A fuel cell membrane electrode and a preparation method thereof and a fuel cell

The fuel cell membrane electrode is directly compounded and prepared through a multi-layer melt co-extrusion method, which solves the problems of excessive use of organic solvents and defects between the catalyst layer and the proton exchange membrane in wet preparation, achieving efficient and environmentally friendly membrane electrode preparation, and improving improve the performance and production efficiency of membrane electrodes.

CN114335565BActive Publication Date: 2024-10-29STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111413302.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-25
Publication Date
2024-10-29
Estimated Expiration
2041-11-25

AI Technical Summary

Technical Problem

The existing wet preparation method of fuel cell membrane electrodes requires a large amount of organic solvents, which leads to environmental pollution, and there are defects and gaps between the cathode and anode catalyst layers and the proton exchange membrane, which affects the mass transfer effect and consistency of the membrane electrodes.

Method used

The multi-layer melt co-extrusion method is used to directly compound the proton exchange membrane material, cathode catalyst layer material and anode catalyst layer material to prepare the membrane electrode, avoiding the use of organic solvents, simplifying the process flow, and reducing defects and defects between the catalyst layer and the proton exchange membrane. gap.

Benefits of technology

It improves the preparation efficiency and performance of the membrane electrode, reduces the use of solvents, reduces the production cost, realizes a green and environmentally friendly process, and significantly improves the mass transfer effect and consistency of the membrane electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114335565B_ABST
    Figure CN114335565B_ABST
Patent Text Reader

Abstract

The present invention discloses a fuel cell membrane electrode and a preparation method thereof, comprising preparing a membrane electrode by compounding a proton exchange membrane material, a cathode catalyst layer material and an anode catalyst layer material of the membrane electrode through multi-layer melt co-extrusion. The preparation method of the anode catalyst layer material or the cathode catalyst layer material comprises uniformly mixing the anode catalyst or the cathode catalyst with a proton conductive polymer under an inert atmosphere, without adding an organic solvent during the mixing process, to obtain the anode catalyst layer material or the cathode catalyst layer material. The preparation method of the fuel cell membrane electrode of the present invention does not require the use of an organic solvent, the preparation method is simple, the production efficiency is improved, and the defects and gaps between the catalyst layer and the proton exchange membrane in the membrane electrode are reduced, effectively improving the mass transfer effect and consistency of the membrane electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a fuel cell membrane electrode and a preparation method thereof, and further relates to a fuel cell. Background Art

[0002] As an efficient, environmentally friendly and sustainable energy utilization device, fuel cells are being increasingly used in various fields such as transportation, power generation and energy storage. The membrane electrode is the core component of the fuel cell. The cathode and cathode catalyst layers and proton exchange membrane of the membrane electrode are the places where the electrochemical reaction of the fuel cell occurs and the proton transfer occurs, which is crucial to the performance of the fuel cell. At present, the cathode and cathode catalyst layers and proton exchange membrane of the membrane electrode are mainly prepared by wet method, that is, the proton exchange membrane resin is first dissolved and dispersed in the solvent, and then prepared into a solid proton exchange membrane; then the cathode and cathode catalyst materials are mixed in a specific solvent to prepare a slurry, and then the cathode and cathode catalyst layers are prepared on both sides of the proton exchange membrane by transfer printing or spraying.

[0003] Since the wet method of preparing membrane electrodes requires the use of a large amount of organic solvents, which is harmful to the human body and the environment and is not conducive to environmental protection, it is necessary to improve the existing membrane electrode preparation method. Summary of the invention

[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: when the membrane electrode is prepared by the wet method, the proton exchange membrane and the cathode catalyst layer are made separately, which involves many processes, is not conducive to improving the preparation efficiency of the membrane electrode, and requires the use of a large amount of organic solvents, causing environmental pollution. Moreover, since the functional layer is prepared separately, there are usually various defects and gaps in the contact interface between the catalyst layer and the proton exchange membrane, which affects the mass transfer effect and consistency of the membrane electrode.

[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, an embodiment of the present invention provides a method for preparing a fuel cell membrane electrode, which does not require the use of an organic solvent, is simple in preparation, improves production efficiency, and reduces defects and gaps between the catalyst layer and the proton exchange membrane in the membrane electrode, effectively improving the mass transfer effect and consistency of the membrane electrode.

[0006] The method for preparing a fuel cell membrane electrode according to an embodiment of the present invention comprises compounding a proton exchange membrane material, a cathode catalyst layer material and an anode catalyst layer material of the membrane electrode by multi-layer melt co-extrusion to prepare the membrane electrode.

