A method for evaluating the long-term migration performance of oil recovery polymers in formations

By shearing the polymer solution and using cores to simulate oil displacement, the problem of unstable long-term migration performance changes of the polymer in the formation is solved, accurate performance monitoring and simulation under low pressure is achieved, and the oil displacement efficiency of the oil field is improved. .

CN114397228BActive Publication Date: 2024-10-18SOUTHWEST PETROLEUM UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210067502.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-20
Publication Date
2024-10-18
Estimated Expiration
2042-01-20

AI Technical Summary

Technical Problem

During the polymer flooding process, the performance changes of the polymer solution are unstable after long-term migration in the oil layer, resulting in a decrease in displacement pressure and oil displacement efficiency. The injection pressure of the existing simulation method is too high and the performance changes cannot be monitored in real time.

Method used

After shearing the polymer solution, multiple or single cores are used to simulate oil displacement, and the performance of each effluent is evaluated to evaluate the performance changes of the polymer during long-term migration in the formation, avoiding the need for long core simulations. The problem of excessive injection pressure during the process can be solved, and performance changes can be monitored at any time.

Benefits of technology

It achieves accurate simulation of long-term migration of polymers in formations, provides theoretical guidance for oilfield polymer injection sites, improves oil displacement efficiency and recovery, and avoids the problem of excessive injection pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003480755260000031
    Figure BDA0003480755260000031
  • Figure BDA0003480755260000061
    Figure BDA0003480755260000061
  • Figure FDA0004948471650000021
    Figure FDA0004948471650000021
Patent Text Reader

Abstract

The invention discloses a method for evaluating the long-term migration performance of a polymer for oil displacement in a formation. The method comprises the following steps: firstly shearing a polymer solution and keeping it for later use; then passing the polymer solution through a plurality of cores to simulate the long-term migration of the polymer for oil displacement in a formation, evaluating the performance of the effluent from each core, thereby evaluating and determining the performance of the polymer for oil displacement in the long-term migration process; or passing the polymer solution through a single core for multiple times to simulate the long-term migration of the polymer for oil displacement in a formation, evaluating the performance of the effluent from each core, thereby evaluating the performance of the polymer for oil displacement in the long-term migration process. The two methods for simulating the long-term migration of the polymer for oil displacement in a formation disclosed by the invention avoid the problem of excessive injection pressure in the long core simulation process, and can monitor the performance change of the polymer at any time, have good application prospects, can effectively simulate the long-term migration of the polymer for oil displacement in a formation, and provide theoretical guidance for the polymer injection site in an oil field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oil and gas field development, and in particular to a method for evaluating the long-term migration performance of an oil recovery polymer in a formation. Background Art

[0002] In the polymer flooding process, after the polymer solution is injected into the oil layer, the viscosity of the displacement phase is increased and the performance-stabilized polymer is retained in the pores of the oil layer, causing the permeability of the oil layer to decrease, thereby controlling the mobility of the water phase, improving the water-oil mobility ratio and adjusting the water absorption profile, and increasing the interlayer sweep coefficient, thereby achieving the purpose of improving the recovery rate. However, due to the influence of long-term migration in the formation after high-speed shear in the near-wellbore area, the performance of the polymer solution will change, and the mobility control ability in the porous medium will be weakened, thereby affecting the displacement pressure, water content and oil recovery efficiency, etc., resulting in the failure of polymer flooding to achieve the expected effect.

