A kind of degradable fruit and vegetable fresh-keeping film and preparation method thereof

By adopting a double-layer film structure and modified hemp fiber processing, the problem of poor film-forming performance and non-degradability of traditional fruit and vegetable cling film has been solved, and a degradable and air-permeable fruit and vegetable cling film has been achieved, which has good antibacterial properties and heavy metal resistance. adsorption effect.

CN114393901BActive Publication Date: 2024-10-22SHANXI TONGXIN CLOTHING NEW MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111526522.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-14
Publication Date
2024-10-22
Estimated Expiration
2041-12-14

AI Technical Summary

Technical Problem

Traditional fruit and vegetable cling film has poor film-forming performance and is not degradable, leading to environmental pollution and poor preservation effect on fruits and vegetables.

Method used

It adopts a double-layer membrane structure. The inner membrane is made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer. The outer membrane is made of polylactic acid, polyadipate-terephthalate. Made of butylene terephthalate, modified starch and compatibilizer, the modified hemp fiber is treated with coupling agent and green onion extract to enhance breathability and antibacterial properties.

Benefits of technology

The air permeability and antibacterial properties of the degradable fruit and vegetable cling film have been achieved, which can effectively prevent fruits and vegetables from rotting, reduce the consumption of nutrients, and have good heavy metal adsorption capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114393901B_ABST
    Figure CN114393901B_ABST
Patent Text Reader

Abstract

The invention discloses a degradable fruit and vegetable fresh-keeping film and a preparation method thereof, comprising an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of the polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is (45 The weight ratio of polylactic acid, polybutylene adipate terephthalate, modified starch and compatibilizer in the outer film is (45-65): (20-35): (5-20): (1-5). The fruit and vegetable fresh-keeping film has a double-layer film structure, is biodegradable, has good air permeability, has a certain adsorption effect on heavy metals, has good antibacterial properties, can effectively prevent bacteria in the air from entering, and prevent fruits and vegetables from rotting and deteriorating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fruit and vegetable fresh-keeping films, and in particular to a degradable fruit and vegetable fresh-keeping film and a preparation method thereof. Background Art

[0002] Traditional plastic bags and cling films are mostly made of polyethylene, which has poor biocompatibility and is non-degradable. When discharged into the environment, it causes serious white pollution. Incineration will produce highly toxic dioxins, which pollute the atmosphere and harm the growth of animals and plants. In addition, the amount of white garbage in the ocean is increasing year by year, which has caused harm to marine life. Non-degradable products will gradually be replaced by degradable products.

[0003] The surface of hemp fiber is rough, with many cracks and holes, and a central cavity, which forms an interwoven fiber network with the side wall holes. However, its film-forming property is poor. After modification, its air permeability can be enhanced, and it has a better adsorption effect on heavy metal ions on the surface of fruits and vegetables.

[0004] Polylactic acid, as a biopolymer material derived from corn starch, has excellent mechanical properties, biocompatibility and degradability, is easy to process and shape, has high transparency, is safe and hygienic, and can be completely degraded into water and carbon dioxide in the soil. It is an environmentally friendly raw material. However, polylactic acid is relatively expensive and has disadvantages such as high brittleness and poor toughness, which affect the large-scale promotion and use of polylactic acid. Therefore, the applicant conducted further research on the current situation and adopted different methods to deal with it. Summary of the invention

[0005] The first technical problem to be solved by the present invention is to provide a degradable fruit and vegetable cling film, which has a double-layer film structure, is degradable, has good air permeability, has a certain adsorption effect on heavy metals, has good antibacterial properties, can effectively prevent bacteria in the air from entering, and prevents fruits and vegetables from rotting and deteriorating, thereby solving the problems of poor film-forming performance, difficult film blowing and non-degradability of traditional fruit and vegetable cling films.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing a degradable fruit and vegetable cling film. The method is simple and easy to operate, can be promoted on a large scale, and the prepared fruit and vegetable cling film is degradable, has good air permeability, has a certain adsorption effect on heavy metals, and has good antibacterial properties.

