Viscous-state hydrogenated nitrile rubber as well as preparation method and application thereof

By changing the regularity of hydrogenated nitrile rubber and using new vulcanizing agents, the problems of decreasing adhesion force and electrochemical stability of hydrogenated nitrile rubber at low temperatures were solved, and a viscous current with good low temperature resistance and electrochemical stability were prepared. Hydrogenated nitrile rubber is used in lithium-ion battery electrode sheets, improving battery performance.

CN118909566APending Publication Date: 2024-11-08FUJIAN LIANGJINGJING NEW MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411153499.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing hydrogenated nitrile rubber has high crystallinity at low temperatures, resulting in a decrease in adhesion force. The introduction of active sites of conventional vulcanizing agents affects the electrochemical stability, making it difficult to maintain good performance in lithium batteries.

Method used

Modified hydrogenated nitrile rubber is prepared by adding N-vinyl-2-pyrrolidone, and a new vulcanizing agent is used to reduce solubility and increase electrochemical stability, combined with specific feeding speeds and reaction conditions , viscous fluid hydrogenated nitrile rubber with good low temperature resistance and electrochemical stability was prepared.

Benefits of technology

The good adhesion and conductivity of the electrode sheet of the lithium-ion battery under low temperature conditions is achieved, which reduces side reactions, improves the performance and electrochemical stability of the lithium battery, and reduces the amount of adsorbed water and reduces the dehydration time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004252380000101
    Figure BDA0005004252380000101
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogenated butadiene-acrylonitrile rubber, in particular to viscous-state hydrogenated butadiene-acrylonitrile rubber and a preparation method thereof.The viscous-state hydrogenated butadiene-acrylonitrile rubber is prepared from, by weight, 30-40 parts of modified hydrogenated butadiene-acrylonitrile rubber, 2-3 parts of sulfur, 2-3 parts of vulcanizing agent, 1-2 parts of vulcanization accelerator, 270-360 parts of solvent and 540-720 parts of dehydrating agent. The viscous-state hydrogenated butadiene-acrylonitrile rubber provided by the invention has good electrochemical inertness and cold resistance, and can be applied to manufacturing of lithium battery electrode plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogenated nitrile rubber, and in particular to a viscous hydrogenated nitrile rubber and a preparation method and application thereof. Background Art

[0002] Nitrile rubber is obtained by copolymerization of acrylonitrile and butadiene. It has polar cyano groups in its molecular structure, so it has good oil resistance and chemical resistance. However, due to the large number of unsaturated double bonds in nitrile rubber, its aging resistance and heat resistance are poor. When used, the carbon-carbon unsaturated double bonds in nitrile rubber are usually selectively hydrogenated to obtain hydrogenated nitrile rubber, which has good oil resistance, wear resistance, weather resistance and chemical stability and is widely used in automobiles, petroleum, aerospace, battery energy storage and other fields. In lithium-ion batteries, hydrogenated nitrile rubber is one of the alternative materials for lithium-ion battery binders due to its good viscoelasticity and electrochemical stability. However, conventional hydrogenated nitrile rubber has a high degree of crystallinity and decreased elasticity at low temperatures, which will lead to a decrease in its adhesion and a decrease in battery performance at low temperatures. In addition, in order to reduce the solubility of hydrogenated nitrile rubber in the electrolyte, hydrogenated nitrile needs to be cross-linked using a vulcanizing agent. Conventional vulcanizing agents inevitably introduce active sites such as sulfur and peroxide groups, affecting its electrochemical stability. Therefore, enhancing the elasticity and electrochemical stability of hydrogenated nitrile rubber has become a key research topic for researchers in this field.

[0003] Patent CN105524313B discloses a high and low temperature resistant nitrile rubber material. The patent uses a high acrylonitrile content nitrile rubber and an ethylene propylene rubber to blend to prepare a high and low temperature resistant nitrile rubber material, and uses ethylene-vinyl acetate rubber, ethylene acrylate rubber, etc. as a compatibilizer, and then adds methyl acrylate, and cross-links with various rubbers under a peroxide vulcanization system, thereby improving the physical and mechanical properties of the blended rubber. The blended rubber prepared by this method has excellent mechanical properties, good oil resistance and high and low temperature resistance, but the vulcanizing agent used introduces a large number of active sites and cannot be used as an adhesive for electrode sheets.

