness T of the second portion 212b S1 Therefore, no mask is required, and the fluid material 191 can be removed by a self-aligned etching step. Figure 1H As shown, the thickness T of the insulating blocks 211' and 214' formed after etching is S2 Less than the thickness T of the first portion 211 deposited before etching S0 , but the height above the stacked structure can be increased, which helps to increase the height of the air gap formed subsequently.

[0066] Furthermore, if Figure 1H As shown in FIG. 1 , after the self-aligned etching step, the side surface 211s of each insulating block 211' is substantially flush with the side surface of the first dielectric layer. Figure 1H In the example shown, the side surface 211 s of each insulating block 211 ′ is substantially flush with the side surface 162 s of the second portion 162 of the first dielectric layer located between adjacent stacked structures S1 .

[0067] Reference Fig. 1I Then, a dielectric layer 23 is formed on the insulating block 211' (corresponding to the stacking structure S1) and the insulating block 214' (corresponding to the stacking structure S2), and an air gap 25 is formed, and the dielectric layer 23 covers the air gap 25 and the insulating blocks 211' and 214'. Specifically, after the dielectric layer 23 is formed, the air gap 25 is formed in the space between the bottom surface 23b of the dielectric layer 23 and the first trench 171 and the insulating block 211' above the stacking structure S1.

[0068] According to some embodiments of the present invention, the formed air gap 25 at least fills the space between the first dielectric layer (e.g., the second portion 162) on the side of the adjacent stacked structures S1. In other words, only the dielectric layer 16 and the air gap 25 exist between the adjacent stacked structures S1 in the direction D1, and no dielectric layer 23 exists.

[0069] According to the present invention, the material of the dielectric layer 23 is different from the material of the dielectric layer 16. In this example, the dielectric layer 23 is an oxide layer, and the dielectric layer 16 is a nitride layer. Furthermore, in some embodiments, the material of the dielectric layer 23 and the insulating material layer 21 / insulating block 211', 214' are the same, for example, including the same oxide.

[0070] like Fig. 1I In the structure shown, due to the provision of the insulating blocks 211' and 214', the first groove 171 between adjacent stacked structures S1 can extend in the direction D2, thereby increasing the distance between the subsequently deposited dielectric layer 23 and the substrate 10, and further increasing the height of the air gap 25 (in the direction D2) between the adjacent stacked structures S1. Therefore, in some embodiments, the formed air gap 25 not only fills the space between the first dielectric layer (such as the second portion 162) on the side of the adjacent stacked structure S1, but also fills the space between the adjacent insulating blocks 211' (corresponding to the top of the stacked structure S1). In other words, between the adjacent stacked structures S1 and between the adjacent insulating blocks 211' in the direction D1, only the dielectric layer 16 and the air gap 25 exist, and no dielectric layer 23 exists.

[0071] like Fig. 1I As shown, the width W1 of the space between the first dielectric layers (eg, the second portion 162) on the side of the stack structure S1 in the direction D1 is equal to the width W1 of the air gap in the direction D1. Air equal.

[0072] Furthermore, if Fig. 1I As shown, in one example, the air gap 25 at least exposes a portion of the dielectric layer (e.g., the second portion 162) located on all sides of the control gate CG of each stacked structure S1. In this example, the air gap 25 extending in the direction D2 also directly contacts the side of the insulating block 211', so that only the dielectric layer 16 and the air gap 25 exist between adjacent insulating blocks 211' in the direction D1, and no dielectric layer 23 exists.

[0073] Furthermore, in some embodiments, the top end 25 a of the air gap 25 extending in the direction D2 is higher than the top surface 211 a of the insulating block 211 ′.

[0074] In addition, the dielectric layer 23 can be deposited by a general deposition method or other suitable deposition methods. In some examples, the stacked structures S1 in the first area A1 (eg, array area) are arranged more closely and have narrow first trenches 171 , so the dielectric layer 23 is not easy to fill in the first trenches 171 .

[0075] In some other examples, tetraethoxysilane (TEOS) material can be selected and deposited in a selective manner. For example, TEOS is deposited at sub-atmospheric pressure (SA) by chemical vapor deposition to form a dielectric layer 23. The TEOS sub-atmospheric pressure process has different deposition rates on different materials, for example, a faster deposition rate on an oxide layer and a slower deposition rate on a nitride layer, and the deposition rate ratio is, for example, about 2:1. In this example, the insulating block 211' is, for example, an oxide layer, and the dielectric layer 16 on the side of the stacked structure S1 is, for example, a nitride layer, and the dielectric layer 23 is not easy to fill in the narrow first trench 171. Therefore, after the dielectric layer 23 is deposited, the air gap 25 formed, such as Fig. 1I As shown, the top end 25a thereof is higher than the top surface 211a of the insulating block 211'.