[0007] To solve the above-mentioned first technical problem, the technical solution of the present invention is: a degradable fruit and vegetable fresh-keeping film, comprising an inner film and an outer film, the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch, and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer in the inner film is (45-65): (20-35): (5-20): (1-5), and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer in the outer film is (45-65): (20-35): (5-20): (1-5).

[0008] Preferably, the modified hemp fiber is prepared by treating hemp fiber, a coupling agent and green onion extract. First, the hemp fiber is rinsed, dried and crushed, a coupling agent is added, and the fiber is treated in a high-speed mixer. Then, the green onion extract is added and heated to obtain the modified hemp fiber. The green onion extract is obtained by crushing the green onion and then heating and refluxing it with ethanol having a mass concentration of 95%. The obtained extract is subjected to rotary evaporation to remove the ethanol, thereby obtaining an oily substance without alcohol taste, namely the green onion extract.

[0009] Preferably, the mass ratio of hemp fiber, coupling agent and green onion extract is 100:(1-5):(1-5).

[0010] Preferably, the hemp fiber is one or more of flax fiber, apocynum fiber and sisal fiber.

[0011] Preferably, the hemp fiber is rinsed with 30% by mass H2O2 at 60°C for 2h, vacuum dried, crushed into 1000 mesh, a coupling agent is added, and heated at 100°C in a high-speed mixer for 20min, and then the green onion extract is added and heated for 5min to obtain the modified hemp fiber; the green onion extract is prepared by crushing the green onions and then heating and refluxing them with 95% by mass ethanol at 85°C for 2h, and the obtained extract is subjected to rotary evaporation to remove the ethanol to obtain an oily substance without alcohol taste.

[0012] Preferably, the coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent.

[0013] Preferably, the modified starch is prepared by processing corn starch and glycerol, and the mass ratio of corn starch to glycerol is 100:30.

[0014] Preferably, the compatibilizer is one of maleic anhydride, epoxidized soybean oil and stearic acid.

[0015] After adopting the above-mentioned first technical scheme, the effect of the present invention is as follows: a degradable fruit and vegetable fresh-keeping film includes an inner film and an outer film, the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch, and a compatibilizer. The modified hemp fiber contained has a porous structure, a rough surface, many cracks and holes, a middle cavity, and a fiber network interwoven and interconnected with the side wall holes. The air permeability is good, and the carbon dioxide generated by respiration can be effectively prevented from being discharged from the outside of the film and the oxygen outside the film can be prevented from entering, thereby reducing the respiration of fruits and vegetables, thereby reducing the consumption of nutrients, and the mechanical properties are good, and there is a certain adsorption effect on heavy metals.

[0016] In addition, the modified hemp fiber contains green onion extract, which has good antibacterial properties and can effectively prevent the entry of bacteria in the air and prevent fruits and vegetables from rotting and spoiling, so as to better achieve the preservation effect. The structural design of the inner membrane can effectively prevent the volatilization of green onion extract.

[0017] In order to solve the above second technical problem, the technical solution of the present invention is: a method for preparing a degradable fruit and vegetable cling film, comprising the following steps:

[0018] 1) Preparation of green onion extract: Crush the green onion and use 95% ethanol at 85° C. to perform water bath reflux extraction for 2 h, then put the obtained extract into a rotary evaporator and perform reduced pressure rotary evaporation to remove the ethanol, and obtain an oily substance without alcohol taste, which is the green onion extract;

[0019] 2) Preparation of modified hemp fiber: After the hemp fiber was rinsed with 30% by mass H2O2 at 60°C for 2h, it was vacuum dried at 50°C, and then crushed into 1000 mesh hemp fiber. A certain amount of the crushed hemp fiber was added with a coupling agent, heated at 100°C in a high-speed mixer for 20min, and then the green onion extract was added and continued to heat for 5min to obtain the modified hemp fiber;

[0020] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0021] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation respectively, the granulation temperature of the inner layer film is 165-190°C, and the granulation temperature of the outer layer film is 160-190°C. Then, the double-layer co-extrusion blown film is used to prepare the degradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 165-180°C.