[0003] Therefore, it is necessary to propose a method to characterize the long-term migration of polymers in formations, simulate the long-term migration process of polymers in formations, and analyze and evaluate the performance changes of polymers after long-term migration, which is the only way to improve the effect of polymer flooding. However, the current method of simulating the long-term migration of formations by splicing short cores of polymers into long cores or filling and compacting long cores of sand filling tubes with cuttings shows strong water sensitivity, resulting in excessive injection pressure, and the performance changes of polymers cannot be monitored at any time during the process. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for evaluating the long-term migration performance of an oil-displacing polymer in a formation. The method comprises the following steps: firstly shearing a polymer solution and setting it aside; then passing the polymer solution through a plurality of cores to simulate the long-term migration of the oil-displacing polymer in a formation, evaluating the performance of the effluent from each core, thereby evaluating and determining the performance of the oil-displacing polymer in the long-term migration process of the formation; or passing the polymer solution through a single core for multiple times to simulate the long-term migration of the oil-displacing polymer in a formation, evaluating the performance of the effluent from each core, thereby evaluating the performance of the oil-displacing polymer in the long-term migration process of the formation; the two methods for simulating the long-term migration of the oil-displacing polymer in a formation disclosed by the present invention avoid the problem of excessive injection pressure in the long core simulation process, and can monitor the performance change of the polymer at any time, have good application prospects, can effectively simulate the long-term migration of the oil-displacing polymer in a formation, and provide theoretical guidance for the oil field polymer injection site.

[0005] In order to achieve the above technical effects, the following technical solutions are adopted:

[0006] A method for evaluating the long-term migration performance of an oil displacement polymer in a formation comprises the following steps:

[0007] Step S1: The polymer solution to be tested is first sheared by a shear simulation device, and the polymer solution is collected for later use after the performance is stable;

[0008] Step S2: The sheared solution obtained in step S1 is passed through a single core multiple times to simulate the long-term migration of the oil recovery polymer in the formation, and the performance of the core outflow liquid each time is evaluated, thereby evaluating the performance of the oil recovery polymer during the long-term migration process in the formation.

[0009] Furthermore, in step S2, the performance of the oil recovery polymer during long-term migration in the formation is evaluated by passing the sheared solution obtained in step S1 through multiple cores to simulate the long-term migration of the oil recovery polymer in the formation, and evaluating the performance of the effluent from each core, thereby evaluating and determining the performance of the oil recovery polymer during long-term migration in the formation.

[0010] Furthermore, in step S1, the specific steps of shearing the polymer solution to be tested by a shearing device are as follows:

[0011] Step S11: preparing a polymer solution of required concentration, filling a core according to the porosity and permeability of the target formation, connecting a shear simulation device and connecting a pipeline;

[0012] Step S12: adding the polymer solution into the intermediate container, setting the injection pump flow rate, starting the injection pump, and performing a shear experiment;

[0013] Step S13: measuring the viscosity of the polymer solution after shearing, and collecting it for later use after the viscosity remains unchanged.

[0014] Furthermore, the shear simulation device in step S1 includes: an injection pump, a sand filling pipe or a core, a core holder, an intermediate container, a liquid storage tank, a pipeline and an oven.

[0015] Furthermore, in step S12, the injection pump flow rate is determined according to the actual polymer shear rate.

[0016] Furthermore, in step S2, the sheared solution is passed through a single core multiple times to simulate the long-term migration of the oil recovery polymer in the formation, and the performance of the core outflow liquid is evaluated each time, thereby evaluating the performance of the oil recovery polymer in the long-term migration process of the formation. The specific method is:

[0017] Step S21: Select a certain diameter A core with a length L and a permeability equal to the permeability K1 of the formation near the wellbore is placed in a core holder, connected to an intermediate container, a pipeline and saturated with water;

[0018] Step S22: adding the sheared polymer to the intermediate container and starting the injection pump;

[0019] Step S23: measuring the viscosity of the polymer output fluid at the core outlet, collecting the polymer output fluid after the viscosity stabilizes, recording the flow rate Q, time t, and measuring the viscosity μ of the outflow fluid;

[0020] Step S24, calculate the core permeability K after the viscosity of the output fluid is stabilized, and compare it with the target formation permeability K2. If it is greater than the target formation permeability K2, loop steps S22 and S23 until the core permeability is less than the target formation permeability K2, and collect the polymer output fluid, which is the target polymer test fluid; if it is less than or equal to the target formation permeability K2, collect the polymer output fluid as the target polymer test fluid, and calculate the actual migration distance of the polymer.

[0021] Furthermore, the method for calculating the permeability in step S24 is Darcy's formula:

[0022]

[0023] The actual migration distance of the polymer is L 实 =L*n 实 , where n 实 is the actual number of polymer injection cycles, and L is the core length.