[0004] Patent CN117247566A discloses a method for preparing a viscous flow state of hydrogenated nitrile rubber, wherein crushed hydrogenated nitrile rubber and N-methylpyrrolidone are poured into a reactor and heated and stirred, and then an external circulation is started, and the material in the reactor is sent out from the bottom of the reactor, passes through three filters along an external pipe, and the filtered material returns to the reactor and circulates repeatedly; then the circulation is closed, and the material is heated and stirred again in the reactor, and the material is discharged and packaged through the filter. This method will inevitably absorb water during the preparation process, resulting in a significant reduction in the performance of the viscous flow hydrogenated nitrile rubber in lithium batteries when used.

[0005] Therefore, there is an urgent need in the market for a viscous hydrogenated nitrile rubber that has good low temperature resistance and electrochemical stability and will not reduce the performance of lithium batteries. Summary of the invention

[0006] In view of the problems existing in the prior art, the purpose of the present invention is to obtain a viscous hydrogenated nitrile rubber which has good low temperature resistance and electrochemical stability and will not reduce the performance of lithium batteries.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] On one hand, the present invention provides a viscous hydrogenated nitrile rubber, which comprises the following raw materials, measured in parts by weight: 30-40 parts of modified hydrogenated nitrile rubber, 1-2 parts of sulfur, 2-3 parts of vulcanizing agent, 0.5-1 part of vulcanization accelerator, 270-360 parts of solvent, and 540-720 parts of dehydrating agent.

[0009] In some embodiments, the method for preparing the modified hydrogenated nitrile rubber comprises the following steps:

[0010] (1) adding deionized water, an emulsifier, acrylonitrile, and a chelating agent into a reaction vessel, stirring for 15-25 minutes, removing air from the reaction system, adding butadiene, a reducing agent, and an initiator at 30-40° C., reacting for 1-2 hours, and obtaining a copolymer A having a weight average molecular weight of 30,000-40,000;

[0011] (2) adding deionized water, an emulsifier, and N-vinyl-2-pyrrolidone into a reaction vessel, stirring for 15-25 minutes, removing air from the reaction system, adding butadiene, a reducing agent, and an initiator at 30-40° C., reacting for 1-2 hours, and obtaining a copolymer B having a weight average molecular weight of 30,000-40,000;

[0012] (3) adding copolymer B to copolymer A, reacting at 30-40° C. for 7-8 hours to obtain modified nitrile rubber;

[0013] (4) adding a first catalyst to the modified nitrile rubber obtained in step (3), introducing hydrogen at a pressure of 5-6 MPa, reacting at 55-65° C. for 2-3 h, filtering, adding a flocculant to the filtrate, filtering, washing, and drying to obtain a modified hydrogenated nitrile rubber.

[0014] Preferably, in step (3), the rate of adding copolymer B to copolymer A is 400-500 g / h.

[0015] Conventional hydrogenated nitrile rubber has a relatively regular structure, and has a high crystallinity and reduced elasticity at low temperatures, which will lead to a decrease in its bonding strength and make it unusable at low temperatures. The present invention reduces its crystallization ability by changing the regularity of hydrogenated nitrile rubber, so that the hydrogenated nitrile rubber has better low temperature resistance. The applicant destroys the regularity of hydrogenated nitrile rubber by adding N-vinyl-2-pyrrolidone to obtain a modified hydrogenated nitrile rubber, which is used as a binder for lithium ion battery electrode sheets and has good bonding strength at low temperatures. At the same time, the conductivity of the electrode sheet is increased. On the one hand, it may be because the modified hydrogenated nitrile rubber has better elasticity after modification. When the volume of the active substance in the battery changes before and after the reaction, it can still maintain good bonding strength and maintain the structure of the electrode sheet. On the other hand, copolymer A may be added through copolymer B, and a certain feeding speed is set to make N-vinyl-2-pyrrolidone relatively evenly distributed in the obtained rubber, so that the pyrrole ring and the metal ions on the surface of the lithium iron phosphate particles in the battery interact with each other by electrostatic adsorption, coordination, etc., reducing the surface energy of the particles, making them more dispersible in solution and not easy to aggregate, thereby increasing the ion conductivity of the lithium battery and improving the performance of the lithium battery. In addition, nitrile rubber with a higher degree of hydrogenation can reduce side reactions with electrolytes, but too high a degree of hydrogenation will lead to poor solubility in N-methylpyrrolidone. N-vinyl-2-pyrrolidone used in the present invention also contains a pyrrolidone ring, and similar substances are soluble in each other, thereby increasing the solubility of hydrogenated nitrile rubber.

