A binder for preparing positive electrode slurry of lithium-sulfur soft-pack battery

By using composite binders of PEO, CMS-Na and PSSA-Li in the positive electrode of lithium sulfur battery, the problems of volume changes in sulfur positive electrode material and the shuttle effect of polysulfide dissolution are solved, and the circulation and rate performance of lithium sulfur batteries are improved. .

CN114284500BActive Publication Date: 2024-12-03GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111603908.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-12-03
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

The volume of the sulfur positive electrode material of lithium sulfur batteries changes greatly during the charging and discharging process, resulting in unstable structure, and the polysulfide dissolution shuttle effect leads to poor circulation performance. The conductivity of sulfur elements and its electrochemical reaction products is insufficient, which affects the rate performance.

Method used

The composite binder is made of polyethylene oxide (PEO), sodium carboxymethyl starch (CMS-Na) and poly(4-styrene sulfonic acid) lithium salt (PSSA-Li) as the main components, and it is mutually connected by hydrogen bonding. The cross-linking network is formed, which enhances the solid sulfur performance and structural stability, and uses the good ionic conductivity of PSSA-Li to reduce the positive electrode sheet impedance and inhibits the diffusion of polysulfides.

Benefits of technology

It significantly improves the mechanical stability, solid sulfur characteristics and conductivity of the positive electrode of the lithium-sulfur battery, extends the cycle life and improves the rate performance, and prevents cracking and brittle breaking of the electrode sheet structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114284500B_ABST
    Figure CN114284500B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-sulfur battery binders, and in particular to a binder for preparing positive electrode slurry of lithium-sulfur soft-pack batteries. The binder is made of polyethylene oxide, sodium carboxymethyl starch and poly (4-styrene sulfonic acid) lithium salt, and has good bonding performance, sulfur fixation performance, structural stability and electrical conductivity. The binder is used for preparing positive electrode slurry of lithium-sulfur batteries, can prevent cracking and brittle fracture of pole piece structures, ensure ion transmission and electron transmission, and greatly improve the cycle performance and rate performance of positive electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium-sulfur battery binders, and in particular to a binder for preparing positive electrode slurry of lithium-sulfur soft-pack batteries. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicles, lithium-sulfur batteries with high theoretical energy density (2600Wh·kg -1 ) is attracting more and more attention. Lithium-sulfur batteries use lightweight, low-cost, environmentally friendly and large-capacity lithium metal anodes (3860mAh·g -1 ) and elemental sulfur (1675 mAh g -1 ) as the electrode material, so that its actual energy density can reach 500-600Wh·kg -1 , almost twice that of traditional lithium-ion batteries (patent CN112652773A). However, the commercial application of lithium-sulfur batteries is hindered by some of their own problems. First, the volume change of sulfur positive electrode materials during charging and discharging is large, which is not conducive to maintaining the structural integrity of the sulfur positive electrode during the electrochemical process; secondly, during the electrochemical reaction of the sulfur positive electrode, polysulfides that can be dissolved in the electrolyte will be produced. These polysulfides will pass through the diaphragm, reach the surface of the lithium metal negative electrode and react with metallic lithium, which is not conducive to maintaining the cycle performance of the lithium-sulfur battery; finally, the electronic conductivity of sulfur and its electrochemical reaction products (such as Li2S2 and Li2S) is poor, which is not conducive to improving the rate performance of lithium-sulfur batteries.

[0003] The properties of the positive electrode of lithium-sulfur batteries are important factors affecting the electrochemical performance of lithium-sulfur batteries, and the type and properties of the binder are important aspects that affect the structural integrity of the positive electrode of lithium-sulfur batteries, the diffusion performance of lithium ions, and the electronic conductivity. The main types of binders reported in sulfur-lithium batteries are polyvinyl pyrrolidone, polyimide, polyethylene oxide, polyvinylidene fluoride, carboxymethyl cellulose, etc. For example, in "Aqueous Binders for Lithium-Sulfur Secondary Batteries" (Yao Zhendong, Shanghai Jiaotong University, published in 2012), the effects of polyethylene oxide (PEO) and gelatin as binders on the performance of sulfur-based positive electrode materials were compared. The battery with PEO as the binder had a first discharge specific capacity of 996 mAh / g, and after 50 cycles, the reversible specific capacity was only about 300 mAh / g, and obvious agglomeration occurred.

