A composite solid polymer electrolyte and preparation method thereof

By adding materials such as boron nitride nanopowder and g-C3N4 to the PEO solid electrolyte, a composite electrolyte membrane with a smooth surface and high mechanical strength is prepared, which solves the problems of low mechanical strength and insufficient conductivity of the electrolyte in the existing technology, and achieves Provides more stable and efficient lithium metal battery performance.

CN114373995BActive Publication Date: 2024-10-15HEBEI GELLEC NEW ENERGY MATERIAL SCI&TECHNOLOY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202111563740.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-10-15
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

In the existing technology, PEO solid electrolyte has low mechanical strength, poor surface flatness, low ionic conductivity, and harsh preparation conditions, which limits its application in lithium metal batteries.

Method used

A method for preparing a composite solid polymer electrolyte is used. The slurry is prepared by stirring the electrolyte lithium salt, boron nitride nanopowder, g-C3N4, PVDF and powder dispersant in an organic solvent, and coating it on a smooth and flat plate. Apply vacuum drying and clamp drying to obtain a composite solid electrolyte membrane with a smooth surface, which improves mechanical strength and conductivity.

Benefits of technology

It significantly improves the mechanical strength and conductivity of the electrolyte membrane, reduces surface roughness, simplifies the preparation process, is suitable for industrial production, and improves the cycle stability and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114373995B_ABST
    Figure CN114373995B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of a composite solid polymer electrolyte, which comprises: S1, dispersing electrolyte lithium salt in an organic solvent, stirring until completely dissolved, and obtaining an electrolyte solution; S2, adding boron nitride nanopowder, g-C3N4, PEO, PVDF and powder dispersant to the electrolyte solution in sequence while stirring, and stirring fully until a dark yellow slurry is obtained; S3, coating the slurry on a smooth and flat plate, vacuum drying, and obtaining a solid film on the plate; making the solid film detach from the plate and float by a water immersion method; S4, clamping the solid film between two smooth and flat plates, and drying, that is, obtaining a composite solid polymer electrolyte with a smooth surface. The present invention solves the technical problems of low mechanical strength, poor surface flatness, low ionic conductivity, and harsh preparation conditions of the PEO solid electrolyte prepared by the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid electrolytes, in particular to a composite solid polymer electrolyte and a preparation method thereof. Background Art

[0002] The development trend of energy storage systems is high energy density batteries. Using lithium metal as the anode of the battery can greatly improve the energy density of the battery. However, lithium metal batteries are prone to produce lithium dendrites during the cycle process, which may pierce the diaphragm and cause the battery to short-circuit and thus cause the battery to burn or explode, greatly limiting the practical application of lithium metal batteries. The application of solid electrolytes in lithium metal batteries can improve their safety, especially solid polymer electrolytes have attracted widespread attention due to their good flexibility, excellent processing performance, and low interface resistance with lithium metal anodes. In the prior art, all-solid-state polymer electrolyte batteries use polyethylene oxide as the polymer matrix, but the polyethylene oxide system has high crystallinity and low ionic conductivity at room temperature. The battery must be raised to a certain temperature before it can operate normally. However, as the temperature increases and gradually approaches the glass transition temperature of the polymer electrolyte, the mechanical strength of the electrolyte is greatly reduced, and it is difficult to inhibit the growth of lithium dendrites. Through research, it is found that improving the mechanical strength and interface stability of the polymer electrolyte can inhibit the growth of lithium dendrites, thereby improving the cycle stability of lithium metal batteries.