[0016] In some embodiments, the mass ratio of acrylonitrile to butadiene in step (1) is 1:(1-1.5).

[0017] In some embodiments, in step (2), the mass ratio of N-vinyl-2-pyrrolidone to butadiene is 1:(2-3).

[0018] In some embodiments, the mass ratio of copolymer A to copolymer B in step (3) is 1:(0.2-0.4).

[0019] The invention controls the mass ratio of acrylonitrile to butadiene to prevent the acrylonitrile content from being too high, which leads to an overly fast vulcanization speed and reduced elasticity and tear resistance of the generated rubber; in addition, the mass ratio of N-vinyl-2-pyrrolidone to butadiene is controlled to make the copolymer B more compatible with the copolymer A, promote the occurrence of polymerization reaction, and obtain the modified hydrogenated nitrile rubber with uniform texture and better performance; in addition, the mass ratio of copolymer A to copolymer B is limited to increase the low temperature resistance of the modified hydrogenated nitrile rubber without affecting other properties.

[0020] In some embodiments, the method for preparing the vulcanizing agent comprises the following steps:

[0021] 1) adding oxidized resveratrol and an initiator to ethanol, reacting at 60-70° C. for 25-35 min, filtering, washing, and drying to obtain a polymer with a weight average molecular weight of 800-1100;

[0022] 2) reacting the polymer obtained in step 1), 2-fluoroacrylic acid and a second catalyst at 70-80° C. for 5-6 hours, filtering, washing and drying to obtain a vulcanizing agent.

[0023] In some embodiments, the mass ratio of the polymer to 2-fluoroacrylic acid in step 2) is (1-2):1.

[0024] Hydrogenated nitrile rubber has a certain solubility in the electrolyte of lithium ion battery. Crosslinking hydrogenated nitrile rubber is a feasible method to reduce its solubility in electrolyte. Thermal crosslinking method will lead to reduced toughness of hydrogenated nitrile rubber. The vulcanizing agent used in chemical crosslinking method inevitably brings sulfur-containing or peroxide groups, which affects electrochemical stability. The present invention prepares a new type of vulcanizing agent, which replaces part of the traditional vulcanizing agent, so that the network crosslinking structure produced by hydrogenated nitrile rubber reduces the solubility in the electrolyte, and has good adhesion and electrochemical stability. On the one hand, it may be that the alkane segment increases the flexibility of the rubber, making it easier to increase elasticity. On the other hand, it may be due to the introduction of a certain amount of F atoms by limiting the mass ratio of polymer and 2-fluoroacrylic acid, increasing electrochemical inertness, making up for the deficiency of traditional vulcanizing agent, and at the same time, the ester group has polarity and can form a strong interaction with the surface of electrode active material, further improving adhesion; in addition, benzene ring, alkane segment, and ester group all have strong hydrophobicity, which reduces the amount of adsorbed water in viscous hydrogenated nitrile rubber and reduces the dehydration time.

[0025] In some embodiments, the vulcanization accelerator is SA1801.

[0026] In some embodiments, the solvent is N-methylpyrrolidone.

[0027] In some embodiments, the dehydrating agent is anhydrous ethanol.

[0028] A second aspect of the present invention provides a method for preparing a viscous-fluid hydrogenated nitrile rubber, comprising the following steps:

[0029] S1, vulcanization: adding modified hydrogenated nitrile rubber, sulfur, vulcanizing agent, and vulcanization accelerator to an open mill and rolling together until there is no viscous liquid on the surface of the rubber roll, then adding to a vulcanizer for vulcanization, the vulcanization temperature is 145-150°C, the vulcanization time is 50-60min, the vulcanization pressure is 10MPa-15MPa, and the lower sheet is cooled to obtain a vulcanized modified hydrogenated nitrile rubber;

[0030] S2, dissolving: crush the obtained vulcanized modified hydrogenated nitrile rubber into 1-3 cm particles, add solvent, stir at 105-115° C. for 55-65 min under nitrogen protection, filter, and continue stirring the filtrate at 90-100° C. for 55-65 min to obtain material 1;

[0031] S3, dehydration and discharging: add material 1 and part of the dehydrating agent into the reaction kettle respectively, stir for 55-65 minutes at 55-65°C and pressure of -0.1-0KPa, then add the remaining dehydrating agent, continue stirring for 55-65 minutes at 55-65°C and pressure of -0.1-0KPa, cool to room temperature, and discharge to obtain viscous hydrogenated nitrile rubber.