[0007] The advantages and technical effects brought by the preparation method of the fuel cell membrane electrode of the embodiment of the present invention are as follows: 1. In the method of the embodiment of the present invention, the proton exchange membrane material, the cathode catalyst layer material and the anode catalyst layer material are directly melt-coextruded to prepare the membrane electrode, without the need to prepare the functional layers separately. The preparation method is simple and the production efficiency is improved; 2. In the method of the embodiment of the present invention, there is no need to add organic solvents, which not only reduces the use of solvents and saves production costs, but also is green and environmentally friendly and easy to promote and apply; 3. In the method of the embodiment of the present invention, the simultaneous preparation of the anode and cathode catalyst layers and the proton exchange membrane is achieved, which effectively reduces the defects and gaps between the catalyst layer and the proton exchange membrane and improves the performance of the membrane electrode.

[0008] In some embodiments, the method for preparing the anode catalyst layer material or the cathode catalyst layer material comprises uniformly mixing the anode catalyst or the cathode catalyst with a proton conductive polymer under an inert atmosphere to obtain the anode catalyst layer material or the cathode catalyst layer material.

[0009] In some embodiments, no organic solvent is added during the mixing of the anode catalyst or cathode catalyst and the proton conducting polymer.

[0010] In some embodiments, the anode catalyst or cathode catalyst includes a platinum-containing catalyst or a non-platinum catalyst for a membrane electrode; and the proton-conducting polymer is a perfluorosulfonic acid polymer.

[0011] In some embodiments, the proton-conducting polymer is heated and dried to obtain a proton exchange membrane material.

[0012] In some embodiments, the heating temperature is 60-100° C., and the heating time is 1-24 h.

[0013] In some embodiments, the proton conductive polymer includes at least one of a perfluorosulfonic acid polymer, a partially fluorinated sulfonated polymer, and a non-fluorinated sulfonated polymer, and the proton exchange equivalent EW value thereof is 700-1200.

[0014] In some embodiments, the melting heating temperature of the cathode catalyst layer material and the anode catalyst layer material is 100-200°C.

[0015] In some embodiments, the die temperature of the multi-layer melt co-extrusion is 150-250°C.

[0016] The present invention also provides a membrane electrode, which is prepared by the method of the present invention. The membrane electrode of the present invention has a simple preparation method, does not require the use of organic solvents, has few defects and gaps between the catalyst layer and the proton exchange membrane, and has excellent performance.

[0017] The embodiment of the present invention further provides a fuel cell, comprising the membrane electrode of the embodiment of the present invention. The fuel cell of the embodiment of the present invention has all the advantages that the membrane electrode of the embodiment of the present invention can bring, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the structure of the membrane electrode prepared in an embodiment of the present invention.

[0019] Figure 2 This is a scanning electron microscope cross-sectional image of the membrane electrode prepared in Example 1.

[0020] Figure 3 This is a scanning electron microscope cross-sectional view of the membrane electrode prepared in Comparative Example 1. DETAILED DESCRIPTION

[0021] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0022] The method for preparing a fuel cell membrane electrode according to an embodiment of the present invention comprises compounding a proton exchange membrane material, a cathode catalyst layer material and an anode catalyst layer material of the membrane electrode by multi-layer melt co-extrusion to prepare the membrane electrode.

[0023] In the method for preparing the fuel cell membrane electrode of the embodiment of the present invention, the proton exchange membrane material, the cathode catalyst layer material and the anode catalyst layer material are directly melt-coextruded to prepare the membrane electrode, without the need to prepare the functional layers separately, the preparation method is simple, and the production efficiency is improved; in the method of the embodiment of the present invention, there is no need to add organic solvents, which not only reduces the use of solvents and saves production costs, but also is green and environmentally friendly and easy to promote and apply; in the method of the embodiment of the present invention, the simultaneous preparation of the anode and cathode catalyst layers and the proton exchange membrane is achieved, which effectively reduces the defects and gaps between the catalyst layer and the proton exchange membrane, and improves the performance of the membrane electrode.

[0024] In some embodiments, the preparation method of the anode catalyst layer material or the cathode catalyst layer material comprises uniformly mixing the anode catalyst or the cathode catalyst with a proton conductive polymer under an inert atmosphere, preferably by grinding or, ball milling or mixing, to obtain the anode catalyst layer material or the cathode catalyst layer material. Preferably, no organic solvent is added during the mixing of the anode catalyst or the cathode catalyst with the proton conductive polymer. Preferably, the inert gas comprises at least one of argon or nitrogen. In the method of the embodiment of the present invention, there is no need to use a large amount of organic solvent to prepare the anode catalyst layer slurry and the cathode catalyst layer slurry separately. It is only necessary to uniformly mix the anode catalyst or the cathode catalyst with the proton conductive polymer to form the anode catalyst layer material or the cathode catalyst layer material, and then form a membrane electrode by multi-layer melt co-extrusion with the proton exchange membrane material. The preparation method is simple, environmentally friendly and pollution-free, and easy for industrial application.

