A method for preparing spherical gold nanorod self-assembled super particles

Spherical gold nanorod superparticles are prepared through seed method and multi-step coating technology, which solves the problem of insufficient application capabilities of nanogold in surface-enhanced Raman scattering and up-conversion particle luminescence effects, and achieves simple operation, high repeatability and stability. Strong self-assembly process, suitable for a variety of nanoscale samples.

CN114309580BActive Publication Date: 2024-10-22HANGZHOU DIANZI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111654775.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-10-22
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

It is difficult to effectively improve the application capabilities of gold nanoparticles in surface-enhanced Raman scattering and upconversion particle luminescence with existing technology, and there are few preparation methods with complex self-assembly processes and high requirements for repeatability and stability.

Method used

The seed method is used to prepare the gold nanorod dispersion, and through multi-step coating with silica and surface modification, combined with ultrasonic emulsification technology, the preparation of self-assembled super particles of spherical gold nanorods is achieved, which is simple to operate, highly reproducible, and has a wide range of applications. , high yield.

Benefits of technology

Achieved efficient preparation of spherical gold nanorod self-assembled super particles, with strong physical and chemical stability, wide application range, and high yield. Compared with traditional methods, the stability and accuracy requirements of the synthesis environment are lower, and it is suitable for a variety of nanometer scales. Sample self-assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114309580B_ABST
    Figure CN114309580B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing spherical gold nanorod self-assembled super particles. After coating a mesoporous silica layer, the sample is subjected to lipophilic surface modification. After the surface modification, the gold nanorods can be dissolved in an oily solvent, such as cyclohexane and chloroform. After the gold nanorods are dispersed in the oily solvent, SDS, dextran, water and cyclohexane are used to prepare an oil-in-water emulsion. The solution is emulsified by ultrasound. At this time, the oily substance is emulsified into micron-level droplets in the solution. Finally, the solution is evaporated to dry the volatile oily solution. The gold nanorods gradually become compact during the evaporation of the oily droplets, and finally shrink into a sphere and self-assemble into super particles. The invention has simple operation method, high repeatability, low requirements on the stability and accuracy of the synthesis environment, and high yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of photon nanocrystal materials, in particular to a method for preparing spherical gold nanorod self-assembled super particles. Background Art

[0002] Self-assembly of nanomaterials is a method to drive individual nanoparticles / nanomolecules to come together in an ordered manner and structure. It has great potential in developing new functions and properties of existing nanomaterials. Controllable manipulation of nanostructures (including DNA, proteins and superlattices) gives them unique optical, sensing and magnetic properties.

[0003] For gold nanoparticles, many strategies have been used to obtain different self-assembled structures, such as polymer-terminated nanochains, nanorafts, nanospheres, macroscopic nanofilms, nanocomposite constructs, and so on.

[0004] The spatial organization of inorganic nanoparticles into layered and ordered superstructures is crucial for the manufacture of functional materials and devices, which originates from the strong interaction between adjacent nanoparticles. Based on the surface plasmon resonance effect of gold, theoretical calculations show that the distance between gold nanoparticles affects the electric field intensity generated by mutual coupling. Under a certain coupling distance, mutual enhancement can be achieved. The electric field intensity under large-scale self-assembly is greatly improved. Its sub-wavelength electric field intensity enhancement has outstanding performance in application fields such as surface enhanced Raman scattering and upconversion particle luminescence. Summary of the invention

[0005] The present invention aims to improve the application capability of nano-gold in surface enhanced Raman scattering, up-conversion particle luminescence and other effects, and provides a preparation method of spherical gold nano-rod self-assembled super particles with simple operation method, high repeatability, low requirements on the stability and accuracy of the synthesis environment and high yield.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: 1. A method for preparing spherical gold nanorod self-assembled super particles, comprising the following steps:

[0007] (1) Preparing gold nanorod dispersion by seed method;

[0008] (2) After the gold nanorod dispersion is centrifuged, the centrifuge is dispersed in a 1-2 mM CTAB solution, and a NaOH solution is added to adjust the pH to 11. The TEOS methanol solution is added in multiple times under stirring. After the last addition of the TEOS methanol solution, stirring is continued for at least 24 hours to obtain a gold nanorod dispersion coated with silica.

[0009] (3) After centrifuging the gold nanorod dispersion coated with silica, take the washed centrifuge, add 32% ammonia water to the centrifuge, add OTMS chloroform solution, stir for at least 24 hours, centrifuge, wash the centrifuge with ethanol, and disperse it in an appropriate amount of chloroform to obtain a chloroform dispersion of gold nanorods coated with silica.