[0032] The third aspect of the present invention provides an application of viscous flow hydrogenated nitrile rubber in manufacturing lithium battery electrode sheets.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The present invention obtains a viscous hydrogenated nitrile rubber having good low temperature resistance and electrochemical stability and will not reduce the performance of lithium batteries by adding N-vinyl-2-pyrrolidone and a vulcanizing agent.

[0035] 2. The present invention reduces the crystallization ability of hydrogenated nitrile rubber by changing its regularity, so that the hydrogenated nitrile rubber has better low temperature resistance, and the modified hydrogenated nitrile rubber used as a binder for lithium ion battery electrode sheets also has good bonding force at low temperatures, while increasing the conductivity of the electrode sheets. In addition, the nitrile rubber with an excessively high degree of hydrogenation can reduce side reactions with electrolytes. In addition, N-vinyl-2-pyrrolidone is used in the present invention, which also contains a pyrrolidone ring, and similar things dissolve in each other, thereby increasing the solubility of the hydrogenated nitrile rubber.

[0036] 3. The present invention prepares a new type of vulcanizing agent, which makes the hydrogenated nitrile rubber produce a network cross-linked structure, reduces the solubility in the electrolyte, and has good adhesion and electrochemical stability; in addition, the benzene ring, alkane chain segment, and ester group all have strong hydrophobicity, which reduces the amount of adsorbed water in the viscous hydrogenated nitrile rubber and reduces the dehydration time. DETAILED DESCRIPTION

[0037] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0038] In the following examples and comparative examples, the compound monomers and related reagents used can be purchased from the market, among which SA1801 was purchased from Wuhan Proloff Biotechnology Co., Ltd.

[0039] Preparation Example 1

[0040] The preparation method of modified hydrogenated nitrile rubber-1 comprises the following steps:

[0041] (1) 300 g of deionized water, 4 g of sodium dodecyl sulfate, 24 g of acrylonitrile, and 0.05 g of disodium ethylenediaminetetraacetate were added to a reaction vessel, stirred for 20 min, nitrogen was passed through, 31.2 g of 1,3-butadiene, 0.05 g of ferrous sulfate, and 0.25 g of ammonium persulfate were added at 35° C., and the mixture was reacted for 1.5 h to obtain a copolymer A with a weight average molecular weight of 36347;

[0042] (2) 100 g of deionized water, 1.5 g of sodium dodecyl sulfate, and 10 g of N-vinyl-2-pyrrolidone were added to a reaction vessel and stirred for 20 min. The air in the reaction system was removed, and 25 g of 1,3-butadiene, 0.015 g of ferrous sulfate, and 0.08 g of ammonium persulfate were added at 35° C. and reacted for 1.5 h to obtain a copolymer B with a weight average molecular weight of 35686;

[0043] (3) adding 30 g of copolymer B to 100 g of copolymer A at a rate of 450 g / h, and reacting at 35° C. for 7.5 h to obtain a modified nitrile rubber;

[0044] (4) Add 0.5 g of Pd / C to 100 g of the modified nitrile rubber obtained in step (3), introduce hydrogen, the pressure is 5 MPa, react at 60° C. for 2.5 h, filter, add 30 g of 20 wt % CaCl2 to the filtrate, filter, wash and dry to obtain modified hydrogenated nitrile rubber-1.

[0045] Preparation Example 2

[0046] The preparation method of modified hydrogenated nitrile rubber-2 is the same as that of Preparation Example 1, except that the amount of 1,3-butadiene added in step (1) is 48 g.

[0047] Preparation Example 3

[0048] The preparation method of modified hydrogenated nitrile rubber-3 is the same as that of Preparation Example 1, except that the amount of 1,3-butadiene added in step (2) is 20 g.

[0049] Preparation Example 4

[0050] The preparation method of modified hydrogenated nitrile rubber-4 is the same as that of Preparation Example 1, except that the amount of copolymer B added in step (3) is 10 g.