[0003] In order to improve the mechanical strength of polymer electrolytes, researchers have proposed a technology, that is, first preparing a polyethylene oxide polymer electrolyte, and then coating the boron nitride nanosheets prepared by the chemical stripping method onto the PEO polymer electrolyte membrane by hot pressing transfer. The boron nitride nanosheet coating layer can enhance the mechanical strength of the PEO polymer electrolyte surface, ensure that the interface between the electrolyte and the lithium metal remains stable, reduce the tip effect, make the lithium ion flow uniformly distributed, inhibit the growth of lithium dendrites, and improve the cycle stability and rate performance of the solid electrolyte. However, although this method improves the mechanical strength of the polymer electrolyte, the surface roughness of the prepared electrolyte is large, and this method is not only complex and unsuitable for industrial production, but also has no obvious improvement on the overall mechanical properties of the polymer electrolyte, which limits the practical application of the PEO polymer electrolyte. In addition, the prior art only focuses on improving the mechanical strength of the polymer electrolyte and inhibiting the growth of lithium dendrites, but has no effect on improving the lithium ion conductivity of the solid electrolyte, and its electrochemical performance is still unsatisfactory. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a composite solid polymer electrolyte and a preparation method thereof, which solves the technical problems of low mechanical strength, poor surface flatness, low ionic conductivity, and harsh preparation conditions of the PEO solid electrolyte prepared by the prior art.

[0006] (II) Technical solution

[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0008] In a first aspect, the present invention provides a method for preparing a composite solid polymer electrolyte, comprising:

[0009] S1. Dispersing electrolyte lithium salt in an organic solvent and stirring until completely dissolved to obtain an electrolyte solution;

[0010] S2, adding boron nitride nanopowder, g-C3N4, PEO, PVDF and powder dispersant to the electrolyte solution in sequence while stirring, and stirring thoroughly until a dark yellow slurry is obtained;

[0011] S3, coating the slurry prepared in S2 on a smooth and flat plate, vacuum drying, and obtaining a solid film on the plate; and making the solid film separate from the plate and float by water immersion;

[0012] S4. The solid film is clamped between two smooth and flat plates and dried to obtain a composite solid polymer electrolyte with a smooth surface.

[0013] According to a preferred embodiment of the present invention, in S1, the electrolyte lithium salt is lithium hexafluorophosphate (LiPF6) and / or lithium bis(trifluoromethanesulfonyl)imide (LiTFSi). Of course, the electrolyte lithium salt can also be lithium tetrafluoroborate (LiBF4).

[0014] According to a preferred embodiment of the present invention, in S1, the organic solvent is any one of DMF, NMP, DMAC and DEF, preferably DEF environmentally friendly solvent.

[0015] According to a preferred embodiment of the present invention, in S2, the boron nitride is boron nitride nanopowder obtained by wet ball milling, and the particle size thereof is 45-50 nm.

[0016] According to a preferred embodiment of the present invention, in S2, the stirring process is divided into three stages, the first stage is: adding boron nitride nanopowder, g-C3N4, PEO, PVDF and powder dispersant to the electrolyte solution while stirring, and the stirring speed is 300-400rpm (preferably 350rpm); the second stage is: after the addition is completed, the stirring speed is adjusted to 700-800rpm (preferably 750rpm), and stirred for 50-90min (preferably 60min); the third stage is: the stirring speed is increased to 1000-1200rpm (preferably 1000rpm), stirred for 5-7h (preferably 6h), and a dark yellow slurry can be obtained.

[0017] According to a preferred embodiment of the present invention, in S3, the smooth and flat plate is glass, the coating method is scraping or spin coating, etc., and the coating thickness of the slurry is adjusted according to the thickness of the solid polymer electrolyte membrane to be prepared.

[0018] According to a preferred embodiment of the present invention, in S3, the vacuum drying condition is drying at 75-85°C for 5-8h; preferably drying at 80°C for 6h.

[0019] According to a preferred embodiment of the present invention, in S1, the concentration of the electrolyte lithium salt in the electrolyte solution is 55-65 g / L, preferably 60 g / L.

[0020] According to a preferred embodiment of the present invention, in S2, the mass ratio of electrolyte lithium salt, boron nitride nanopowder, g-C3N4, PEO, and PVDF is 14-16:6-7:2.5-3.5:30:5-15; preferably, the mass ratio of the aforementioned materials is 15:6-7:3:30:10.