[0076] In some embodiments, the ratio of the deposition rate of the dielectric layer 23 on the insulating block 211 ′ to the deposition rate on the dielectric layer 16 is, for example, in a range from about 1.5 to about 2.5, such as about 2.

[0077] According to the above embodiment, by setting the insulating blocks 211' and 214' ( Figure 1H ), so that the first trench 171 between adjacent stacked structures S1 can extend in the direction D2 to increase the distance between the subsequently deposited dielectric layer 23 and the substrate 10 ( Fig. 1I ), thereby increasing the height of the air gap 25 (in the direction D2) between the adjacent stacked structures S1. Furthermore, by performing a recessing step of the fluid material 191 in each first trench with a uniform depth, the insulating blocks 211' and 214' with a uniform thickness can be formed subsequently, thereby controlling the height and profile consistency of the subsequently formed air gap 25, thereby improving the stability of the non-volatile memory structure. In some embodiments, the air gap 25 has the same height in the direction D2 (e.g., the Z direction).

[0078] FIG. 2A to FIG. 2F 1 is a cross-sectional schematic diagram corresponding to different intermediate stages of manufacturing a non-volatile memory structure according to another embodiment of the present invention, which shows the steps of Figure 1G Another manufacturing process after step. FIG. 2A to FIG. 2F Zhongyu FIG. 1A to FIG. 1I The same or similar elements are marked with the same or similar reference numerals to facilitate clear description.

[0079] Figure 2A The formation steps and configuration of Figure 1H The formation steps and configurations are the same, and for simplicity, they are not described in detail. In addition, in this example, the insulating blocks 211', 214' formed on the stacked structures S1, S2 respectively according to the aforementioned method are referred to as first insulating layers 211', 214' in the following description.

[0080] Next, refer to Figure 2B In one embodiment, another fluid material 29 is deposited on the first insulating layers 211' and 214'. The fluid material 29 can be made of the same material as the fluid material 19. The deposition method and material of the fluid material 29 are the same as those of the fluid material 19, and are not described again here.

[0081] Next, refer to Figure 2C In one embodiment, a portion of the fluid material 29 is removed to expose the first insulating layer 211', 214' and the remaining oxide layer portion 182, so that the fluid material 29 corresponding to the first trench 171 is recessed. Figure 2C As shown, after a portion of the fluid material 29 is removed, a recess 2710 is formed above the fluid material 291 remaining in the first groove 171 .

[0082] In some embodiments, after removing a portion of the fluid material 29, the top surface 291a of the fluid material 291 remaining in the first trench 171 is lower than the top surfaces 211a, 214a of the first insulating layers 211', 214'. Figure 2C As shown, the depth of the recess of the fluid material 29 is, for example (but not limited to), such that the side surfaces of the first insulating layer 211 ′ and 214 ′ are exposed.

[0083] Next, refer to Figure 2D In one embodiment, another insulating material layer 31 is formed on the first insulating layer 211', 214', the remaining oxide layer portion 182 and the remaining fluid material 291. In this example, the insulating material layer 31 is deposited by isotropic deposition. The insulating material layer 31 is, for example, an oxide layer. In addition, the insulating material layer 31 can have the same or different material as the insulating material layer 21; and the insulating material layer 31 can have the same or different thickness as the insulating material layer 21, depending on the actual application conditions.

[0084] like Figure 2DAs shown, in one example, the insulating material layer 31 includes a first portion 311 located on the top surface of the first insulating layer 211', a second portion 312s and 312b deposited on the side walls and bottom surface of the recess 2710, a third portion 313 located above the remaining oxide layer 182, and a fourth portion 314 located on the top surface of the first insulating layer 214'.

[0085] Next, refer to Figure 2E In one embodiment, the insulating material layer and the fluid material at the first trench 171 are removed. Specifically, the second portions 312s and 312b of the insulating material layer 31 (located on the sidewalls and bottom surface of the recessed portion 2710) are removed, and the remaining fluid material 291 corresponding to the first trench 171 is removed to expose the first trench 171, and second insulating layers 311' and 314' are formed above the first insulating layers 211' and 214', respectively. Figure 2E As shown, the first insulating layer 211' and the second insulating layer 311' corresponding to the stacked structure S1 form an insulating block IL1, and the first insulating layer 214' and the second insulating layer 314' corresponding to the first stacked structure S2 form an insulating block IL2. At this step, an insulating block containing two insulating layers is constructed above the stacked structure.

[0086] Similarly, the insulating material layer and the fluid material 291 at the first trench 171 can be removed without using a mask. For example, the removal is performed by self-aligned etching, and after the removal, the side surfaces of each insulating block are substantially flush with the side surfaces of the dielectric layer 16. Figure 2E As shown, the side surface 211 s of the first insulating layer 211 ′ and the side surface 311 s of the second insulating layer 311 ′ included in the insulating block IL1 are substantially flush with the side surface 162 s of the dielectric layer 16 .