[0051] Preparation Example 5

[0052] The preparation method of hydrogenated nitrile rubber comprises the following steps:

[0053] (1) 300 g of deionized water, 4 g of sodium dodecyl sulfate, 24 g of acrylonitrile, and 0.05 g of disodium ethylenediaminetetraacetate were added to a reaction container, stirred for 20 min, nitrogen was passed through, 31.2 g of 1,3-butadiene, 0.05 g of ferrous sulfate, and 0.25 g of ammonium persulfate were added at 35° C., and the mixture was reacted for 1.5 h to obtain a copolymer A with a weight average molecular weight of 36447;

[0054] (2) 100 g of deionized water, 1.5 g of sodium dodecyl sulfate, and 10 g of acrylonitrile were added to a reaction vessel and stirred for 20 min. The air in the reaction system was removed, and 25 g of 1,3-butadiene, 0.015 g of ferrous sulfate, and 0.08 g of ammonium persulfate were added at 35° C. and reacted for 1.5 h to obtain a copolymer B with a weight average molecular weight of 35586;

[0055] (3) adding 30 g of copolymer B to 100 g of copolymer A at a rate of 450 g / h, and reacting at 35° C. for 7.5 h to obtain a modified nitrile rubber;

[0056] (4) Add 0.5 g of Pd / C to 100 g of the modified nitrile rubber obtained in step (3), introduce hydrogen, the pressure is 5 MPa, react at 60° C. for 2.5 h, filter, add 30 g of 20 wt % CaCl 2 to the filtrate, filter, wash and dry to obtain hydrogenated nitrile rubber.

[0057] Preparation Example 6

[0058] The preparation method of vulcanizing agent-1 comprises the following steps:

[0059] 1) adding 10 g of oxidized resveratrol and 0.03 g of isobutyl peroxide to 50 g of anhydrous ethanol, reacting at 65° C. for 30 min, filtering, washing, and drying to obtain a polymer with a weight average molecular weight of 931;

[0060] 2) 15 g of the polymer obtained in step 1), 10 g of 2-fluoroacrylic acid and 0.15 g of tetraisopropyl titanate were reacted at 75° C. for 5.5 h, filtered, washed and dried to obtain vulcanizing agent 1.

[0061] Preparation Example 7

[0062] The preparation method of vulcanizing agent-2 is the same as that of Preparation Example 7, except that the amount of polymer added in step 2) is 25 g.

[0063] Example 1

[0064] A viscous hydrogenated nitrile rubber comprises the following raw materials, measured in parts by weight: 35 parts of modified hydrogenated nitrile rubber-1, 1.5 parts of sulfur, 2.5 parts of vulcanizing agent-1, 0.8 parts of SA1801, 315 parts of N-methylpyrrolidone and 630 parts of anhydrous ethanol.

[0065] The preparation method of the viscous-fluid hydrogenated nitrile rubber of this embodiment comprises the following steps:

[0066] S1, vulcanization: add modified hydrogenated nitrile rubber-1, sulfur, vulcanizing agent-1, and SA1801 into an open mill and roll together until there is no viscous liquid on the surface of the rubber roll, then add into a vulcanizer for vulcanization, the vulcanization temperature is 148°C, the vulcanization time is 55min, the vulcanization pressure is 13MPa, and the lower sheet is cooled to obtain a vulcanized modified hydrogenated nitrile rubber;

[0067] S2, dissolving: crush the obtained vulcanized modified hydrogenated nitrile rubber into 2 cm particles, add N-methylpyrrolidone, stir at 110 ° C for 60 min under nitrogen protection, filter, and continue to stir the filtrate at 95 ° C for 60 min to obtain material 1;

[0068] S3, dehydration and discharging: material 1 and half amount of anhydrous ethanol are added into the reactor through different pipes at the same time, stirred for 60 minutes at 60°C and pressure of -0.05 KPa, and then the remaining anhydrous ethanol is added, stirred for 60 minutes at 60°C and pressure of 0.05 KPa, cooled to room temperature, and discharged to obtain viscous hydrogenated nitrile rubber.

[0069] Example 2

[0070] A viscous hydrogenated nitrile rubber comprises the following raw materials, measured in parts by weight: 30 parts of modified hydrogenated nitrile rubber-1, 1 part of sulfur, 2 parts of vulcanizing agent-1, 0.5 parts of SA1801, 270 parts of N-methylpyrrolidone and 540 parts of anhydrous ethanol.

