Composite electrolyte used in field of energy storage solid-state batteries, and preparation method and application thereof

By adding inorganic dielectric nanofilters to a polyvinylidene fluoride-hexafluoropropylene copolymer system in lithium-ion batteries, a composite solid electrolyte with high lithium ion conductivity and electrochemical stability was prepared, which solved the safety of liquid electrolytes and The problem of low energy density improves the safety performance and energy density of the battery.

CN118919826APending Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411284764.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Liquid electrolytes in existing lithium-ion batteries are prone to safety accidents, and have low energy density, poor cycle stability, and the mechanical properties and preparation costs of solid electrolytes are difficult to meet safety and performance needs.

Method used

Inorganic dielectric nanofillers were added to the polyvinylidene fluoride-hexafluoropropylene copolymer system, and composite solid electrolytes were prepared by volatile solvent drying to form a composite electrolyte membrane with mechanical flexibility, high lithium ion conductivity and electrochemical stability.

Benefits of technology

The high cyclic charge and discharge specific capacity and rate charge and discharge specific capacity of the composite solid electrolyte are realized, which improves the safety performance and energy density of the battery and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919826A_ABST
    Figure CN118919826A_ABST
Patent Text Reader

Abstract

The invention relates to a composite electrolyte used in the field of energy storage solid-state batteries and a preparation method and application thereof, and the preparation method comprises the following steps: step (1): mixing a polyvinylidene fluoride-hexafluoropropylene copolymer and lithium bis (trifluoromethanesulfonimide), and dissolving in a solvent to obtain a polymer solid-state electrolyte solution; (2) adding an inorganic dielectric nanofiller into the polymer solid electrolyte solution, and adding a solvent again to obtain a composite solid electrolyte dispersion liquid; and (3) performing high-temperature drying on the composite solid electrolyte dispersion liquid to obtain the solid electrolyte. The composite solid electrolyte and a total battery assembled by taking lithium iron phosphate as a positive electrode and metal lithium as a negative electrode have the characteristics of large cyclic charge-discharge specific capacity and high rate charge-discharge specific capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of energy storage technology, and specifically relates to a composite electrolyte used in the field of energy storage solid-state batteries, and a preparation method and application thereof. Background Art

[0002] Most of the lithium-ion batteries that have been commercialized currently use electrolytes as transmission media and liquid organic carbonate solvents as solvents. Organic carbonates are volatile and flammable, which can easily lead to frequent battery safety accidents, including decomposition of the protective solid electrolyte interface, thermal runaway, and even combustion or explosion, which seriously affect people's daily lives. And over time, liquid electrolytes will degrade battery components and performance. In addition, liquid electrolytes are usually toxic and prone to combustion accidents, so they need to be firmly packaged to avoid leakage. These problems bring great inconvenience to people's daily life environment safety. In addition, lithium-ion batteries are very difficult to use in the long term. + Lithium dendrites will spontaneously form during the deposition and stripping process, which can also easily cause battery short circuits. If used improperly, they may even cause major safety issues such as fires and explosions. Therefore, it has become a top priority to improve the safety performance of lithium batteries while increasing their energy density, especially for portable electronic devices and electric vehicles. Solid electrolytes can further improve the energy density of liquid lithium-ion batteries and solve the current problems of low battery energy density and poor cycle stability. In the current research status of solid electrolytes, inorganic solid electrolyte systems have poor mechanical properties and are difficult to form effective contact with the positive and negative electrode interfaces. Sulfide solid electrolyte systems have high requirements for the preparation environment, are easily oxidized, and have high production costs. Polymer-based solid electrolytes are represented by polyethylene oxide (PEO), but they have a large degree of crystallinity and low room temperature ionic conductivity. Their batteries can only operate stably at 60°C. Summary of the invention

[0003] In order to overcome the problems existing in the above prior art, the purpose of the present invention is to provide a composite electrolyte for the field of energy storage solid-state batteries, a preparation method and application thereof, which adopts a solvent volatilization drying preparation molding method, can adapt to different molding mold shapes, and after adding inorganic dielectric nanofillers to the polyvinylidene fluoride-hexafluoropropylene copolymer system, the obtained composite solid electrolyte has mechanical flexibility, high lithium ion conductivity, large lithium ion migration number, wide electrochemical stability window, and can withstand high critical current density of charge and discharge. The composite solid electrolyte and the full battery assembled with lithium iron phosphate as the positive electrode and metallic lithium as the negative electrode achieve large cycle charge and discharge specific capacity and high rate charge and discharge specific capacity characteristics.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries comprises the following steps:

[0006] Step (1): mixing polyvinylidene fluoride-hexafluoropropylene copolymer and lithium bis(trifluoromethanesulfonyl imide) and dissolving them in a solvent to obtain a polymer solid electrolyte solution;

[0007] Step (2): adding an inorganic dielectric nanofiller to a polymer solid electrolyte solution, and then adding a solvent to obtain a composite solid electrolyte dispersion;

[0008] Step (3): drying the composite solid electrolyte dispersion at high temperature to obtain a solid electrolyte.

[0009] In the step (1), the molecular structures of the polyvinylidene fluoride-hexafluoropropylene copolymers are respectively as shown in formula (1):

[0010]

[0011] In the step (1), the mass fraction ratio of the polyvinylidene fluoride-hexafluoropropylene copolymer to lithium bis(trifluoromethanesulfonyl)imide is 1:0.3 to 1:2, and the solvent is a polar organic solvent such as N-methyl-2-pyrrolidone (NMP) or N,N-dimethylformamide (DMF).

[0012] The process is carried out under the following conditions: stirring at 25° C. (room temperature) for more than 30 minutes to fully dissolve the polyvinylidene fluoride-hexafluoropropylene copolymer and lithium bis(trifluoromethanesulfonylimide) in the solvent, and to evenly disperse the composite solid electrolyte dispersion solution.

[0013] The inorganic dielectric nanofiller added in step (2) has a mass fraction of 0.1-20 wt % of the mass of the polyvinylidene fluoride-hexafluoropropylene copolymer, and the added solvent is N-methyl-2-pyrrolidone (NMP);

[0014] The process is carried out under the following conditions: stirring at 25°C (room temperature) for 0.5-12h to allow the nanofiller to be evenly dispersed.

[0015] In the step (2), the inorganic dielectric nanofillers are titanium dioxide and barium titanate particles, respectively, with a particle size of 1-900 nm, and the crystal form of the particles is not limited.

[0016] In the step (3), the following conditions are applied:

[0017] The composite solid electrolyte dispersion is coated in a mold and dried at high temperature to form a composite solid electrolyte membrane;

[0018] Place the polytetrafluoroethylene mold coated with the composite solid electrolyte solution in a vacuum environment at 80°C-120°C for 10h-20h to ensure that the solvent evaporates and dries, stop heating until the temperature of the composite solid electrolyte membrane drops below 60°C, and remove it to obtain a polyvinylidene fluoride-hexafluoropropylene copolymer composite solid electrolyte with added inorganic dielectric nanofillers, i.e., a composite solid electrolyte membrane.

[0019] The polytetrafluoroethylene mold is a mold substrate on which circular pits with a diameter of 19-20 mm or other sizes are drilled to accommodate the composite solid electrolyte solution for volatilizing the solvent, and the required molding size can be designed and changed according to actual conditions.

[0020] The composite solid electrolyte membrane is assembled into a complete button battery in an argon-filled environment in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode metal lithium, gasket, shrapnel, and negative electrode shell.

[0021] A composite electrolyte for the field of energy storage solid-state batteries, wherein an inorganic dielectric nanofiller is dispersed in a polyvinylidene fluoride-hexafluoropropylene copolymer, and the composite solid-state electrolyte membrane maintains the flexibility of the polymer composite membrane; titanium dioxide and barium titanate have a large dielectric constant, and are used to effectively promote the dissociation and transmission behavior of lithium bis(trifluoromethanesulfonyl imide) in the polyvinylidene fluoride-hexafluoropropylene copolymer, so that the lithium bis(trifluoromethanesulfonyl imide) dissociates into free lithium ions and bis(trifluoromethanesulfonyl imide) anions, and the free lithium ions participate in the ion charge transport process in the solid-state electrolyte membrane; at the same time, the inorganic dielectric nanofiller affects the crystallinity of the polyvinylidene fluoride-hexafluoropropylene copolymer matrix, and synergizes with the large-volume -CF3 group of the polyvinylidene fluoride-hexafluoropropylene copolymer, so that the composite solid-state electrolyte membrane structure maintains the crystallinity of the polymer spherulite morphology and the rich pore morphology existing between the adhered spherulites, which is beneficial to the efficient and stable transmission of lithium ions in the composite solid-state electrolyte membrane.