[0022] Preferably, the granulation temperature of the inner layer film is 180°C, the granulation temperature of the outer layer film is 180°C, the film blowing temperature is 180°C, and the reduced pressure rotary evaporation temperature is 65°C.

[0023] After adopting the above second technical scheme, the effect of the present invention is: a method for preparing a degradable fruit and vegetable cling film, the method is simple and easy to operate, and can be promoted on a large scale. The fruit and vegetable cling film prepared by the method is degradable, has good air permeability, has a certain adsorption effect on heavy metals, and has good antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention is further described below with reference to the accompanying drawings and embodiments.

[0025] Figure 1 It is a schematic diagram of the weight loss rate of apple;

[0026] Figure 2 It is a schematic diagram of the weight loss rate of cabbage; DETAILED DESCRIPTION

[0027] The present invention is further described in detail below through specific examples.

[0028] Example 1

[0029] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is 65:20:20:3, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 45:30:20:3.

[0030] In this embodiment, the modified hemp fiber is prepared by treating hemp fiber, a coupling agent, and green onion extract, the modified starch is prepared by treating corn starch and glycerol, the mass ratio of hemp fiber, coupling agent, and green onion extract is 100:1:5, and the compatibilizer is stearic acid.

[0031] The hemp fiber is one or more of flax fiber, apocynum fiber, and sisal fiber. In this embodiment, flax fiber is selected.

[0032] The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. In this embodiment, the aluminate coupling agent is selected.

[0033] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0034] 1) Preparation of green onion extract: Select Zhangqiu green onion, crush the Zhangqiu green onion, and then use 95% ethanol at 85°C for 2h in a water bath for heating and reflux extraction. Then put the obtained extract into a rotary evaporator, and remove the ethanol by rotary evaporation at 65°C to obtain an oily substance without alcohol taste, which is the green onion extract;

[0035] 2) Preparation of modified hemp fiber: After rinsing the flax fiber with 30% by mass of H2O2 at 60°C for 2h, the flax fiber is vacuum dried in a vacuum drying oven at 50°C, and then crushed into 1000 mesh flax fiber with an ultrafine grinder. A certain amount of the crushed flax fiber is taken, a coupling agent is added, and the mixture is heated at 100°C in a high-speed mixer for 20min, and then the green onion extract in step 1) is added, and the heating treatment is continued for 5min to obtain the modified hemp fiber;

[0036] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0037] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation, the granulation temperature of the inner layer film is 165°C, and the granulation temperature of the outer layer film is 160°C. Then, the double-layer co-extrusion blown film is used to prepare the degradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 170°C.

[0038] Example 2

[0039] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is 45:35:5:1, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 60:20:5:1.

[0040] In this embodiment, the modified hemp fiber is prepared by treating hemp fiber, a coupling agent, and green onion extract, the modified starch is prepared by treating corn starch and glycerol, the mass ratio of hemp fiber, coupling agent, and green onion extract is 100:5:3, and the compatibilizer is stearic acid.

[0041] The hemp fiber is one or more of flax fiber, apocynum fiber, and sisal fiber. In this embodiment, flax fiber is selected.

[0042] The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. In this embodiment, the aluminate coupling agent is selected.