[0087] Afterwards, refer to Figure 2F In one embodiment, a dielectric layer 23 is formed on the second insulating layer 311' (corresponding to the stacking structure S1) and the second insulating layer 314' (corresponding to the stacking structure S2), and an air gap 35 is formed. The dielectric layer 23 can be deposited by a general deposition method or other suitable deposition methods. For example, the dielectric layer 23 can be formed by a sub-atmospheric pressure (SA) selective deposition method, the contents of which are described above and will not be repeated here.

[0088] In some embodiments, each air gap 35 extending in the direction D2 directly contacts the side surfaces of the first insulating layer 211' and the second insulating layer 311' of each insulating block. Figure 2FAs shown, according to some embodiments of the present invention, the formed air gap 35 not only fills the space between the first dielectric layers (such as the second portion 162) on the side of the adjacent stacked structures S1, and fills the space between the adjacent first insulating layers 211' (corresponding to the top of the stacked structure S1), but also fills the space between the adjacent second insulating layers 311' (corresponding to the top of the stacked structure S1). In other words, between the adjacent stacked structures S1, between the adjacent first insulating layers 211', and between the adjacent second insulating layers 311' in the direction D1, only the dielectric layer 16 and the air gap 25 exist, and no dielectric layer 23 exists.

[0089] According to the above embodiment FIG. 2A to FIG. 2E As shown, an insulating block having a multilayer structure (e.g. Figure 2E Insulation blocks IL1 and IL2 are shown in the figure, wherein each insulation block comprises a plurality of insulation layers vertically stacked in a direction D2. Furthermore, the following steps may be repeated depending on the actual process requirements. FIG. 2A to FIG. 2E steps to produce an insulating block containing three or more insulating material layers.

[0090] Furthermore, comparison Fig. 1I The air gap of 25 and Figure 2F The air gap 35 has a height H2 in the direction D2 greater than the height H1 of the air gap 25 in the direction D2 (H2>H1). Therefore, the thicker the insulating block is or the more insulating layers it contains, the higher the height of the air gap in the direction D2 is.

[0091] In summary, the non-volatile memory structure and manufacturing method proposed in some embodiments of the present invention have many advantages. For example, a single-layer or multi-layer insulating block can be provided in a simple manner without increasing additional manufacturing costs, thereby increasing the height of the air gap 25 / 35 formed between the stacked structures (e.g., word line gate structures) in the future. The thickness of the insulating block and / or the number of insulating layers included depends on the height of the air gap to be formed. The embodiments also form an insulating block with a uniform thickness in the future by performing a recessing step of a flowable material filled in the grooves (e.g., the first grooves) between the stacked structures, thereby controlling the consistency of the height and profile of each air gap 25 / 35, thereby improving the stability of the non-volatile memory structure. Furthermore, according to the manufacturing method of the embodiment, the fluid material in the first trench can be completely removed by self-aligned etching without using a mask, so as to form a sufficiently wide air gap 25 / 35 after depositing the dielectric layer 23, so that only the dielectric layer 16 (such as a nitride layer) and the air gap 25 / 35 exist between adjacent stacked structures (such as word line gate structures), and no dielectric layer 23 (such as an oxide layer) exists. Even between adjacent insulating blocks, only the air gap 25 / 35 exists without the dielectric layer 23, thereby improving the electrical isolation between adjacent stacked structures (such as word line gate structures), reducing leakage current and coupling capacitance, so that the non-volatile memory structure has stable electrical performance, thereby improving the yield and reliability of the final product.

[0092] Although the present invention has been disclosed as above with several preferred embodiments, they are not intended to limit the present invention. Any person skilled in the art may make any changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the definition of the claims.

Claims

1. A non-volatile memory structure, characterized in that: include: A substrate comprising an array region and a peripheral region; a tunnel dielectric layer located on the substrate; A plurality of gate structures are located above the substrate and in the array region, and the gate structures are spaced apart from each other, each of the gate structures comprising a floating gate located on the tunnel dielectric layer and a control gate located above the floating gate; a stacked structure located above the substrate and in the peripheral region and adjacent to the array region, wherein the distance between the gate structure closest to the peripheral region among the gate structures and the stacked structure is greater than the distance between two adjacent gate structures; a first dielectric layer, located above the substrate and covering the top surface of the tunnel dielectric layer, the first dielectric layer also covering the side surfaces and top surfaces of the aforementioned gate structures and the stacked structure, wherein the space between the first dielectric layers on the side surfaces of the adjacent gate structures is filled with air gaps, and the space between the gate structure closest to the peripheral region and the first dielectric layers on the side surfaces of the stacked structure is filled with an oxide layer; A plurality of insulating blocks are located on the first dielectric layer in the array region and correspond to the gate structures respectively; an insulating layer located on the first dielectric layer and the oxide layer in the peripheral region and covering and contacting the first dielectric layer and the oxide layer; and A second dielectric layer is located on the insulating blocks and covers the insulating blocks and the air gaps.