[0022] Beneficial effects of the present invention:

[0023] First, due to the presence of bulky -CF3 groups, polyvinylidene fluoride-hexafluoropropylene copolymer has lower crystallinity than polyvinylidene fluoride;

[0024] Secondly, adding inorganic dielectric nanofillers to the electrolyte can further show a more obvious ability to dissociate lithium salts and adsorb anions. + The ratio of increases, promoting the ionic conductivity of the electrolyte;

[0025] Finally, the solution is simply coated on a polytetrafluoroethylene mold and dried at high temperature to obtain a composite electrolyte membrane. In short, the simple preparation method enables the present invention to have a wide range of application scenarios and provides more possibilities for the preparation of composite electrolytes. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a photo of the composite solid electrolyte prepared by the present invention.

[0027] Figure 2 The present invention is a flow chart for preparing the composite solid electrolyte.

[0028] Figure 3 This is a SEM image of the composite solid electrolyte with barium titanate added prepared in the present invention.

[0029] Figure 4 This is a SEM image of the composite solid electrolyte with titanium dioxide added prepared in the present invention.

[0030] Figure 5 This is the SEM image of Comparative Example 1 of the present invention.

[0031] Figure 6 This is the activation energy image of Example 1 of the present invention.

[0032] Figure 7 This is the activation energy image of Example 5 of the present invention.

[0033] Figure 8 Schematic diagram of the electrochemical window of the composite solid electrolyte with barium titanate prepared in the present invention.

[0034] Fig. 9 Schematic diagram of the electrochemical window of the composite solid electrolyte with titanium dioxide added prepared in the present invention.

[0035] Fig.10 Schematic diagram of the full-battery rate performance of Example 3 of the present invention.

[0036] Fig.11 Schematic diagram of the full-battery rate performance of Example 5 of the present invention.

[0037] Fig.12 Schematic diagram of the full-battery rate performance of comparative example 1 of the present invention.

[0038] Fig.13 Schematic diagram of the full battery cycle performance of Example 3 of the present invention.

[0039] Fig.14 Schematic diagram of the full battery cycle performance of Example 5 of the present invention.

[0040] Fig.15 Schematic diagram of the full battery cycle performance of comparative example 1 of the present invention. DETAILED DESCRIPTION

[0041] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0042] Example 1

[0043] like Figure 2 As shown:

[0044] (1) Preparation of polymer solid electrolyte solution

[0045] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0046] (2) Preparation of composite solid electrolyte dispersion

[0047] At 25° C., 0.01 g of barium titanate was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0048] (3) Preparation of composite solid electrolyte membrane

[0049] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0050] (4) Battery assembly

[0051] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0052] Example 2

[0053] (1) Preparation of polymer solid electrolyte solution

[0054] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0055] (2) Preparation of composite solid electrolyte solution

[0056] At 25° C., 0.05 g of barium titanate was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0057] (3) Preparation of composite solid electrolyte membrane

[0058] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0059] (4) Battery assembly

[0060] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0061] Example 3

[0062] (1) Preparation of polymer solid electrolyte solution

[0063] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0064] (2) Preparation of composite solid electrolyte solution

[0065] At 25° C., 0.1 g of barium titanate was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0066] (3) Preparation of composite solid electrolyte membrane

[0067] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0068] (4) Battery assembly

[0069] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0070] Example 4

[0071] (1) Preparation of polymer solid electrolyte solution

[0072] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0073] (2) Preparation of composite solid electrolyte solution

[0074] At 25° C., 0.2 g of barium titanate was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0075] (3) Preparation of composite solid electrolyte membrane

[0076] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0077] (4) Battery assembly

[0078] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0079] Example 5

[0080] (1) Preparation of polymer solid electrolyte solution

[0081] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0082] (2) Preparation of composite solid electrolyte dispersion

[0083] At 25° C., 0.01 g of titanium dioxide was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0084] (3) Preparation of composite solid electrolyte membrane

[0085] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0086] (4) Battery assembly