[0043] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0044] 1) Preparation of green onion extract: Select Zhangqiu green onion, crush the Zhangqiu green onion, and then use 95% ethanol at 85°C for 2h in a water bath for heating and reflux extraction. Then put the obtained extract into a rotary evaporator, and remove the ethanol by rotary evaporation at 65°C to obtain an oily substance without alcohol taste, which is the green onion extract;

[0045] 2) Preparation of modified hemp fiber: After rinsing the flax fiber with 30% by mass of H2O2 at 60°C for 2h, the flax fiber is vacuum dried in a vacuum drying oven at 50°C, and then crushed into 1000 mesh flax fiber with an ultrafine grinder. A certain amount of the crushed flax fiber is taken, a coupling agent is added, and the mixture is heated at 100°C in a high-speed mixer for 20min, and then the green onion extract in step 1) is added, and the heating treatment is continued for 5min to obtain the modified hemp fiber;

[0046] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0047] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation, the granulation temperature of the inner layer film is 190°C, and the granulation temperature of the outer layer film is 190°C. Then, the double-layer co-extrusion blown film is used to prepare the biodegradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 165°C.

[0048] Example 3

[0049] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is 55:30:10:5, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 50:35:10:5.

[0050] In this embodiment, the modified hemp fiber is made by treating hemp fiber, a coupling agent, and green onion extract, the modified starch is made by treating corn starch and glycerol, the mass ratio of hemp fiber, coupling agent, and green onion extract is 100:4:3, and the compatibilizer is epoxidized soybean oil.

[0051] The hemp fiber is one or more of flax fiber, apocynum fiber, and sisal fiber. In this embodiment, flax fiber is selected.

[0052] The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. In this embodiment, the aluminate coupling agent is selected.

[0053] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0054] 1) Preparation of green onion extract: Select Zhangqiu green onion, crush the Zhangqiu green onion, and then use 95% ethanol at 85°C for 2h in a water bath for heating and reflux extraction. Then put the obtained extract into a rotary evaporator, and remove the ethanol by rotary evaporation at 65°C to obtain an oily substance without alcohol taste, which is the green onion extract;

[0055] 2) Preparation of modified hemp fiber: After rinsing the flax fiber with 30% by mass of H2O2 at 60°C for 2h, the flax fiber is vacuum dried in a vacuum drying oven at 50°C, and then crushed into 1000 mesh flax fiber with an ultrafine grinder. A certain amount of the crushed flax fiber is taken, a coupling agent is added, and the mixture is heated at 100°C in a high-speed mixer for 20min, and then the green onion extract in step 1) is added, and the heating treatment is continued for 5min to obtain the modified hemp fiber;

[0056] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0057] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation respectively, the granulation temperature of the inner layer film is 180°C, and the granulation temperature of the outer layer film is 180°C. Then, the double-layer co-extrusion blown film is used to prepare the biodegradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 180°C.

[0058] Example 4

[0059] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is 50:30:15:3, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 65:35:15:5.

[0060] In this embodiment, the modified hemp fiber is prepared by treating hemp fiber, a coupling agent, and green onion extract, the modified starch is prepared by treating corn starch and glycerol, the mass ratio of hemp fiber, coupling agent, and green onion extract is 100:3:1, and the compatibilizer is maleic anhydride.

[0061] The hemp fiber is one or more of flax fiber, apocynum fiber, and sisal fiber. In this embodiment, flax fiber is selected.

[0062] The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. In this embodiment, the aluminate coupling agent is selected.

[0063] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0064] 1) Preparation of green onion extract: Select Zhangqiu green onion, crush the Zhangqiu green onion, and then use 95% ethanol at 85°C for 2h in a water bath for heating and reflux extraction. Then put the obtained extract into a rotary evaporator, and remove the ethanol by rotary evaporation at 65°C to obtain an oily substance without alcohol taste, which is the green onion extract;

[0065] 2) Preparation of modified hemp fiber: After rinsing the flax fiber with 30% by mass of H2O2 at 60°C for 2h, the flax fiber is vacuum dried in a vacuum drying oven at 50°C, and then crushed into 1000 mesh flax fiber with an ultrafine grinder. A certain amount of the crushed flax fiber is taken, a coupling agent is added, and the mixture is heated at 100°C in a high-speed mixer for 20min, and then the green onion extract in step 1) is added, and the heating treatment is continued for 5min to obtain the modified hemp fiber;

[0066] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0067] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation, the granulation temperature of the inner layer film is 180°C, and the granulation temperature of the outer layer film is 170°C. Then, the double-layer co-extrusion blown film is used to prepare the biodegradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 180°C.