[0024] Furthermore, the specific method of passing the sheared solution through multiple cores to simulate the long-term migration of the oil displacement polymer in the formation, evaluating the performance of the effluent from each core, and thus evaluating and determining the performance of the oil displacement polymer in the long-term migration process of the formation is:

[0025] Step S31: comparing the permeability K1 of the near-wellbore zone and the permeability K2 of the target formation, and selecting a moderate permeability gradient ΔK;

[0026] Step S32: Select a certain length L and a certain diameter The core with permeability equal to the near-wellbore zone permeability K1 is placed in the core holder, connected to the intermediate container, pipeline and saturated with water, the sheared polymer is added to the intermediate container and the injection pump is started;

[0027] Step S33: measuring the viscosity of the polymer output liquid at the core outlet, and collecting the polymer output liquid for standby use after the viscosity stabilizes;

[0028] Step S34: Replace the core with a permeability of K=K1+ΔK, and repeat steps S32 and S33 until the last core has a permeability of K=K2. The polymer output liquid collected before each core replacement is the target polymer test liquid.

[0029] Furthermore, in step S34, the number of cores is changed Actual polymer migration distance L 实=L*n, where n is the number of cores with actual polymer migration and L is the core length.

[0030] Furthermore, any one method may be selected to evaluate the long-term migration performance of the oil recovery polymer in the formation, or both methods may be used simultaneously for verification and evaluation.

[0031] The beneficial effects of the present invention are:

[0032] The invention provides a method for evaluating the long-term migration performance of an oil-displacing polymer in a formation. The method comprises the following steps: firstly shearing a polymer solution and keeping it for later use; then passing the polymer solution through a plurality of cores to simulate the long-term migration of the oil-displacing polymer in a formation, evaluating the performance of the effluent from each core, thereby evaluating and determining the performance of the oil-displacing polymer in the long-term migration process of the formation; or passing the polymer solution through a single core for multiple times to simulate the long-term migration of the oil-displacing polymer in a formation, evaluating the performance of the effluent from each core, thereby evaluating the performance of the oil-displacing polymer in the long-term migration process of the formation; the two methods for simulating the long-term migration of the oil-displacing polymer in a formation disclosed by the invention avoid the problem of excessive injection pressure in the long core simulation process, and can monitor the performance change of the polymer at any time, have good application prospects, can effectively simulate the long-term migration of the oil-displacing polymer in a formation, and provide theoretical guidance for the polymer injection site in an oil field.

[0033] The advantages of the present invention are:

[0034] (1) It provides a method for accurately simulating the long-term migration of polymers in formations, providing a reference for the efficient development of polymer injection oil fields.

[0035] (2) The two simulation methods of the present invention avoid the problem of excessive injection pressure in the long core simulation process, and the performance changes of the polymer can be monitored at any time. DETAILED DESCRIPTION

[0036] The present invention is further described below, and the protection scope of the present invention is not limited to the following:

[0037] Example 1

[0038] The data provided by an oil field are shown in Table 1, which discloses the average permeability of the near-well zone and the average permeability of the target formation. The viscosity of the target formation polymer at a concentration of 2500 mg / L tested by the observation well is 29.7 mPa·s:

[0039] Table 1 Data of an oil field

[0040] Average permeability near the wellbore, mD Average permeability of target formation, mD Target formation polymer viscosity, mPa·s 1500 1342 29.7

[0041] A method for characterizing the long-term migration of a polymer in a formation comprises the following steps:

[0042] Step S1: The polymer solution to be tested is first sheared by a shear simulation device, and the polymer solution is collected for later use after the performance is stable;

[0043] The specific steps are as follows:

[0044] Step S11: preparing a polymer solution of the required concentration of 2500 mg / L, filling a near-wellbore shear simulation device with an average formation permeability of 1500 mD and an average formation porosity of 33% according to the porosity and permeability of a certain oil field formation, and connecting the pipeline;

[0045] Step S12: adding the polymer solution into the intermediate container, setting the injection pump flow rate to 260.4 mL / min, starting the injection pump, and performing a shear experiment;

[0046] Step S13: measuring the viscosity of the polymer solution after shearing, and collecting it for later use after the viscosity remains unchanged.