[0087] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0088] Example 6

[0089] (1) Preparation of polymer solid electrolyte solution

[0090] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0091] (2) Preparation of composite solid electrolyte dispersion

[0092] At 25° C., 0.05 g of titanium dioxide was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0093] (3) Preparation of composite solid electrolyte membrane

[0094] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0095] (4) Battery assembly

[0096] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0097] Example 7

[0098] (1) Preparation of polymer solid electrolyte solution

[0099] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0100] (2) Preparation of composite solid electrolyte dispersion

[0101] At 25° C., 0.1 g of titanium dioxide was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0102] (3) Preparation of composite solid electrolyte membrane

[0103] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0104] (4) Battery assembly

[0105] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0106] Example 8

[0107] (1) Preparation of polymer solid electrolyte solution

[0108] At 25° C., 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 min to obtain a polymer PVDF-HFP-based electrolyte solution.

[0109] (2) Preparation of composite solid electrolyte dispersion

[0110] At 25° C., 0.2 g of titanium dioxide was added to the polymer solid electrolyte solution, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added again and stirred for 12 h to obtain a PVDF-HFP-based composite solid electrolyte dispersion.

[0111] (3) Preparation of composite solid electrolyte membrane

[0112] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0113] (4) Battery assembly

[0114] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0115] Comparative Example 1

[0116] (1) Preparation of polymer solid electrolyte solution without inorganic dielectric nanofillers

[0117] At 25°C, 1 g of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and 1.25 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were weighed, and 5 ml of N-methyl-2-pyrrolidone (NMP) solvent was added and stirred for 30 minutes to obtain a polymer PVDF-HFP-based electrolyte solution free of inorganic dielectric nanofillers.

[0118] (2) Preparation of composite solid electrolyte membrane

[0119] The uniformly dispersed solution was coated on a polytetrafluoroethylene mold and dried at 100° C. for 12 h under a vacuum environment to obtain the desired polyvinylidene fluoride-hexafluoropropylene copolymer-based composite electrolyte.

[0120] (3) Battery assembly

[0121] The obtained composite solid electrolyte is assembled into a complete button battery in the order of positive electrode shell, positive electrode, electrolyte, negative electrode, gasket, spring and negative electrode shell in an argon-filled environment.

[0122] Figure 1 It shows a real picture of the prepared composite electrolyte; it can be seen from the figure that the composite electrolyte prepared by drying maintains a consistent shape with the polytetrafluoroethylene circular molding mold, and has excellent processability. The composite electrolyte membrane in the figure has a diameter of 19 mm and shows a uniform translucent milky white color after adding inorganic nano-dielectric fillers, proving that the composite electrolyte membrane prepared by stirring has uniformity and consistency of nano-filler dispersion.

[0123] Figure 2 It shows the flow chart of electrolyte preparation;

[0124] Figure 3 The cross-sectional scanning electron microscope image of the prepared composite solid electrolyte membrane with barium titanate added is shown, in which a large number of spherulites exist, and the spherulites are conducive to ion conduction; it can be seen from the figure that in the composite solid electrolyte membrane, the polyvinylidene fluoride-hexafluoropropylene copolymer as a polymer matrix has a crystalline form of polymer spherulites, and the spherulites are dispersed and adhered to each other, and the gaps are dispersed between the adhered spherulites; the nano-sized barium titanate particles are distributed in the composite solid electrolyte membrane, and no obvious agglomeration and dispersion phenomenon is observed, the dispersion is good, and the composite solid electrolyte film has a uniform morphology;

[0125] Figure 4The scanning electron microscope cross-sectional image of the prepared composite solid electrolyte membrane with titanium dioxide added is shown, and its surface is smooth and there is a tendency to form spherulites. The 10um magnification image shows a uniform and smooth surface morphology; in the 1um magnification image, pores on the surface of the polyvinylidene fluoride-hexafluoropropylene copolymer spherulites after film formation can be seen, and the pore size is generally small. The inorganic dielectric nanofiller can affect the formation and growth behavior of the polymer spherulites and further promote the composite solid electrolyte membrane to form a dense, uniform overall structure and a smooth surface morphology;

[0126] Figure 5 The scanning electron microscope cross-sectional image of Comparative Example 1 shown in FIG. 1 shows that since no inorganic nano-dielectric filler is added, a tendency to form spherulites can be observed on its surface, but there are many pores, indicating that the solid electrolyte membrane without inorganic nano-dielectric filler cannot form a smooth surface during the drying and molding process. This may be because the spherulites are large in size and cannot effectively diffuse and adhere to each other and serve as channels for the volatilization and dispersion of the solvent, resulting in the formation of larger pores on the surface.