[0068] Example 5

[0069] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and the compatibilizer in the inner film is 55:20:15:5, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 50:30:20:5.

[0070] In this embodiment, the modified hemp fiber is prepared by treating hemp fiber, a coupling agent, and green onion extract, the modified starch is prepared by treating corn starch and glycerol, the mass ratio of hemp fiber, coupling agent, and green onion extract is 100:3:5, and the compatibilizer is maleic anhydride.

[0071] The hemp fiber is one or more of flax fiber, apocynum fiber, and sisal fiber. In this embodiment, flax fiber is selected.

[0072] The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. In this embodiment, the aluminate coupling agent is selected.

[0073] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0074] 1) Preparation of green onion extract: Select Zhangqiu green onion, crush the Zhangqiu green onion, and then use 95% ethanol at 85°C for 2h in a water bath for heating and reflux extraction. Then put the obtained extract into a rotary evaporator, and remove the ethanol by rotary evaporation at 65°C to obtain an oily substance without alcohol taste, which is the green onion extract;

[0075] 2) Preparation of modified hemp fiber: After rinsing the flax fiber with 30% by mass of H2O2 at 60°C for 2h, the flax fiber is vacuum dried in a vacuum drying oven at 50°C, and then crushed into 1000 mesh flax fiber with an ultrafine grinder. A certain amount of the crushed flax fiber is taken, a coupling agent is added, and the mixture is heated at 100°C in a high-speed mixer for 20min, and then the green onion extract in step 1) is added, and the heating treatment is continued for 5min to obtain the modified hemp fiber;

[0076] 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 minutes in a high-speed mixer to obtain modified starch;

[0077] 4) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation, the granulation temperature of the inner layer film is 175°C, and the granulation temperature of the outer layer film is 175°C. Then, the double-layer co-extrusion blown film is used to prepare the biodegradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 170°C.

[0078] Comparative Example 1

[0079] In this comparative example 1, the modified hemp fiber is not added to the inner film material of the cling film, and the rest is basically the same as that of Examples 1-5.

[0080] A degradable fruit and vegetable fresh-keeping film comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate and the compatibilizer in the inner film is 55:30:5, and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and the compatibilizer in the outer film is 50:35:10:5.

[0081] The modified starch is made by processing corn starch with glycerol, and the compatibilizer is epoxidized soybean oil.

[0082] The coupling agent is an aluminate coupling agent.

[0083] The preparation method of the above-mentioned degradable fruit and vegetable cling film comprises the following steps:

[0084] 1) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 min in a high-speed mixer to obtain modified starch;

[0085] 2) Double-layer co-extrusion blown film: the raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, and a compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and a compatibilizer. After granulation, the granulation temperature of the inner layer film is 180°C, and the granulation temperature of the outer layer film is 180°C. Then, the double-layer co-extrusion blown film is used to prepare the degradable fruit and vegetable fresh-keeping film, and the film blowing temperature is 180°C.

[0086] 1. Mechanical properties test results

[0087] The samples prepared in each embodiment and comparative example were cut into rectangular strips of 15 mm*150 mm and tested using a universal testing machine at a test speed of 200 mm / min. The cling films prepared in embodiments 1 to 5 and comparative example 1 were tested for mechanical properties, and the results are shown in Table 1 below.