[0004] Therefore, the present invention comprehensively considers the problems of the electrode structure cracking caused by the volume change caused by the electrochemical process in the positive electrode of the lithium-sulfur battery, the poor cycle stability of the lithium-sulfur battery caused by the dissolution and shuttle effect of polysulfides, and the reduced rate performance caused by the poor conductivity of sulfur, Li2S2 and Li2S, and adopts PEO with hydrogen bond interaction to improve the bonding effect of the binder, adopts sodium carboxymethyl starch (CMS-Na) that can esterify with the PEO chain and has a surface film-forming effect to inhibit the shuttle of polysulfides, and adopts PSSA-Li with good ionic conductivity to reduce the impedance of the positive electrode, and obtains a composite binder with comprehensive excellent characteristics in three aspects: mechanical stability, sulfur fixation characteristics and conductivity. For example, poly (4-styrene sulfonic acid) lithium salt (PSSA-Li) is used as a binder. Although it has the advantages of good ionic conductivity and low impedance, the electrode obtained by using PSSA-Li alone as a binder is prone to structural cracking and brittle fracture.

[0005] Therefore, the present invention comprehensively considers the problems in the positive electrode of the lithium-sulfur battery, such as the rupture of the pole piece structure caused by the volume change caused by the electrochemical process, the poor cycle stability of the lithium-sulfur battery caused by the dissolution and shuttle effect of polysulfides, and the reduced rate performance caused by the poor conductivity of sulfur, Li2S2 and Li2S. It is of great significance to the development of lithium-sulfur batteries to study a binder with good mechanical stability, sulfur-fixing properties and conductivity. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention provides a binder for preparing positive electrode slurry of lithium-sulfur soft-pack batteries.

[0007] This is achieved specifically through the following technical solutions:

[0008] A binder for preparing positive electrode slurry of lithium-sulfur soft-pack batteries is prepared from polyethylene oxide (PEO), sodium carboxymethyl starch (CMS-Na) and poly (4-styrene sulfonic acid) lithium salt (PSSA-Li) in a mass ratio of (1-4): (0.8-1.6): (0.2-0.4).

[0009] The method for using the binder to prepare positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps:

[0010] 1) PEO and CMS-Na are dissolved in a dispersion medium and heated and stirred. After the heating and stirring are completed, the temperature is cooled to room temperature, and then PSSA-Li is added and stirred evenly to obtain a binder solution;

[0011] 2) The conductive agent and sulfur-carbon material are evenly stirred into the binder solution to obtain the positive electrode slurry.

[0012] The dispersion medium is water.

[0013] The heating and stirring is performed at a temperature of 90-100° C. and for a time of 12-24 hours.

[0014] The mass concentration of the binder in the dispersion medium is 0.5-20%.

[0015] The conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, and graphene.

[0016] The mass ratio of S / C in the sulfur-carbon material is 3.5:1 to 4:1.

[0017] The mass ratio of the sulfur-carbon material, the conductive agent and the binder in the positive electrode slurry of the lithium-sulfur soft-pack battery is (70-80):(10-20):(10-20).

[0018] Beneficial effects:

[0019] The adhesive of the present invention has the following excellent properties:

[0020] 1) Good bonding performance: The present invention improves the bonding effect of the adhesive by introducing PEO, which has hydrogen bond interaction and can form a hydrogen bond cross-linking network, into the adhesive system.

[0021] 2) Good sulfur fixation performance: The present invention introduces CMS-Na with good solubility and good film-forming properties, which greatly improves the sulfur fixation effect of the positive electrode plate.

[0022] 3) Excellent structural stability: The present invention strengthens the cross-linking effect of the PEO binder through the esterification of CMS-Na with the terminal hydroxyl groups of the PEO chain, thereby improving the structural stability of the PEO-based binder.