[0071] The preparation method of the viscous-fluid hydrogenated nitrile rubber of this embodiment comprises the following steps:

[0072] S1, vulcanization: add modified hydrogenated nitrile rubber-1, sulfur, vulcanizing agent-1, and SA1801 into an open mill and roll together until there is no viscous liquid on the surface of the rubber roll, then add into a vulcanizer for vulcanization, the vulcanization temperature is 145°C, the vulcanization time is 50min, the vulcanization pressure is 10MPa, and the lower sheet is cooled to obtain a vulcanized modified hydrogenated nitrile rubber;

[0073] S2, dissolving: crush the obtained vulcanized modified hydrogenated nitrile rubber into 1 cm particles, add N-methylpyrrolidone, stir at 105 ° C for 55 min under nitrogen protection, filter, and continue to stir the filtrate at 90 ° C for 55 min to obtain material 1;

[0074] S3, dehydration and discharging: material 1 and half amount of anhydrous ethanol are added into the reactor through different pipes at the same time, stirred for 55 minutes at 55° C. and pressure of -0.1 KPa, and then the remaining anhydrous ethanol is added, stirred for 55 minutes at 55° C. and pressure of -0.1 KPa, cooled to room temperature, and discharged to obtain viscous hydrogenated nitrile rubber.

[0075] Example 3

[0076] A viscous hydrogenated nitrile rubber comprises the following raw materials, measured in parts by weight: 40 parts of modified hydrogenated nitrile rubber-1, 2 parts of sulfur, 3 parts of vulcanizing agent-1, 1 part of SA1801, 360 parts of N-methylpyrrolidone and 720 parts of anhydrous ethanol.

[0077] The preparation method of the viscous-fluid hydrogenated nitrile rubber of this embodiment comprises the following steps:

[0078] S1, vulcanization: add modified hydrogenated nitrile rubber-1, sulfur, vulcanizing agent-1, and SA1801 into an open mill and roll together until there is no viscous liquid on the surface of the rubber roll, then add into a vulcanizer for vulcanization, the vulcanization temperature is 150°C, the vulcanization time is 60min, the vulcanization pressure is 15MPa, and the lower sheet is cooled to obtain a vulcanized modified hydrogenated nitrile rubber;

[0079] S2, dissolving: crush the obtained vulcanized modified hydrogenated nitrile rubber into 3 cm particles, add N-methylpyrrolidone, stir at 115 ° C for 65 min under nitrogen protection, filter, and continue to stir the filtrate at 100 ° C for 65 min to obtain material 1;

[0080] S3, dehydration and discharging: material 1 and half amount of anhydrous ethanol are added into the reactor through different pipes at the same time, stirred at 65°C and pressure of 0 KPa for 65 minutes, then the remaining anhydrous ethanol is added, stirred at 65°C and pressure of 0 KPa for 65 minutes, cooled to room temperature, and discharged to obtain viscous hydrogenated nitrile rubber.

[0081] Example 4

[0082] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydrogenated nitrile rubber-1 is replaced by modified hydrogenated nitrile rubber-2.

[0083] Example 5

[0084] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydrogenated nitrile rubber-1 is replaced by modified hydrogenated nitrile rubber-3.

[0085] Example 6

[0086] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydrogenated nitrile rubber-1 is replaced by modified hydrogenated nitrile rubber-4.

[0087] Example 7

[0088] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of vulcanizing agent-1 is replaced by vulcanizing agent-2.

[0089] Comparative Example 1

[0090] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydrogenated nitrile rubber-1 is replaced by hydrogenated nitrile rubber.

[0091] Comparative Example 2

[0092] A viscous hydrogenated nitrile rubber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of vulcanizing agent-1 is replaced by sulfur.

[0093] Performance Testing

[0094] 1. Adhesion test

[0095] The viscous hydrogenated butyronitrile obtained in each embodiment and comparative example is used as a binder to prepare a positive electrode sheet for a lithium ion battery. The preparation method of the positive electrode sheet for a lithium ion battery is as follows: lithium iron phosphate, carbon nanotubes, and a binder are added to N-methylpyrrolidone, wherein the mass ratio of lithium iron phosphate, carbon nanotubes, binder, and N-methylpyrrolidone is 6:2:2:25, and the mixture is ground evenly to obtain a slurry, and the slurry is coated on the surface of an aluminum foil with a coating thickness of 1 mm, and dried at 0.5 MPa and 110°C for 12 hours to obtain a positive electrode sheet. The mixture is placed at a temperature of -20±5°C for 4 hours, and a 180° peel strength test is performed using a Z005 universal tensile testing machine.