[0088] Table 1 Mechanical properties test results

[0089]

[0090]

[0091] As shown in Table 1, the tensile strength and elongation at break of the fruit and vegetable cling film prepared in Examples 1 to 5 are improved compared with the cling film prepared in Comparative Example 1, wherein the tensile strength in Example 3 is improved by 28% and the elongation at break is improved by 6%, indicating that the fruit and vegetable cling film of the present invention has better mechanical properties.

[0092] 2. Antibacterial effect

[0093] Staphylococcus aureus and Escherichia coli were used as the test bacteria to test the antibacterial effects of the vegetable cling film prepared in Examples 1-5 and the fruit and vegetable cling film prepared in Comparative Example 1 on the test bacteria. 6 CFU / ml of Staphylococcus aureus and Escherichia coli were evenly coated on the agar medium with a sterile glass rod. When the bacterial solution was completely spread, a film with a diameter of 0.5 cm was cut with a sterilized puncher and placed in the center of the medium. The culture dish was inverted and cultured at 37°C for 24 hours, and the diameter of the inhibition zone was measured. The results are shown in Table 2.

[0094] Table 2 Antibacterial effect test

[0095]

[0096] It can be seen from the diameters of the inhibition zones in Table 2 that the diameters of the inhibition zones in Examples 1 to 5 are significantly larger than those in Comparative Example 1, and the antibacterial effect of Comparative Example 1 is almost 0, indicating that the addition of modified hemp fiber in Examples 1 to 5 can significantly enhance the antibacterial effect.

[0097] 3. Heavy metal adsorption test results

[0098] Choose no heavy metal Cu 2+ and Pb 2+ apples were used as test materials and smeared with 1 mg / L Cu 2+ and Pb 2+ 0.5 ml of the standard solution was placed for 2 hours, and then the cling film prepared in Examples 1-5 and the cling film prepared in Comparative Example 1 were respectively used to wrap the surface of the apple. After 24 hours, the fruit and vegetable cling film was removed, and the heavy metal content of the apple and the fruit and vegetable cling film was determined by atomic absorption spectrophotometry. Heavy metal removal rate (%) = (total heavy metal content of fruits and vegetables - adsorption amount of fruit and vegetable cling film) / total heavy metal content of fruits and vegetables * 100%. The results are shown in Table 3 below.

[0099] Table 3 Results of heavy metal adsorption tests

[0100]

[0101] It can be seen from Table 3 that the fruit and vegetable fresh-keeping films prepared in Examples 1 to 5 have an effect on Cu 2+ and Pb 2+ It has a good adsorption effect. The degradable fruit and vegetable fresh-keeping film prepared in Example 3 has an adsorption effect of 55% on heavy metal ions, and has a good effect of removing heavy metals on the surface of fruits and vegetables.

[0102] 4. Freshness preservation test results

[0103] Apple and cabbage were selected as test materials, and the fruit and vegetable cling film prepared in Examples 1-5 and the fruit and vegetable cling film prepared in Comparative Example 1 were respectively wrapped around fresh apples and cabbages, tightly wrapped in 2 layers, and stored at 0-4°C. The weight of the fruits and vegetables was weighed every 2 days, and the weight loss rate was calculated. Weight loss rate (%) = (original weight - residual weight) / original weight * 100%. The results are shown in the attached Figure 1 and attached Figure 2 .

[0104] As can be seen from the figure, the fruit and vegetable cling film prepared in Examples 1-5 has a better preservation effect than the fruit and vegetable cling film prepared in Comparative Example 1, and can effectively regulate the permeation of carbon dioxide and oxygen, reduce the respiration of fruits and vegetables, and reduce the consumption of nutrients and the loss of water.

[0105] The above-described embodiments are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Various modifications and alterations to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the scope of protection defined by the claims of the present invention.