[0023] 4) Good conductivity: The cross-linking of the carboxyl groups on the surface of CMS-Na and the hydroxyl groups of PEO in the present invention can effectively reduce the crystallinity of PEO and improve the ionic conductivity of the PEO-based binder. The introduction of PSSA-Li with good ionic conductivity reduces the impedance of the positive electrode sheet, improves the ionic conductivity of the positive electrode and the interface contact between the electrolyte and the positive electrode. The anionic PSSA-Li can selectively promote lithium ion conduction while inhibiting the diffusion of polysulfide anions into the electrolyte.

[0024] Therefore, the present invention utilizes a binder with good bonding properties, sulfur-fixing properties, structural stability and conductivity for the preparation of the positive electrode slurry for the sulfur-lithium battery, which can prevent the cracking and brittle fracture of the pole piece structure, ensure ion transmission and electron transmission, and greatly improve the cycle performance and rate performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a rate performance curve diagram of the lithium-sulfur soft-pack battery 1;

[0026] Figure 2 It is a rate performance curve diagram of lithium-sulfur soft pack battery 2;

[0027] Figure 3 It is a rate performance curve diagram of lithium-sulfur soft pack battery 3;

[0028] Figure 4 This is the cycle performance diagram of lithium-sulfur soft-pack batteries 1, 2, and 3 at 0.05C. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention.

[0030] Example 1

[0031] A method for applying a binder in preparing positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps:

[0032] (1) PEO and CMS-Na were dissolved in water and heated and stirred at 95° C. for 12 h. After the temperature was lowered to room temperature, PSSA-Li was added and stirred evenly to prepare a binder solution with a concentration of 4.7%, wherein the mass ratio of PEO, CMS-Na and PSSA-Li was 4:1:0.3;

[0033] (2) Adding sulfur-carbon material and carbon nanotubes with a S / C mass ratio of 4:1 to a binder solution with a mass concentration of 4.7% and stirring evenly to obtain a positive electrode slurry; wherein the mass ratio of sulfur-carbon material, carbon nanotubes and binder is 7:2:1.

[0034] The positive electrode slurry prepared in this embodiment was coated on a carbon-coated aluminum foil to prepare the positive electrode of a lithium-sulfur battery, and a lithium ribbon was used as the counter electrode to assemble a soft-pack battery 1 ( Figure 1 and Figure 4 ). The charge and discharge test was carried out at a temperature of 25°C, a voltage range of 1.7 to 2.8V, and a current density of 0.01C. The soft pack battery capacity was 7.95Ah and the lithium-sulfur battery energy density was 413Wh / kg. The discharge capacity of the lithium-sulfur battery at 0.05C was 6.54Ah. After 50 cycles, the discharge capacity was 3.67Ah, and the capacity retention rate was 56.1%.

[0035] At the same time, we used PSSA-Li as a binder to make soft pack battery 2, and PEO / CMS-Na as a binder to make soft pack battery 3. The results are as follows Figure 2-4 ,according to Figure 2-4It can be seen that: under the condition of current density of 0.01C, the capacity of soft-pack battery 2 is 7.62Ah, and the energy density of lithium-sulfur battery is 406Wh / kg; the discharge capacity of lithium-sulfur battery at 0.05C is 6.39Ah, and after 50 cycles, the discharge capacity is 3.01Ah, and the capacity retention rate is 47.1%. Under the condition of current density of 0.01C, the capacity of soft-pack battery 3 is 6.48Ah, and the energy density of lithium-sulfur battery is 373Wh / kg; the discharge capacity of lithium-sulfur battery at 0.05C is 5.36Ah, and after 50 cycles, the discharge capacity is 2.01Ah, and the capacity retention rate is 37.5%.