2. The non-volatile memory structure according to claim 1, characterized in that: Top ends of the air gaps are higher than top surfaces of the insulating blocks.

3. The non-volatile memory structure according to claim 1, characterized in that: The air gaps at least expose a portion of the first dielectric layer on all sides of the control gate of each of the aforementioned gate structures.

4. The non-volatile memory structure according to claim 1, characterized in that: The air gaps more directly contact the side surfaces of the insulating blocks.

5. The non-volatile memory structure according to claim 1, characterized in that: The air gaps have the same height in a direction perpendicular to the substrate.

6. The non-volatile memory structure according to claim 1, characterized in that: The aforementioned insulating blocks and the control gate of the aforementioned gate structures are separated by the first dielectric layer.

7. The non-volatile memory structure according to claim 1, characterized in that: The side surfaces of the aforementioned insulating blocks are flush with the side surfaces of the first dielectric layer.

8. The non-volatile memory structure according to claim 1, characterized in that: In each of the aforementioned gate structures, the control gate includes a polysilicon gate and a metal gate located on the polysilicon gate, wherein each of the aforementioned insulating blocks and the metal gate of each of the aforementioned gate structures are separated by the first dielectric layer.

9. A method for manufacturing a non-volatile memory structure, characterized in that: include: Providing a substrate, the substrate comprising a first region and a second region; forming a tunnel dielectric layer on the substrate; Forming a plurality of first stacked structures and a plurality of second stacked structures spaced apart from each other on the tunnel dielectric layer, wherein the first stacked structures and the second stacked structures are respectively located in the first region and the second region; A first dielectric layer is formed on the substrate and covers the top surface of the tunnel dielectric layer and the top and side surfaces of the first stacked structures and the second stacked structures, wherein after the first dielectric layer is formed, a first trench is provided between the first stacked structures, and a second trench is provided between adjacent first stacked structures and second stacked structures, wherein the width of the second trench in the first direction is greater than the width of each of the aforementioned first trenches in the first direction, and further comprising: Depositing an oxide layer on the first dielectric layer, wherein the oxide layer is located above the first trenches but fills the second trenches; Removing a portion of the oxide layer to expose the first dielectric layer and the first trenches, and leaving the oxide layer to fill the second trenches; Depositing a fluid material on the first dielectric layer and the remaining oxide layer, wherein the fluid material fills the first trenches; and Removing a portion of the fluid material to make the fluid material corresponding to the first grooves concave: Removing the remaining fluid material corresponding to the first trenches and forming a plurality of insulating blocks on the first dielectric layer, wherein the insulating blocks correspond to the top surfaces of the first stack structures and the second stack structures respectively; and A second dielectric layer is formed above the first stacked structures and the second stacked structures, and air gaps are formed. The second dielectric layer covers the insulating blocks and the air gaps, wherein the air gaps fill the spaces between the first dielectric layers on the sides of the adjacent first stacked structures.

10. The method for manufacturing a non-volatile memory structure according to claim 9, characterized in that: The air gaps further fill up the spaces between the insulating blocks on the adjacent first stacked structures, and the top ends of the air gaps are higher than the top surfaces of the insulating blocks.

11. The method for manufacturing a non-volatile memory structure according to claim 9, characterized in that: After removing part of the fluid material, recesses are formed above the fluid material remaining in the first grooves, wherein the recesses expose at least a portion of the first dielectric layer covering the side surfaces of the first stacking structures, and the top surface of the fluid material remaining in the first grooves is lower than the top surface of the first stacking structures.

12. The method for manufacturing a non-volatile memory structure according to claim 9, wherein: Each of the above-mentioned first stacked structures includes a floating gate located on the tunneling dielectric layer and a control gate located above the floating gate, and the control gate includes a polysilicon gate and a metal gate located on the polysilicon gate. After removing part of the fluid material, the top surface of the fluid material remaining in the first trenches is not lower than the top surfaces of the polysilicon gates of the first stacked structures.

13. The method for manufacturing a non-volatile memory structure according to claim 9, characterized in that: After removing part of the flowable material, the method further comprises: forming an insulating material layer on the first dielectric layer, the remaining oxide layer and the remaining fluid material; removing the portion of the insulating material layer corresponding to the first trenches and the remaining fluid material to expose the first trenches and form the insulating blocks corresponding to the first stacked structures and the second stacked structures; and The second dielectric layer is deposited.

Citation Information

Patent Citations

  • Flash memory manufacturing method

    CN106653758A

  • Method of manufacturing a semiconductor device

    KR100843044B1

  • Semiconductor memory device and method for manufacturing the same

    US20150060986A1