[0010] (4) Centrifuging the chloroform dispersion of gold nanorods coated with silica, dispersing the centrifuged product in cyclohexane to obtain a cyclohexane dispersion of gold nanorods coated with silica; adding purified water, dextran and SDS, mixing evenly, and ultrasonically dispersing to obtain a milky white emulsion.

[0011] (5) The emulsion is heated in a water bath, and after the color of the emulsion changes from milky white to reddish brown, it is added to a centrifuge tube, centrifuged, the supernatant is removed, and the centrifuge is dispersed in water to obtain a spherical gold nanorod self-assembled super particle dispersion. In the present invention, after the mesoporous silica layer is coated, the sample is subjected to lipophilic surface modification. After the surface modification, the gold nanorods can be dissolved in an oily solvent, such as cyclohexane and chloroform. After the gold nanorods are dispersed in the oily solvent, SDS, dextran, water, and cyclohexane are used to prepare an oil-in-water emulsion, and the solution is emulsified by ultrasound. At this time, the oily substance is emulsified into small droplets of micrometer level in the solution. Finally, the solution is evaporated to dry the volatile oily solution. The gold nanorods gradually become compact during the evaporation of the oily droplets, and finally shrink into a sphere and self-assemble into super particles.

[0012] Preferably, in step (1), the specific steps of preparing the gold nanorod dispersion by the seed method are: after mixing the CTAB solution and the HAuCl4 solution, adding the NaBH4 solution, stirring vigorously to obtain the seed solution; after dissolving the CTAB solution and NaOL in water, adding the AgNO3 solution, after standing, adding the HAuCl4 solution, stirring until the solution becomes colorless, to obtain the growth solution; after adjusting the pH of the growth solution to 1.3 with hydrochloric acid, adding the AA solution and the seed solution and stirring vigorously, after standing, to obtain the gold nanorod dispersion.

[0013] Preferably, 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution are mixed, and then 0.3 mL of 0.02 M NaBH4 solution is added, and the mixture is stirred vigorously to obtain a seed solution; 9.25 mL of 0.1 M CTAB solution and 0.062 g of NaOL are dissolved in 14.5 mL of water at 50°C, and the mixture is cooled to 30°C after dissolution, and then 1.2 mL of 4 mM AgNO3 solution is added, and the mixture is allowed to stand at a constant temperature of 30°C for 15 min, and then 0.25 mL of 10 mM HAuCl4 solution is added, and the mixture is stirred until the solution becomes colorless to obtain a growth solution; after adding hydrochloric acid to the growth solution to adjust the pH to 1.3, 75 μL of 64 mM AA solution and 40 μL of seed solution are added and stirred vigorously, and the mixture is allowed to stand at a constant temperature of 30°C for 12 h to obtain a gold nanorod dispersion.

[0014] Preferably, in step (2), the volume percentage of TEOS in the TEOS methanol solution is 20%, and 3% of the total solution volume of TEOS methanol solution is added. The TEOS methanol solution is added in six portions, and stirring is performed for at least 30 minutes after each addition of TEOS.

[0015] Preferably, in step (3), the OTMS chloroform solution has an OTMS content of 2.4% by mass, and the ratio of the volume of ammonia water added to the volume of the centrifuge is 1:30; the ratio of the volume of the OTMS chloroform solution added to the volume of the centrifuge is 1:6.

[0016] Preferably, in step (4), the mass ratio of purified water, dextran and SDS is 500:20:3, the volume ratio of the cyclohexane dispersion of gold nanorods coated with silica to purified water is 1:10, and the mass percentage of gold nanorods coated with silica in the cyclohexane dispersion of gold nanorods coated with silica is 0.17%.

[0017] Preferably, in step (5), the emulsion is evaporated in a water bath at 60° C. for 2 h.

[0018] Therefore, the present invention has the following beneficial effects:

[0019] (1) The operation method is simple and has high repeatability. The sample is coated with mesoporous silica and has strong physical and chemical stability. The reaction will basically not fail if it is carried out according to the steps. Compared with many preparation methods of self-assembled samples, the requirements for the stability and accuracy of the synthesis environment are much lower;

[0020] (2) It has a wide range of applications and can be extended to many nanoscale sample self-assemblies. It is less restricted by the concentration of raw materials and has strong stability.

[0021] (3) The yield is high, and most of the gold nanorods successfully self-assemble into spherical superparticles. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a transmission electron microscope image of the spherical gold nanorod superparticles in Example 1.

[0023] Figure 2 This is a transmission electron microscope image of the spherical gold nanorod superparticles in Example 2.