[0127] Figure 6 and Figure 7 The activation energy images of lithium ion dissociation and transmission in Example 1 and Example 5 are shown respectively. The lower the activation energy, the faster the migration speed of lithium ions.

[0128] Figure 8 and Fig. 9 They respectively represent the electrochemical windows of the composite solid electrolyte membrane with added barium titanate and the composite solid electrolyte membrane with added titanium dioxide. The larger electrochemical window can be well adapted to high-voltage positive electrode materials.

[0129] Fig.10 The full battery rate performance of Example 1 is 110 mAh g at a current density of 0.2 C. -1 discharge capacity.

[0130] Fig.11 The full battery rate performance of Example 5 is 80 mAh g at a current density of 0.5 C. -1 The discharge capacity of

[0131] Fig.12 The full battery rate performance of Comparative Example 1 is 100 mAh g at a current density of 0.2 C. -1 The discharge capacity of

[0132] Fig.13 The full battery cycle performance of Example 3, wherein the electrolyte cycle performance represented by Example 3 is stable, and the discharge capacity is still 160 mAh g after 40 cycles at 0.1C. -1 , the capacity retention rate is 98.7%;

[0133] Fig.14 The full battery cycle performance of Example 5, wherein the electrolyte represented by Example 5 still has a discharge capacity of 129 mAh g after 40 cycles at 0.1C. -1 , the capacity retention rate is 96.2%;

[0134] Fig.15 The full battery cycle performance of Comparative Example 1, where the electrolyte represented by Comparative Example 1 still has a discharge capacity of 140 mAh g after 40 cycles at 0.1C. -1 , the capacity retention rate is 89.8%.

[0135] Table 1 shows the ionic conductivity of the composite solid electrolyte prepared by the present invention with the addition of barium titanate;

[0136] Sample 1 Sample 2 Sample 3 Sample 4 <![CDATA[7.87×10 -4 S cm -1 ]]> <![CDATA[6.98×10 -4 S cm -1 ]]> <![CDATA[6.97×10 -4 S cm -1 ]]> <![CDATA[6.41×10 -4 S cm -1 ]]>

[0137] Sample 1: the preparation method corresponding to Example 1.

[0138] Sample 2: corresponding to the preparation method of Example 2.

[0139] Sample 3: corresponding to the preparation method of Example 3.

[0140] Sample 4: the preparation method corresponding to Example 4.

[0141] Table 2 shows the ionic conductivity of the composite solid electrolyte added with titanium dioxide prepared in the present invention;

[0142] Sample 5 Sample 6 Sample 7 Sample 8 <![CDATA[6.21×10 -5 S cm -1 ]]> <![CDATA[2.83×10 -5 S cm -1 ]]> <![CDATA[1.83×10 -5 S cm -1 ]]> <![CDATA[1.21×10 -5 S cm -1 ]]>

[0143] Sample 5: corresponding to the preparation method of Example 5.

[0144] Sample 6: the preparation method corresponding to Example 6.

[0145] Sample 7: preparation method corresponding to Example 7.

[0146] Sample 8: corresponding to the preparation method of Example 8.

[0147] Table 3 shows the electronic conductivity of the composite solid electrolyte added with barium titanate prepared by the present invention;

[0148] Sample 1 Sample 2 Sample 3 Sample 4 <![CDATA[4.28×10 -9 S cm -1 ]]> <![CDATA[3.71×10 -9 S cm -1 ]]> <![CDATA[3.44×10 -9 S cm -1 ]]> <![CDATA[3.62×10 -9 S cm -1 ]]>

[0149] Sample 1: corresponding to the preparation method of Example 1.

[0150] Sample 2: corresponding to the preparation method of Example 2.

[0151] Sample 3: corresponding to the preparation method of Example 3.

[0152] Sample 4: corresponding to the preparation method of Example 4.