[0025] In some embodiments, the anode catalyst or cathode catalyst includes a platinum-containing catalyst or a non-platinum catalyst for a membrane electrode; the proton-conducting polymer is a perfluorosulfonic acid polymer. In the embodiments of the present invention, there is no particular restriction on the catalyst used in the anode catalyst layer material or the cathode catalyst layer material, as long as the catalyst can be used for a fuel cell membrane electrode, and there is no particular restriction on the amount ratio between the catalyst and the proton-conducting polymer, which can be designed according to the requirements of the fuel cell membrane electrode.

[0026] In some embodiments, the proton exchange membrane material is a proton conductive polymer, which can be pretreated according to the specific conditions of the proton conductive polymer. Preferably, the proton conductive polymer is heated and dried to obtain the proton exchange membrane material. Preferably, the heating temperature is 60-100°C and the heating time is 1-24h. Further preferably, the proton conductive polymer includes at least one of a perfluorosulfonic acid polymer, a partially fluorinated sulfonated polymer, and a non-fluorinated sulfonated polymer, and its proton exchange equivalent EW value is 700-1200. In the method of the embodiment of the present invention, it is not necessary to disperse the proton conductive polymer in an organic solvent to prepare a solid proton exchange membrane. The lack of an organic solvent not only reduces the production cost, but is also green and environmentally friendly. In addition, the proton exchange membrane and the anode and cathode catalyst layers are formed simultaneously by a multi-layer melt co-extrusion method, which significantly reduces the interface defects of the membrane electrode and improves the performance of the membrane electrode.

[0027] In some embodiments, the melting heating temperature of the cathode catalyst layer material and the anode catalyst layer material is 100-200° C. Preferably, the die temperature of the multi-layer melt co-extrusion is 150-250° C. In the method of the embodiment of the present invention, there is no particular restriction on the melting heating temperature of the cathode catalyst layer material, the anode catalyst layer material, and the proton exchange membrane material, as long as the melting heating temperature is not lower than the melting temperature of each material and not higher than the decomposition temperature of each material.

[0028] The present invention also provides a membrane electrode, which is prepared by the method of the present invention. The membrane electrode of the present invention has a simple preparation method, does not require the use of organic solvents, has few defects and gaps between the catalyst layer and the proton exchange membrane, and has excellent performance.

[0029] The embodiment of the present invention further provides a fuel cell, comprising the membrane electrode of the embodiment of the present invention. The fuel cell of the embodiment of the present invention has all the advantages that the membrane electrode of the embodiment of the present invention can bring, which will not be described in detail here.

[0030] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0031] Example 1

[0032] (1) To prepare the anode catalyst layer material, 100 g of a platinum carbon catalyst having a platinum content of 30% and 20 g of a perfluorosulfonic acid resin were taken and mixed thoroughly in a ball mill under a nitrogen atmosphere.

[0033] (2) To prepare the cathode catalyst layer material, 100 g of a platinum carbon catalyst having a platinum content of 60% and 30 g of a perfluorosulfonic acid resin were taken and mixed thoroughly in a ball mill under a nitrogen atmosphere.

[0034] (3) To prepare a proton exchange membrane material, 200 g of perfluorosulfonic acid resin (EW value: 700) was heated at 100° C. for 1 h.

[0035] (4) Add the mixed cathode catalyst layer material, anode catalyst layer material and proton exchange membrane material into the material box of the multilayer melt co-extruder respectively, and heat the catalyst layer material and the proton exchange membrane material to melt them into a fluid state. The heating temperature of the cathode catalyst layer material is 100° C., the heating temperature of the anode catalyst layer material is 100° C., and the heating temperature of the proton exchange membrane material is 200° C.

[0036] (5) The molten cathode catalyst layer material, the anode catalyst layer material and the proton exchange membrane material are co-extruded through an extruder, the die temperature is 150° C., the cathode catalyst layer and the anode catalyst layer are respectively on both sides of the proton exchange membrane layer, and a fuel cell membrane electrode is obtained. The membrane electrode structure is as follows: Figure 1 shown.

[0037] The scanning electron microscope cross-sectional view of the membrane electrode prepared in this embodiment is shown in Figure 2 ,pass Figure 2 It can be seen that the catalyst layer and the proton conductive polymer layer of the membrane electrode prepared simultaneously by multi-layer melt co-extrusion in this embodiment are completely combined with less defects.