[0096] 2. Swelling performance test

[0097] The swelling rate of the binder will affect the conductivity between the active material and the current collector, thereby reducing the battery capacity. The hydrogenated butyronitrile obtained in each embodiment and comparative example is poured into a mold in a viscous flow state to obtain a sample film with a thickness of 1 mm and a weighing mass of m0. The sample film is immersed in an electrolyte with a concentration of 1 mol / L LiPF6 for 72 hours, the surface solvent is wiped off, and the weighing mass is m1. The swelling rate is calculated, and the swelling rate = (m1-m0) / m0×100%.

[0098] 3. Battery performance test

[0099] A lithium sheet was used as the counter electrode, 1 mol / L LiPF6 solution was used as the electrolyte, and the positive electrode sheets were assembled into button cells. The preparation method of the positive electrode sheets was the same as that of the adhesion test.

[0100] (1) Rate performance test

[0101] Tested in electrochemical work: At 25°C, the button cell was charged to 4.2V at a constant current of 0.5C, then discharged at a constant current of 0.5C until the cut-off voltage was 2.5V, and the 0.5C discharge capacity was recorded. The above charging process was repeated, and the battery was charged to 4.2V at a constant current of 2C, and discharged at a constant current of 2C until the cut-off voltage was 2.5V, and the 2C discharge capacity was recorded. Rate performance = 2C discharge capacity / 0.5C discharge capacity × 100%.

[0102] (2) Cyclic performance test

[0103] The button battery was placed in a constant temperature environment of 25°C, charged to 4.2V at a constant current of 0.5C, allowed to stand for 8 hours after full charge, and then discharged to 2.5V at 0.5C. The discharge capacity was recorded as D0. A cycle test was then performed with 0.5C charge / 0.5C discharge for 2000 cycles. The discharge capacity after the 2000th cycle was D1. The cycle capacity retention rate (%) of the lithium-ion battery after 2000 cycles at 25°C = D1 / D0×100%.

[0104] The test results are shown in Table 1.

[0105] Table 1

[0106]

[0107] From the data of Examples 1-3 in Table 1, it can be seen that the ratio of each substance changes, and the viscous hydrogenated nitrile rubber is used as a binder for lithium ion battery positive electrode sheets, which has greater peel strength, lower swelling rate, and good electrochemical performance; Example 4 is compared with Example 1, and it can be seen that the increase in the amount of butadiene may cause the stability of the viscous hydrogenated nitrile rubber to decrease, so that the electrochemical performance of the prepared battery decreases; Example 5 is compared with Example 1, and it can be seen that the mass ratio of N-vinyl-2-pyrrolidone to butadiene in the modified hydrogenated nitrile rubber-3 is changed, which may lead to a decrease in bonding force when used as a binder for lithium ion battery electrode sheets, and a decrease in peel strength and electrochemical performance; Example 6 Compared with Example 1, it can be seen that the amount of copolymer B in modified hydrogenated nitrile rubber-4 is reduced, which may lead to a decrease in the solubility of the modified hydrogenated nitrile rubber in the solvent, thereby reducing the electrochemical performance; compared with Example 1, Example 7 shows that the mass ratio of the polymer to 2-fluoroacrylic acid in the vulcanizing agent-2 is changed, resulting in an increase in the active sites of the viscous hydrogenated nitrile rubber and a decrease in the electrochemical performance; in Comparative Example 1, the modified hydrogenated nitrile rubber-1 is replaced by hydrogenated nitrile rubber in equal amounts, and the peel strength and electrochemical performance are reduced; in Comparative Example 2, sulfur is used as the vulcanizing agent, and it is possible that sulfur reacts with substances in the electrolyte solution, resulting in a decrease in electrochemical inertness, thereby causing a decrease in electrochemical performance.

[0108] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A viscous hydrogenated nitrile rubber, characterized in that: The invention comprises the following raw materials in parts by weight: 30-40 parts of modified hydrogenated nitrile rubber, 1-2 parts of sulfur, 2-3 parts of vulcanizing agent, 1-2 parts of vulcanization accelerator, 270-360 parts of solvent and 540-720 parts of dehydrating agent.