[0024] Figure 3 This is a transmission electron microscope image of the spherical gold nanorod superparticles in Example 3. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0026] Example 1

[0027] (1) Preparation of gold nanorod dispersion by seed method: 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution were mixed, and then 0.3 mL of 0.02 M NaBH4 solution was added and stirred vigorously to obtain a seed solution; 9.25 mL of 0.1 M CTAB solution and 0.062 g of NaOL were dissolved in 14.5 mL of water at 50°C, and the temperature was lowered to 30°C after dissolution, and then 1.2 mL of 4 mM AgNO3 solution was added, and the mixture was kept at a constant temperature of 30°C for 15 min, and then 0.25 mL of 10 mM HAuCl4 solution was added, and the mixture was stirred until the solution became colorless to obtain a growth solution; hydrochloric acid was added to the growth solution to adjust the pH to 1.3, and then 75 μL of 64 mM AA solution and 40 μL of seed solution were added and stirred vigorously, and the mixture was kept at a constant temperature of 30°C for 12 h to obtain a gold nanorod dispersion.

[0028] (2) After the gold nanorod dispersion is centrifuged, the centrifuge is dispersed in a 1 mM CTAB solution, and a NaOH solution is added to adjust the pH to 11. TEOS methanol solution is added in multiple times under stirring, and the volume percentage of TEOS in the TEOS methanol solution is 20%. 3% of the total solution volume of TEOS methanol solution is added, and the TEOS methanol solution is added in six times. After each addition of TEOS, stirring is continued for at least 30 minutes. After the last addition of TEOS methanol solution, stirring is continued for at least 24 hours to obtain a gold nanorod dispersion coated with silica.

[0029] (3) After centrifuging the gold nanorod dispersion coated with silica, take the washed centrifuge, add 32% ammonia water to the centrifuge, and then add OTMS chloroform solution, in which the OTMS mass percentage is 2.4%. Based on the volume of the centrifuge, the volume ratio of the added ammonia water to the volume of the centrifuge is 1:30; the volume ratio of the added OTMS chloroform solution to the volume of the centrifuge is 1:6. Stir for at least 24 hours, centrifuge, wash the centrifuge with ethanol, and disperse it in an appropriate amount of chloroform to obtain a chloroform dispersion of gold nanorods coated with silica.

[0030] (4) Centrifuging the chloroform dispersion of gold nanorods coated with silica, dispersing the centrifuge in cyclohexane to obtain a cyclohexane dispersion of gold nanorods coated with silica; adding purified water, dextran and SDS, mixing evenly, and ultrasonically dispersing to obtain a milky white emulsion, wherein the mass percentage of gold nanorods coated with silica in the cyclohexane dispersion of gold nanorods coated with silica is 0.17%, and the mass ratio of purified water, dextran and SDS is 500:20:3; the volume ratio of the cyclohexane dispersion of gold nanorods coated with silica to purified water is 1:10.

[0031] (5) The emulsion was heated in a 60° C. water bath for 2 h. After the color of the emulsion changed from milky white to reddish brown, it was added to a centrifuge tube and centrifuged. The supernatant was removed and the centrifuge was dispersed in water to obtain a dispersion of spherical gold nanorod self-assembled super particles.

[0032] After cleaning, the spherical gold nanorod self-assembled super particles in this embodiment have a transmission electron microscope image as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the size range of the synthesized spherical gold nanorod self-assembled super particles is 200-400nm, the sample is relatively clean, there is no breakage under centrifugation at 500rpm and multiple washings, the structure is stable, and the washing process of this method is to centrifuge and wash all the post-reaction solutions. The vast majority of the electron microscope images obtained are spherical gold nanorod super particles, and there are few unassembled gold nanorods. It can be seen that the conversion rate is very high.

[0033] Example 2

[0034] Compared with Example 1, the present embodiment is different in that: in step (4), the mass percentage (concentration) of the gold nanorods coated with silicon dioxide in the cyclohexane dispersion of gold nanorods coated with silicon dioxide is doubled, and the rest is exactly the same as Example 1.

[0035] After cleaning, the spherical gold nanorod self-assembled super particles in this embodiment have a transmission electron microscope image as shown in FIG. Figure 2 As shown. Figure 2It can be seen that the size of the synthesized spherical gold nanorod self-assembled superparticles is about 400-600nm. Compared with Example 1, the concentration of gold nanorods is higher, which is reflected in the thicker thickness of the balls in the figure. By observing the transparency of the center of the balls, it can be seen that when the concentration of gold nanorods coated with silica is doubled, the solidity of the self-assembled spherical superparticles increases, the stacking is more dense, and the internal space is fully compressed. Even when the concentration of gold nanorods is high, it also has very high stability, the structure is not broken, and the conversion rate is also very high, which reflects the stability of this method under high concentrations of gold nanorods.