[0047] Table 2 Viscosity of polymer before and after shearing

[0048] Polymer concentration, mg / L Viscosity before shear, mPa·s Viscosity after shear, mPa·s 2500 77.6 60.2

[0049] Step S2: After the polymer in S1 is circulated through the core or through multiple cores for multiple times, the target polymer is obtained. The specific steps and methods are as follows:

[0050] (1) Multiple cycles of a core

[0051] Step S21: According to the data provided by an oil field, K1 = 1500mD, K2 = 1342mD, select L = 4.5 cm, the permeability is close to the core of the near-wellbore zone K1, that is, the core permeability = 1502 mD is selected, the core is placed in the core holder, connected to the pipeline and saturated with water;

[0052] Step S23: adding the sheared polymer to the intermediate container and starting the injection pump;

[0053] Step S24: measuring the viscosity of the polymer output fluid at the core outlet, collecting the polymer output fluid after the viscosity stabilizes, recording the flow rate Q, time t, and measuring the viscosity μ of the outflow fluid;

[0054] Step S25: Calculate the core permeability K after the viscosity of the output fluid is stabilized, and compare it with the target formation permeability K2. If it is greater than the target formation permeability K2, loop steps S22 and S23 until the core permeability is less than the target formation permeability K2, and collect the polymer output fluid, which is the target polymer test fluid; if it is less than or equal to the target formation permeability K2, collect the polymer output fluid as the target polymer test fluid, and calculate the actual migration distance of the polymer;

[0055] Table 3 Experimental data

[0056] Water drive stability first Second time The third time Viscosity, mPa·s 60.2 52.5 40.4 30.4 Permeability, mD 1502 1440 1392 1339 Pressure, MPa 0.0039 0.3662 0.3182 0.2690 Migration distance, cm 0 4.5 9.0 13.5

[0057] (2) Single injection of multiple cores

[0058] Step S31: According to the data provided by an oil field, K1 = 1500mD, K2 = 1342mD, select the permeability gradient

[0059] ΔK=53mD, then the number of cores

[0060] Step S32: Select L = 4.5 cm, cores with permeabilities of 1450 mD, 1397 mD and 1341 mD, first put the core with permeability of 1450 mD into the core holder, connect the pipeline and saturate it with water, add the sheared polymer to the intermediate container and start;

[0061] Step S33: measuring the viscosity of the polymer output liquid at the core outlet, and collecting the polymer output liquid for standby use after the viscosity stabilizes;

[0062] Step S34: Replace the core with a permeability of K=K1+ΔK, and repeat steps S32 and S33 until the last core has a permeability of K=K2. The polymer output liquid collected before each core replacement is the target polymer test liquid.

[0063] Table 4 Experimental data

[0064]

[0065]

[0066] Combining the data in Tables 1 to 4, it can be found that the final polymer viscosity obtained by the simulation method of the present invention solves the actual formation polymer viscosity, and the error is within a reasonable range. The target formation polymer viscosity obtained by the two evaluation methods is equivalent to the actual test polymer viscosity of the oil field observation well, which proves that this method for evaluating the long-term migration of polymers in the formation is effective and accurate.

[0067] Comparative Example

[0068] Step S1: according to the provided permeability, a long core with L=13.5 cm, inlet permeability=1500 mD, and outlet permeability=1342 mD is prepared, and polymer output fluid is obtained by shearing with S1;

[0069] Step S2: Place the core in the core holder, connect the pipeline and saturate with water, add the polymer collected in S1 to the intermediate container and start;

[0070] Step S3: Collecting polymer output liquid.