2. The viscous-fluid hydrogenated nitrile rubber according to claim 1, characterized in that: The preparation method of the modified hydrogenated nitrile rubber comprises the following steps: (1) adding deionized water, an emulsifier, acrylonitrile, and a chelating agent into a reaction vessel, stirring for 15-25 minutes, removing air from the reaction system, adding butadiene, a reducing agent, and an initiator at 30-40° C., reacting for 1-2 hours, and obtaining a copolymer A having a weight average molecular weight of 30,000-40,000; (2) adding deionized water, an emulsifier, and N-vinyl-2-pyrrolidone into a reaction vessel, stirring for 15-25 minutes, removing air from the reaction system, adding butadiene, a reducing agent, and an initiator at 30-40° C., reacting for 1-2 hours, and obtaining a copolymer B having a weight average molecular weight of 30,000-40,000; (3) adding copolymer B to copolymer A, reacting at 30-40° C. for 7-8 hours to obtain modified nitrile rubber; (4) adding a first catalyst to the modified nitrile rubber obtained in step (3), introducing hydrogen at a pressure of 5-6 MPa, reacting at 55-65° C. for 1-2 h, filtering, adding a flocculant to the filtrate, filtering, washing, and drying to obtain a modified hydrogenated nitrile rubber.

3. The viscous-fluid hydrogenated nitrile rubber according to claim 2, characterized in that: In the step (1), the mass ratio of acrylonitrile to butadiene is 1:(1-1.5).

4. The viscous-fluid hydrogenated nitrile rubber according to claim 2, characterized in that: In the step (2), the mass ratio of N-vinyl-2-pyrrolidone to butadiene is 1:(2-3).

5. The viscous-fluid hydrogenated nitrile rubber according to claim 2, characterized in that: In the step (3), the mass ratio of copolymer A to copolymer B is 1:(0.2-0.4).

6. The viscous-fluid hydrogenated nitrile rubber according to claim 1, characterized in that: The preparation method of the vulcanizing agent comprises the following steps: 1) adding oxidized resveratrol and an initiator to ethanol, reacting at 60-70° C., controlling, filtering, washing, and drying to obtain a polymer with a weight average molecular weight of 800-1100; 2) reacting the polymer obtained in step 1), 2-fluoroacrylic acid and a second catalyst at 70-80° C. for 5-6 hours, filtering, washing and drying to obtain a vulcanizing agent.

7. The viscous-fluid hydrogenated nitrile rubber according to claim 6, characterized in that: In the step 2), the mass ratio of the polymer to 2-fluoroacrylic acid is (1-2):

1.

8. The viscous-fluid hydrogenated nitrile rubber according to claim 1, characterized in that: The solvent is N-methylpyrrolidone.

9. A method for preparing a viscous hydrogenated nitrile rubber according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, vulcanization: adding modified hydrogenated nitrile rubber, sulfur, vulcanizing agent, and vulcanization accelerator to an open mill and rolling together until there is no viscous liquid on the surface of the rubber roll, then adding to a vulcanizer for vulcanization, the vulcanization temperature is 145-150°C, the vulcanization time is 50-60min, the vulcanization pressure is 10MPa-15MPa, and the lower sheet is cooled to obtain a vulcanized modified hydrogenated nitrile rubber; S2, dissolving: crush the obtained vulcanized modified hydrogenated nitrile rubber into 1-3 cm particles, add solvent, stir at 105-115° C. for 55-65 min under nitrogen protection, filter, and continue stirring the filtrate at 90-100° C. for 55-65 min to obtain material 1; S3, dehydration and discharging: add material 1 and part of the dehydrating agent into the reaction kettle respectively, stir for 55-65 minutes at 55-65°C and pressure of -0.1-0KPa, then add the remaining dehydrating agent, continue stirring for 55-65 minutes at 55-65°C and pressure of -0.1-0KPa, cool to room temperature, and discharge to obtain viscous hydrogenated nitrile rubber.

10. Use of the viscous hydrogenated nitrile rubber according to any one of claims 1 to 8 or the viscous hydrogenated nitrile rubber obtained by the preparation method according to claim 9 in the manufacture of lithium battery electrode sheets.

Citation Information

Cited By

  • Guniting material admixture as well as preparation method and application thereof

    CN120328912A

  • A spraying material admixture and its preparation method and application

    CN120328912B