[0021] According to a preferred embodiment of the present invention, in S2, the powder dispersant is Auda powder dispersant AD8085 or AD8058, and its usage is 0.00005-0.0001% of the total volume of the slurry.

[0022] In a second aspect, the present invention provides a composite solid polymer electrolyte prepared by the preparation method of any one of the above embodiments.

[0023] (III) Beneficial effects

[0024] Compared with the prior art, the innovation and technical effects of the present invention mainly include:

[0025] (1) When preparing the slurry, PVDF accounting for about 1 / 3 of the mass of PEO is added to disperse PVDF into the PEO heterogeneous system, thereby destroying the crystallization of PEO, reducing the crystallinity of PEO, improving the electrochemical properties (including electrochemical properties such as ionic conductivity and breakdown voltage, etc.), and also improving the mechanical strength and flexibility.

[0026] (2) When preparing the slurry, the boron nitride nanopowder is directly added and mixed into the slurry of the PEO system. Compared with the hot pressing transfer method of the prior art, the present invention not only has a simple preparation process, but also can reduce the crystallinity of PEO by blending, and can evenly and effectively improve the mechanical strength of the PEO solid electrolyte membrane as a whole, reduce the roughness of the surface of the solid electrolyte membrane, and the surface of the electrolyte membrane is smoother and has better application performance. In addition, the present invention uses wet ball milling to prepare boron nitride nanopowder, which is finer (45-50nm) than the boron nitride nanosheets prepared by chemical stripping in the prior art, which is conducive to obtaining a solid electrolyte membrane with better surface flatness. In addition, when preparing the slurry, a solution of electrolyte lithium salt is first prepared, and the lithium salt can be completely dissolved in a solvent, and then boron nitride nanopowder, g-C3N4, PVDF, etc. are added for stirring, which can ensure the uniformity of the electrolyte lithium salt in the slurry.

[0027] (3) When preparing the slurry, a certain amount of porous lamellar structured g-C3N4 was also added. It not only reduced the crystallization tendency of the polymer by producing a strong cross-linking effect with the polymer PEO (confirmed by SEM), but also the introduction of g-C3N4 provided a larger surface interaction area, providing channels for more lithium ion transmission and improving the conductivity.

[0028] (4) When preparing the slurry, a small amount of Auda powder dispersant AD8085 is also added, which can be adsorbed on small powder particles to generate electrostatic repulsion to disperse the powder particles, so that the boron nitride nanopowder, g-C3N4, etc. that are originally difficult to disperse can be quickly dispersed, thereby making the prepared slurry disperse more quickly, the time for preparing the slurry is shortened, and the various doping materials in the prepared slurry are also dispersed more evenly, so that the various properties of the prepared polymer electrolyte membrane are more stable and uniform. Compared with the prior art, due to the addition of the powder dispersant, the stirring time for preparing the slurry is significantly shortened (the stirring time of the present invention is about 7.5-8h to obtain a uniform slurry).

[0029] (5) When preparing the polymer solid electrolyte membrane, the water immersion method is used to make the solid membrane after the slurry is dried separate from the smooth and flat plate and float naturally. The method is simple and easy to operate, avoiding the problems of membrane removal difficulty caused by the membrane being too large / thin, membrane breakage / deformation, or damage to the membrane due to operational problems, and is more suitable for industrial production.

[0030] (6) During the whole process of drying the polymer solid electrolyte membrane, the membrane is clamped between two smooth and flat plates by the clamping method, and the membrane is kept clamped while drying, so as to avoid problems such as membrane wrinkling and surface unevenness caused by drying by applying a certain pressure. Experiments have proved that this method can indeed prepare polymer solid electrolyte membranes with regular shapes and smooth surfaces.