[0038] Example 2

[0039] (1) To prepare the anode catalyst layer material, 200 g of a platinum carbon catalyst having a platinum content of 20% and 50 g of a perfluorosulfonic acid resin were taken and mixed thoroughly in a mixer under an argon protective atmosphere.

[0040] (2) To prepare the cathode catalyst layer material, 200 g of a platinum carbon catalyst having a platinum content of 70% and 60 g of a perfluorosulfonic acid resin were taken and mixed thoroughly in a ball mill under an argon protective atmosphere.

[0041] (3) To prepare a proton exchange membrane material, 500 g of sulfonated polyetheretherketone (EW value: 1200, melting temperature: 334° C.) was heated at 60° C. for 24 h.

[0042] (4) Add the mixed cathode catalyst layer material, anode catalyst layer material and proton exchange membrane material into a material box of a multilayer melt co-extruder, respectively, and heat to melt the catalyst layer material and the proton exchange membrane material until they are in a fluid state. The heating and melting temperature of the cathode catalyst layer material is 200° C., the heating and melting temperature of the anode catalyst layer material is 200° C., and the heating and melting temperature of the proton exchange membrane material sulfonated polyetheretherketone is 350° C.

[0043] (5) The molten cathode catalyst layer material, the anode catalyst layer material and the proton exchange membrane material sulfonated polyetheretherketone are co-extruded through an extruder, the die temperature is 150° C., the cathode catalyst layer and the anode catalyst layer are respectively on both sides of the proton exchange membrane layer, and a fuel cell membrane electrode is obtained. The membrane electrode structure is as follows: Figure 1 shown.

[0044] Comparative Example 1

[0045] The method is the same as that of Example 1, except that in step (5), the proton exchange membrane material is first extruded separately, and after the proton exchange membrane is cooled and shaped, the cathode catalyst layer material and the anode catalyst layer material are sequentially extruded on both sides of the proton exchange membrane to obtain the cathode catalyst layer and the anode catalyst layer, respectively, to obtain a membrane electrode. The membrane electrode structure is as follows: Figure 1 shown.

[0046] The scanning electron microscope cross-sectional view of the membrane electrode prepared in Comparative Example 1 is shown in Figure 3 ,pass Figure 3 It can be seen that the catalyst layer and the proton exchange membrane in the membrane electrode of Comparative Example 1 are prepared separately, and there are obvious defects between the catalyst layer and the proton exchange membrane.

[0047] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" and the like mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory. Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and cannot be construed as limitations of the present invention, and those of ordinary skill in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a fuel cell membrane electrode, characterized in that: The invention comprises compounding the proton exchange membrane material, cathode catalyst layer material and anode catalyst layer material of the membrane electrode by multi-layer melt co-extrusion to obtain the membrane electrode, wherein: The preparation method of the anode catalyst layer material or cathode catalyst layer material comprises uniformly mixing the anode catalyst or cathode catalyst with a proton conductive polymer under an inert atmosphere to obtain the anode catalyst layer material or cathode catalyst layer material, wherein no organic solvent is added during the mixing process of the anode catalyst or cathode catalyst with the proton conductive polymer; The proton-conducting polymer is heated and dried to obtain a proton exchange membrane material.

2. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: The anode catalyst or cathode catalyst includes a platinum-containing catalyst or a non-platinum catalyst for a membrane electrode; and the proton-conducting polymer is a perfluorosulfonic acid polymer.

3. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: The heating temperature is 60-100° C., and the heating time is 1-24 hours.

4. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: The proton conductive polymer in the proton exchange membrane material comprises at least one of a perfluorosulfonic acid polymer, a partially fluorinated sulfonated polymer and a non-fluorinated sulfonated polymer, and the proton exchange equivalent EW value thereof is 700-1200.

5. The method for preparing a fuel cell membrane electrode according to claim 1, characterized in that: The melting heating temperature of the cathode catalyst layer material and the anode catalyst layer material is 100-200°C, and / or the die temperature of the multi-layer melt co-extrusion is 150-250°C.

6. A membrane electrode, characterized in that: The method according to any one of claims 1 to 5 is adopted.

7. A fuel cell, characterized in that: Comprising the membrane electrode as claimed in claim 6.

Citation Information

Patent Citations

  • Hot melt extruded solid state battery components

    CN111801838A

  • Packaging method and membrane electrode assembly

    CN112186216A

  • Preparation of three-in-one membrane electrode assembly

    CN1269428A

  • Method for measuring electrode films

    WO2019211278A1