[0036] Example 2

[0037] A method for applying a binder in preparing positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps:

[0038] (1) PEO and CMS-Na were dissolved in water and heated and stirred at 90° C. for 15 h. After the temperature was cooled to room temperature, PSSA-Li was added and stirred evenly to prepare a binder solution with a concentration of 1%, wherein the mass ratio of PEO, CMS-Na and PSSA-Li was 2:1:0.25;

[0039] (2) Add sulfur-carbon material and conductive carbon black with a S / C mass ratio of 3.5:1 to a binder solution with a mass concentration of 1%, and stir evenly to obtain a positive electrode slurry; wherein the mass ratio of sulfur-carbon material, conductive carbon black and binder is 7:1.5:1.5.

[0040] Example 3

[0041] A method for applying a binder in preparing positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps:

[0042] (1) PEO and CMS-Na were dissolved in water, and heated and stirred at 100° C. for 24 h. After the heating and stirring were completed, the mixture was cooled to room temperature, and PSSA-Li was added and stirred evenly to prepare a binder solution with a concentration of 15.2%, wherein the mass ratio of PEO, CMS-Na and PSSA-Li was 10:8:1;

[0043] (2) Adding sulfur-carbon material and conductive graphite with a S / C mass ratio of 4:1 to a binder solution with a mass concentration of 15.2% and stirring evenly to obtain a positive electrode slurry; wherein the mass ratio of the sulfur-carbon material, the conductive graphite and the binder is 8:1:1.

[0044] Example 4

[0045] A method for applying a binder in preparing positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps:

[0046] (1) PEO and CMS-Na were dissolved in water and heated and stirred at 93°C for 17 h. After the temperature was lowered to room temperature, PSSA-Li was added and stirred evenly to prepare a binder solution with a concentration of 10%, wherein the mass ratio of PEO, CMS-Na and PSSA-Li was 10:8:1;

[0047] (2) Adding sulfur-carbon material and conductive graphite with a S / C mass ratio of 4:1 to a binder solution with a mass concentration of 10% and stirring evenly to obtain a positive electrode slurry; wherein the mass ratio of sulfur-carbon material, conductive graphite and binder is 39:6:5.

[0048] At the same time, the positive electrode slurry of Example 2-4 was coated on a carbon-coated aluminum foil to prepare a positive electrode of a lithium-sulfur battery, and a lithium ribbon was used as a counter electrode to assemble a soft-pack battery. The charge and discharge test was carried out under the conditions of a temperature of 25°C, a voltage range of 1.7 to 2.8V, and a current density of 0.05C. After 50 cycles, the capacity retention rate was in the range of 55-58%.

Claims

1. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries, characterized in that: The binder is made of PEO, CMS-Na and PSSA-Li in a mass ratio of (1-4):(0.8-1.6):(0.2-0.4); The method for using the binder to prepare positive electrode slurry for lithium-sulfur soft-pack batteries comprises the following steps: 1) PEO and CMS-Na are dissolved in a dispersion medium and heated and stirred. After the heating and stirring are completed, the temperature is cooled to room temperature, and then PSSA-Li is added and stirred evenly to obtain a binder solution; 2) The conductive agent and sulfur-carbon material are evenly stirred into the binder solution to obtain the positive electrode slurry.

2. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The dispersion medium is water.

3. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The heating and stirring is performed at a temperature of 90-100° C. and for a time of 12-24 hours.

4. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The mass concentration of the binder in the dispersion medium is 0.5-20%.

5. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, and graphene.

6. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The mass ratio of S / C in the sulfur-carbon material is 3.5:1 to 4:

1.

7. A binder for preparing positive electrode slurry for lithium-sulfur soft-pack batteries according to claim 1, characterized in that: The mass ratio of the sulfur-carbon material, the conductive agent and the binder in the positive electrode slurry of the lithium-sulfur soft-pack battery is (70-80):(10-20):(10-20).

Citation Information

Patent Citations

  • Multifunctional self-repairing adhesive for lithium-sulfur battery positive electrode, preparation method and application thereof

    CN112652773A

  • Lithium-sulfur battery cathode material and preparation method thereof

    CN108232176A

  • Alkali metal-sulfur secondary battery

    JP2013225497A

  • Lithium-sulfur battery with high energy density

    KR1020160057006A