[0031] In addition, based on the preparation method of the present invention, it can be known that compared with the prior art, the method of the present invention only includes operations such as dispersion stirring slurrying, coating, drying, and film stripping, and does not require a special atmosphere environment or large equipment. The process is simple and easy to operate, and is not limited by harsh process conditions such as glove boxes or argon atmosphere protection, so it is more suitable for large-scale industrial production. In short, the polymer solid electrolyte membrane prepared by the method of the present invention has the characteristics of adjustable thickness, low cost, environmental protection, good repeatability, stable product quality, and easy large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 These are SEM images of the PEO composite solid electrolyte membrane prepared in Example 1 of the present invention at different magnifications.

[0033] Figure 2 This is a physical photo of the PEO composite solid electrolyte membrane prepared in Example 1 of the present invention.

[0034] Figure 3 This is a physical photo of the PEO composite solid electrolyte membrane prepared in Comparative Example 1.

[0035] Figure 4 This is a physical photo of the PEO composite solid electrolyte membrane prepared in Comparative Example 3.

[0036] Figure 5 This is a photograph of the bending state of the PEO composite solid electrolyte membrane prepared in Example 1 of the present invention.

[0037] Figure 6 This is a photograph showing the uniformity and transparency of the PEO composite solid electrolyte membrane prepared in Example 1 of the present invention.

[0038] Figure 7 The left picture is the SEM picture of g-C3N4, and the right picture is the SEM picture of the electrolyte membrane of Example 1. DETAILED DESCRIPTION

[0039] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0040] Example 1

[0041] This embodiment provides a method for preparing a PEO composite solid electrolyte, the method comprising:

[0042] (1) Dissolving the electrolyte: Weigh 3 g of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and dissolve it in 50 mL of N-methylpyrrolidone (NMP). Stir until the electrolyte is completely dissolved. During this process, the rotation speed is maintained at 350 rpm.

[0043] (2) Adding materials: Boron nitride (1.3 g) (45-50 nm) prepared by wet ball milling, g-C3N4 (0.6 g), PEO (6 g) polyethylene oxide, PVDF (2 g) and Auda powder dispersant AD8085 (0.05 μL) were added in sequence, and the rotation speed remained unchanged during the addition process.

[0044] (3) Stirring and slurrying: First stir at 350 rpm for 30 min, then stir at 750 rpm for 1 h, and then increase to 1000 rpm and stir for 6 h to obtain a dark yellow slurry.

[0045] (4) The slurry is evenly coated on the glass plate, and the thickness is adjusted automatically. The glass plate is then placed in a vacuum drying oven and dried at 80°C for 6 hours. The glass plate is then taken out and immersed in a water pool. The film is taken out after it floats naturally.

[0046] (5) The membrane is placed between two layers of glass plates and the glass is clamped with a clip, and then placed in a 60°C oven for drying to obtain a PEO composite solid electrolyte membrane with adjustable thickness and a smooth surface.

[0047] After testing, the initial size of the PEO composite solid electrolyte membrane is 27*40cm 2 , thickness 30μm, conductivity test using 6*4cm 2 The size used for tensile testing is 14*1.5cm 2 The tested ion conductivity is 1.3966mS / cm and the tensile strength is 198kgf / cm 2 , breakdown voltage 1.97kV.

[0048] At the same time, the PEO composite solid electrolyte membrane prepared in the above embodiment was subjected to SEM test, and the results are as follows: Figure 1 As shown, the right picture is magnified 3000 times, and the left picture is magnified 500 times. At both magnifications, it can be seen that the surface of the PEO composite solid electrolyte membrane prepared in this embodiment has good flatness and is dense and pinhole-free.

[0049] For example Figure 2 As shown, it is a real photo of the PEO composite solid electrolyte membrane prepared in this embodiment. It can be seen that the solid electrolyte membrane is uniform milky white and has a smooth surface, which means that the various materials inside the electrolyte membrane are distributed very evenly (otherwise, there will be different shades of color).