[0153] Table 4 shows the electronic conductivity of the composite solid electrolyte added with titanium dioxide prepared by the present invention;

[0154] Sample 1 Sample 2 Sample 3 Sample 4 <![CDATA[1.30×10 -9 S cm -1 ]]> <![CDATA[4.55×10 -10 S cm -1 ]]> <![CDATA[2.60×10 -10 S cm -1 ]]> <![CDATA[1.05×10 -10 S cm -1 ]]>

[0155] Sample 5: corresponding to the preparation method of Example 5.

[0156] Sample 6: the preparation method corresponding to Example 6.

[0157] Sample 7: preparation method corresponding to Example 7.

[0158] Sample 8: corresponding to the preparation method of Example 8.

[0159] Table 5 shows the lithium ion migration number of the composite solid electrolyte added with barium titanate prepared by the present invention;

[0160] Sample 1 Sample 2 Sample 3 Sample 4 0.287 0.114 0.123 0.0577

[0161] Sample 1: the preparation method corresponding to Example 1.

[0162] Sample 2: corresponding to the preparation method of Example 2.

[0163] Sample 3: corresponding to the preparation method of Example 3.

[0164] Sample 4: corresponding to the preparation method of Example 4.

[0165] Table 6 shows the lithium ion migration number of the composite solid electrolyte added with titanium dioxide prepared by the present invention;

[0166] Sample 5 Sample 6 Sample 7 Sample 8 0.0856 0.0753 0.0599 0.0444

[0167] Sample 5: corresponding to the preparation method of Example 5.

[0168] Sample 6: the preparation method corresponding to Example 6.

[0169] Sample 7: preparation method corresponding to Example 7.

[0170] Sample 8: corresponding to the preparation method of Example 8.

[0171] Table 7 shows the critical current density of the composite solid electrolyte added with barium titanate prepared by the present invention;

[0172] Sample 1 Sample 2 Sample 3 Sample 4 <![CDATA[0.55mA cm -2 ]]> <![CDATA[0.5mA cm -2 ]]> <![CDATA[0.5mA cm -2 ]]> <![CDATA[0.45mA cm -2 ]]>

[0173] Sample 1: the preparation method corresponding to Example 1.

[0174] Sample 2: corresponding to the preparation method of Example 2.

[0175] Sample 3: The preparation method corresponding to Example 3.

[0176] Sample 4: corresponding to the preparation method of Example 4.

[0177] Table 8 shows the critical current density of the composite solid electrolyte with titanium dioxide added prepared by the present invention;

[0178] Sample 1 Sample 2 Sample 3 Sample 4 <![CDATA[0.65mA cm -2 ]]> <![CDATA[0.65mA cm -2 ]]> <![CDATA[0.45mA cm -2 ]]> <![CDATA[0.45mA cm -2 ]]>

[0179] Sample 5: corresponding to the preparation method of Example 5.

[0180] Sample 6: the preparation method corresponding to Example 6.

[0181] Sample 7: preparation method corresponding to Example 7.

[0182] Sample 8: corresponding to the preparation method of Example 8.

[0183] Table 9 shows the anti-lithium dendrite long cycle performance of the composite solid electrolyte added with barium titanate prepared by the present invention;

[0184] Sample 1 Sample 2 Sample 3 Sample 4 445h 181h 254h 143h

[0185] Sample 1: the preparation method corresponding to Example 1.

[0186] Sample 2: corresponding to the preparation method of Example 2.

[0187] Sample 3: The preparation method corresponding to Example 3.

[0188] Sample 4: corresponding to the preparation method of Example 4.

[0189] Table 10 shows the anti-lithium dendrite long cycle performance of the composite solid electrolyte with titanium dioxide added prepared by the present invention;

[0190] Sample 1 Sample 2 Sample 3 Sample 4 119h 330h 109h 205h

[0191] Sample 5: corresponding to the preparation method of Example 5.

[0192] Sample 6: the preparation method corresponding to Example 6.

[0193] Sample 7: preparation method corresponding to Example 7.

[0194] Sample 8: corresponding to the preparation method of Example 8.

Claims

1. A method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries, characterized in that: The steps include: Step (1): mixing polyvinylidene fluoride-hexafluoropropylene copolymer and lithium bis(trifluoromethanesulfonyl imide) and dissolving them in a solvent to obtain a polymer solid electrolyte solution; Step (2): adding an inorganic dielectric nanofiller to a polymer solid electrolyte solution, and then adding a solvent to obtain a composite solid electrolyte dispersion; Step (3): drying the composite solid electrolyte dispersion at high temperature to obtain a solid electrolyte.