Claims

1. A degradable fruit and vegetable cling film, characterized in that: The invention comprises an inner film and an outer film, wherein the raw materials of the inner film are made of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer, and the raw materials of the outer film are made of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer, wherein the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber and a compatibilizer in the inner film is (45-65): (20-35): (5-20): (1-5), and the mass ratio of polylactic acid, polybutylene adipate-terephthalate, modified starch and a compatibilizer in the outer film is (45-65): (20- 35): (5-20): (1-5), the modified hemp fiber is prepared by treating hemp fiber, a coupling agent, and a green onion extract. The hemp fiber is rinsed with 30% by mass H2O2 at 60°C for 2 hours, vacuum dried at 50°C, crushed into 1000 mesh, added with a coupling agent, heated at 100°C in a high-speed mixer for 20 minutes, and then added with the green onion extract and heated for 5 minutes to obtain the modified hemp fiber; the green onion extract is prepared by crushing the green onion and then heating and refluxing it at 85°C with 95% by mass ethanol for 2 hours, and then the obtained extract is subjected to rotary evaporation to remove the ethanol to obtain an oily substance without alcohol taste. The mass ratio of the hemp fiber, the coupling agent and the green onion extract is 100:(1-5):(1-5), The coupling agent is one or both of an aluminate coupling agent and a titanate coupling agent. The modified starch is prepared by processing corn starch and glycerol, and the mass ratio of corn starch to glycerol is 100:

30.

2. A degradable fruit and vegetable cling film as claimed in claim 1, characterized in that: The hemp fiber is one or more of flax fiber, apocynum fiber and sisal fiber.

3. The degradable fruit and vegetable cling film according to claim 1, characterized in that: The compatibilizer is one of maleic anhydride, epoxidized soybean oil and stearic acid.

4. The method for preparing a degradable fruit and vegetable cling film according to claim 1, characterized in that: The following steps are involved: 1) Preparation of green onion extract: Crush the green onion and use 95% ethanol at 85°C for 2 h in a water bath for reflux extraction. Then, place the obtained extract in a rotary evaporator and perform reduced pressure rotary evaporation to remove the ethanol. The obtained oily substance without alcohol taste is the green onion extract. 2) Preparation of modified hemp fiber: After the hemp fiber was rinsed with 30% by mass H2O2 at 60°C for 2h, it was vacuum dried at 50°C and then crushed into 1000 mesh hemp fiber. After adding coupling agent to the crushed hemp fiber, it was heated at 100°C in a high-speed mixer for 20min, and then the green onion extract was added and continued to heat for 5min to obtain the modified hemp fiber; 3) Preparation of modified starch: corn starch and glycerol were mixed in a mass ratio of 100:30 and heated at 90°C for 15 min in a high-speed mixer to obtain modified starch; 4) Double-layer co-extrusion blown film: The raw materials of the inner layer film are polylactic acid, polybutylene adipate-terephthalate, modified hemp fiber, and compatibilizer; the raw materials of the outer layer film are polylactic acid, polybutylene adipate-terephthalate, modified starch, and compatibilizer. After granulation respectively, the granulation temperature of the inner layer film is 165~190℃, and the granulation temperature of the outer layer film is 160~190℃. Then, the double-layer co-extrusion blown film is used to prepare the biodegradable fruit and vegetable cling film, and the film blowing temperature is 165~180℃.

5. The method for preparing a degradable fruit and vegetable cling film according to claim 4, characterized in that: The granulation temperature of the inner layer film was 180°C, the granulation temperature of the outer layer film was 180°C, the film blowing temperature was 180°C, and the reduced pressure rotary evaporation temperature was 65°C.

Citation Information

Patent Citations

  • Hydrophobic polylactic acid and starch compound fully-degradable plastic film and manufacturing method thereof

    CN105968745A

  • Degradable preservative film containing onion extract and preparation method thereof

    CN109181180A

  • High-barrier degradable biaxially oriented film and preparation method thereof

    CN112606511A

  • Biodegradable two-way stretching composite film and preparation method and application thereof

    CN113500769A

  • Biodegradable plastic film and preparation method thereof

    CN113754992A