[0050] like Figure 5 As shown, it is a photograph of the bending state of the PEO composite solid electrolyte membrane prepared in this embodiment (cut into discs). It can be seen that the electrolyte membrane has good flexibility, indicating that it has good bending resistance and good mechanical strength.

[0051] For example Figure 7As shown in the figure, SEM detection shows that the PEO in the electrolyte membrane is tightly wrapped and adhered to the surface of g-C3N4. This shows that when preparing the slurry, the added porous sheet structure g-C3N4 produces a strong cross-linking effect with the polymer PEO.

[0052] like Figure 6 As shown, this is a photograph of the uniformity and transparency of the PEO composite solid electrolyte membrane prepared in this embodiment (cut into discs). It can be seen that it is a uniform and translucent milky white color, indicating that the various materials inside the electrolyte membrane are distributed very evenly, and the electrolyte membrane has a certain transparency and can be suitable for special application fields.

[0053] Example 2

[0054] This embodiment provides a method for preparing a PEO composite solid electrolyte, the method comprising:

[0055] (1) Dissolving electrolyte: Weigh 3 g of lithium hexafluorophosphate (LiPF6) and dissolve it in 50 mL of DEF solvent. Stir until all the electrolyte is dissolved. During this process, the rotation speed is maintained at 350 rpm.

[0056] (2) Adding materials: Boron nitride (1.4 g) (45-50 nm) prepared by wet ball milling, g-C3N4 (0.56 g), PEO (6.15 g), polyethylene oxide, PVDF (2.05 g) and Auda powder dispersant AD8058 (0.06 μL) were added in sequence, and the rotation speed remained unchanged during the addition process.

[0057] (3) Stirring and slurrying: First stir at 350 rpm for 30 min, then stir at 750 rpm for 80 min, and then increase to 1200 rpm and stir for 5 h to obtain a dark yellow slurry.

[0058] (4) The slurry is evenly coated on the glass plate, and the thickness is adjusted automatically. The glass plate is then placed in a vacuum drying oven and dried at 80°C for 6 hours. The glass plate is then taken out and immersed in a water pool. The film is taken out after it floats naturally.

[0059] (5) The membrane is placed between two layers of glass plates and the glass is clamped with a clip, and then placed in a 60°C oven for drying to obtain a PEO composite solid electrolyte membrane with adjustable thickness and a smooth surface.

[0060] According to measurements, the PEO composite solid electrolyte membrane prepared in this embodiment has similar performance to the product prepared in Example 1.

[0061] Comparative Example 1

[0062] This comparative example is based on Example 1, but no boron nitride nanopowder and Auda powder dispersant AD8085 are added in the process of preparing the slurry. The remaining conditions and steps are the same as those in Example 1.

[0063] After testing, the PEO composite solid electrolyte membrane prepared in this comparative example has a thickness of 53 μm, an ionic conductivity of 0.6260 mS / cm, and a tensile strength of 117 kgf / cm 2 , breakdown voltage 1.55kV.

[0064] This shows that when boron nitride nanopowder is not added to the slurry, the tensile strength of the PEO electrolyte membrane will be significantly reduced.

[0065] The actual photo of the PEO composite solid electrolyte membrane prepared in this comparative example is as follows Figure 3 As shown. Figure 3 and Figure 2 By comparison, it can be seen that the PEO composite solid electrolyte membrane of Example 1 is uniform milky white as a whole and has a smooth surface (such as Figure 2 As shown in the figure, the surface color and transparency of the PEO composite solid electrolyte membrane prepared in this example vary in depth, and there are several bubble-like patterns on the surface, indicating that the various materials inside the electrolyte membrane are distributed very unevenly.

[0066] Comparative Example 2

[0067] This comparative example is based on Example 1, and g-C3N4 is not added in the process of preparing the slurry. The remaining conditions and steps are the same as those in Example 1.