2. The method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries according to claim 1, characterized in that: In the step (1), the molecular structures of the polyvinylidene fluoride-hexafluoropropylene copolymers are respectively as shown in formula (1):

3. The method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries according to claim 1, characterized in that: In the step (1), the mass fraction ratio of polyvinylidene fluoride-hexafluoropropylene copolymer to lithium bis(trifluoromethanesulfonyl)imide is 1:0.3 to 1:2, and the solvent is N-methyl-2-pyrrolidone (NMP) or N,N-dimethylformamide (DMF); The process is carried out under the following conditions: stirring at 25° C. (room temperature) for more than 30 minutes to fully dissolve the polyvinylidene fluoride-hexafluoropropylene copolymer and lithium bis(trifluoromethanesulfonylimide) in the solvent, and to evenly disperse the composite solid electrolyte dispersion solution.

4. The method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries according to claim 1, characterized in that: The inorganic dielectric nanofiller added in step (2) has a mass fraction of 0.1-20 wt % of the mass of the polyvinylidene fluoride-hexafluoropropylene copolymer, and the added solvent is N-methyl-2-pyrrolidone (NMP); The process is carried out under the following conditions: stirring at 25°C (room temperature) for 0.5-12h to allow the nanofiller to be evenly dispersed.

5. The method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries according to claim 4, characterized in that: In the step (2), the inorganic dielectric nanofillers are titanium dioxide and barium titanate particles, respectively, with a particle size of 1-900 nm, and the crystal form of the particles is not limited.

6. The method for preparing a composite electrolyte for use in the field of energy storage solid-state batteries according to claim 1, characterized in that: In the step (3), the following conditions are applied: The composite solid electrolyte dispersion is coated in a mold and dried at high temperature to form a composite solid electrolyte membrane; Place the polytetrafluoroethylene mold coated with the composite solid electrolyte solution in a vacuum environment at 80°C-120°C for 10h-20h to ensure that the solvent evaporates and dries, stop heating until the temperature of the composite solid electrolyte membrane drops below 60°C, and remove it to obtain a polyvinylidene fluoride-hexafluoropropylene copolymer composite solid electrolyte with added inorganic dielectric nanofillers, i.e., a composite solid electrolyte membrane.

7. The use of the composite solid electrolyte membrane according to claim 6, characterized in that: The composite solid electrolyte membrane is assembled into a complete button battery in an argon-filled environment in the order of positive electrode shell, positive electrode, electrolyte membrane, negative electrode metal lithium, gasket, shrapnel, and negative electrode shell.

8. A composite electrolyte for use in the field of energy storage solid-state batteries prepared by the method according to any one of claims 1 to 6, characterized in that: Inorganic dielectric nanofillers are dispersed in the polyvinylidene fluoride-hexafluoropropylene copolymer, and the composite solid electrolyte membrane maintains the flexibility of the polymer composite membrane; titanium dioxide and barium titanate have a large dielectric constant, which is used to effectively promote the dissociation and transmission behavior of lithium bis(trifluoromethanesulfonyl imide) in the polyvinylidene fluoride-hexafluoropropylene copolymer, so that the lithium bis(trifluoromethanesulfonyl imide) dissociates into free lithium ions and bis(trifluoromethanesulfonyl imide) anions, and the free lithium ions participate in the ion charge transport process in the solid electrolyte membrane; at the same time, the inorganic dielectric nanofillers affect the crystallinity of the polyvinylidene fluoride-hexafluoropropylene copolymer matrix, and synergistically act with the large-volume -CF3 group of the polyvinylidene fluoride-hexafluoropropylene copolymer, so that the composite solid electrolyte membrane structure maintains the crystallinity of the polymer spherulite morphology and the rich pore morphology existing between the adhesion spherulites, which is beneficial to the efficient and stable transmission of lithium ions in the composite solid electrolyte membrane.

Citation Information

Cited By

  • High-dielectric external-flexible internal-rigid composite solid electrolyte and preparation method and application thereof

    CN120376729A

  • A high-dielectric composite solid electrolyte with a flexible outer layer and a rigid inner layer, its preparation method and application