[0036] Example 3

[0037] Compared with Example 1, the present embodiment is different in that: in step (4), the mass percentage (concentration) of the gold nanorods coated with silicon dioxide in the cyclohexane dispersion of gold nanorods coated with silicon dioxide is reduced by one third, and the rest is exactly the same as Example 1.

[0038] After cleaning, the spherical gold nanorod self-assembled super particles in this embodiment have a transmission electron microscope image as shown in FIG. Figure 3 As shown. Figure 3 It can be seen that after reducing the concentration of gold nanorods, the superparticles obtained have more internal space, which is reflected in the higher degree of transparency and looser structure in the transmission electron microscope image, but the self-assembly structure of spherical superparticles and high conversion rate are also retained. This shows that in addition to maintaining the stability of the assembly at high gold nanorod concentrations, this method can also maintain its stability at low gold nanorod concentrations, is not limited by the harsh specific gold nanorod concentration, and has high universality.

[0039] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A method for preparing spherical gold nanorod self-assembled super particles, characterized in that: The following steps are involved: (1) Preparing gold nanorod dispersion by seed method; (2) After the gold nanorod dispersion is centrifuged, the centrifuge is dispersed in a 1-2 mM CTAB solution, a NaOH solution is added to adjust the pH to 11, and a TEOS methanol solution is added in multiple times under stirring. After the last addition of the TEOS methanol solution, stirring is continued for at least 24 hours to obtain a gold nanorod dispersion coated with silica; (3) After centrifuging the gold nanorod dispersion coated with silica, the washed centrifuge was taken, 32% ammonia water was added to the centrifuge, and then a chloroform solution of OTMS was added, and the mixture was stirred for at least 24 hours and centrifuged. The centrifuge was washed with ethanol and dispersed in an appropriate amount of chloroform to obtain a chloroform dispersion of gold nanorods coated with silica; (4) centrifuging the chloroform dispersion of gold nanorods coated with silica, dispersing the centrifuged product in cyclohexane to obtain a cyclohexane dispersion of gold nanorods coated with silica; adding purified water, dextran and SDS, mixing evenly, and ultrasonically dispersing to obtain a milky white emulsion; (5) heating the emulsion in a water bath until the color of the emulsion changes from milky white to reddish brown, adding the emulsion to a centrifuge tube, centrifuging, removing the supernatant, and dispersing the centrifuged product in water to obtain a dispersion of spherical gold nanorod self-assembled super particles; In the step (1), the specific steps of preparing the gold nanorod dispersion by the seed method are: after mixing 10 mL of 0.1 M CTAB solution and 0.25 mL of 10 mM HAuCl4 solution, adding 0.3 mL of 0.02 M NaBH4 solution, stirring vigorously, to obtain a seed solution; 9.25 mL of 0.1 M CTAB solution and 0.062 g of NaOL were dissolved in 14.5 mL of water at 50°C, cooled to 30°C after dissolution, and then 1.2 mL of 4 mM AgNO3 solution was added, and the mixture was kept at 30°C for 15 min. Then 0.25 mL of 10 mM HAuCl4 solution was added and stirred until the solution became colorless to obtain a growth solution. After adding hydrochloric acid to the growth solution to adjust the pH to 1.3, 75 μL of 64 mM AA solution and 40 μL of seed solution were added and stirred vigorously, and the mixture was kept at 30°C for 12 h to obtain a gold nanorod dispersion.

2. The method for preparing spherical gold nanorod self-assembled super particles according to claim 1, characterized in that: In step (2), the volume percentage of TEOS in the TEOS methanol solution is 20%, and 3% of the total solution volume of TEOS methanol solution is added. The TEOS methanol solution is added in six portions, and stirring is performed for at least 30 minutes after each addition of TEOS.

3. The method for preparing spherical gold nanorod self-assembled super particles according to claim 1, characterized in that: In step (3), the OTMS chloroform solution has an OTMS content of 2.4% by mass. Based on the volume of the centrifuge, the ratio of the volume of the added ammonia water to the volume of the centrifuge is 1:30; and the ratio of the volume of the added OTMS chloroform solution to the volume of the centrifuge is 1:

6.

4. The method for preparing spherical gold nanorod self-assembled super particles according to claim 1, characterized in that: In step (4), the mass ratio of purified water, dextran and SDS is 500:20:3, and the volume ratio of the cyclohexane dispersion of gold nanorods coated with silica to purified water is 1:10; the mass percentage of gold nanorods coated with silica in the cyclohexane dispersion of gold nanorods coated with silica is 0.17%.

5. The method for preparing spherical gold nanorod self-assembled super particles according to claim 1, characterized in that: In step (5), the emulsion is evaporated in a water bath at 60° C. for 2 h.