[0068] After testing, the PEO composite solid electrolyte membrane prepared in this comparative example has a thickness of 20.02 μm, an ionic conductivity of 0.4937 mS / cm, and a tensile strength of 144 kgf / cm 2 , the breakdown voltage is 0.89 kV. This shows that when g-C3N4 powder is not added to the slurry, the conductivity of the PEO electrolyte membrane will decrease significantly.

[0069] Comparative Example 3

[0070] This comparative example is based on Example 1. In the drying process of step (5), the floating film soaked in water is directly placed in a 60°C oven for drying, and no pressure drying is applied by clamping two layers of glass plates. The remaining conditions and steps are the same as those of Example 1. Figure 4 The PEO composite solid electrolyte membrane shown.

[0071] Will Figure 4 and Figure 2 By comparison, it can be seen that the PEO composite solid electrolyte membrane of Example 1 is uniform milky white as a whole and has a very smooth surface (such as Figure 2 As shown in Figure 2, the surface wrinkles of the PEO composite solid electrolyte membrane prepared in this example are obvious (as shown in Figure 2 Figure 4As shown). It can be seen that during the drying process, if a flat and smooth flat plate is used to clamp the PEO composite solid electrolyte membrane for pressure drying, a composite solid electrolyte membrane with a flat surface can be obtained.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a composite solid polymer electrolyte, It is characterized in that It includes: S1. Dispersing electrolyte lithium salt in an organic solvent and stirring until completely dissolved to obtain an electrolyte solution; S2. Add boron nitride nanopowder, gC to the electrolyte solution in sequence while stirring. 3 N 4 , PEO, PVDF and powder dispersant, stir thoroughly until a dark yellow slurry is obtained; electrolyte lithium salt, boron nitride nanopowder, gC 3 N 4 , PEO, PVDF mass ratio is 14-16: 6-7: 2.5-3.5: 30: 5-15; the dosage of the powder dispersant is 0.00005-0.0001% of the total volume of the slurry; S3, coating the slurry prepared in S2 on a smooth and flat plate, vacuum drying, and obtaining a solid film on the plate; and making the solid film separate from the plate and float by water immersion; S4. The solid film is clamped between two smooth and flat plates and dried to obtain a composite solid polymer electrolyte with a smooth surface.

2. The preparation method according to claim 1, It is characterized in that In S1, the electrolyte lithium salt is at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl imide) and lithium tetrafluoroborate.

3. The preparation method according to claim 1, It is characterized in that In S1, the organic solvent is any one of DMF, NMP, DMAC and DEF.

4. The preparation method according to claim 1, It is characterized in that In S2, the boron nitride is boron nitride nanopowder obtained by wet ball milling, and the particle size thereof is 45-50 nm.

5. The preparation method according to claim 1, It is characterized in that In S2, the stirring process is divided into three stages. The first stage is to add boron nitride nanopowder, gC 3 N 4 , PEO, PVDF and powder dispersant are added while stirring at a speed of 300-400rpm; the second stage is: after the addition is completed, the stirring speed is adjusted to 700-800rpm, stirring for 50-90min; the third stage is: the stirring speed is increased to 1000-1200rpm, stirring for 5-7h, and a dark yellow slurry can be obtained.

6. The preparation method according to claim 1, It is characterized in that In S3, the smooth and flat plate is glass, the coating method is scraping or spin coating, and the coating thickness of the slurry is adjusted according to the thickness of the solid polymer electrolyte membrane to be prepared.

7. The preparation method according to claim 1, It is characterized in that In S1, the concentration of the electrolyte lithium salt in the electrolyte solution is 55-65 g / L.

8. The preparation method according to claim 1, It is characterized in that In S2, the powder dispersant is Auda powder dispersant AD8085 or AD8058.

9. A composite solid polymer electrolyte prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Preparation method of solid-state battery based on lithium powder dry electrode

    CN122800545A