[0071] Table 5 Experimental data

[0072] Viscosity, mPa·s Pressure, mD first 0 >10 Second time 21.3 4.215 The third time 20.9 4.112

[0073] As can be seen from Table 5, in the first experiment, the polymer was blocked because the permeability was difficult to control during the long core production process. From the data of the second and third experiments, it can be seen that due to the adsorption and retention of the polymer in the long core, the injection pressure was relatively high during the long-term migration of the polymer, and the viscosity of the polymer output fluid was relatively low.

[0074] The invention discloses a method for evaluating the long-term migration performance of a polymer for oil displacement in a formation. The method comprises the following steps: firstly shearing a polymer solution and keeping it for later use; then passing the polymer solution through a plurality of cores to simulate the long-term migration of the polymer for oil displacement in a formation, evaluating the performance of the effluent from each core, thereby evaluating and determining the performance of the polymer for oil displacement in the long-term migration process; or passing the polymer solution through a single core for multiple times to simulate the long-term migration of the polymer for oil displacement in a formation, evaluating the performance of the effluent from each core, thereby evaluating the performance of the polymer for oil displacement in the long-term migration process. The two methods for simulating the long-term migration of the polymer for oil displacement in a formation disclosed by the invention avoid the problem of excessive injection pressure in the long core simulation process, and can monitor the performance change of the polymer at any time, have good application prospects, can effectively simulate the long-term migration of the polymer for oil displacement in a formation, and provide theoretical guidance for the polymer injection site in an oil field.

[0075] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.

Claims

1. A method for evaluating the long-term migration performance of an oil displacement polymer in a formation, characterized in that: The method comprises the following steps: Step S1: The polymer solution to be tested is first sheared by a shear simulation device, and the polymer solution is collected for later use after the performance is stable; Step S2: passing the sheared solution obtained in step S1 through a single core multiple times to simulate the long-term migration of the oil displacement polymer in the formation, and evaluating the performance of the core outflow liquid each time, thereby evaluating the performance of the oil displacement polymer in the long-term migration process of the formation; The step S2 of evaluating the performance of the oil displacement polymer during the long-term migration process in the formation is to pass the sheared solution obtained in step S1 through multiple cores to simulate the long-term migration of the oil displacement polymer in the formation, and evaluate the performance of the effluent from each core, thereby evaluating and determining the performance of the oil displacement polymer during the long-term migration process in the formation; The specific steps of shearing the polymer solution to be tested by a shearing device in step S1 are: Step S11: preparing a polymer solution of required concentration, filling a core according to the porosity and permeability of the target formation, connecting a shear simulation device and connecting a pipeline; Step S12: adding the polymer solution into the intermediate container, setting the injection pump flow rate, starting the injection pump, and performing a shear experiment; Step S13: measuring the viscosity of the polymer solution after shearing, and collecting it for later use after the viscosity remains unchanged; In step S2, the sheared solution is passed through a single core multiple times to simulate the long-term migration of the oil displacement polymer in the formation, and the performance of the core outflow liquid is evaluated each time, thereby evaluating the performance of the oil displacement polymer in the long-term migration process of the formation. The specific method is: Step S21: Select a certain diameter A core with a length L and a permeability equal to the permeability K1 of the formation near the wellbore is placed in a core holder, connected to an intermediate container, a pipeline and saturated with water; Step S22: adding the sheared polymer to the intermediate container and starting the injection pump; Step S23: measuring the viscosity of the polymer output fluid at the core outlet, collecting the polymer output fluid after the viscosity stabilizes, recording the flow rate Q, time t, and measuring the viscosity μ of the outflow fluid; Step S24, calculate the core permeability K after the viscosity of the output fluid is stabilized, and compare it with the target formation permeability K2. If it is greater than the target formation permeability K2, loop steps S22 and S23 until the core permeability is less than the target formation permeability K2, and collect the polymer output fluid, which is the target polymer test fluid; if it is less than or equal to the target formation permeability K2, collect the polymer output fluid as the target polymer test fluid, and calculate the actual migration distance of the polymer; The method for calculating the permeability in step S24 is Darcy's formula: The actual migration distance of the polymer is L 实 =L*n 实 , where n 实 is the actual number of polymer injection cycles, and L is the core length; The specific method of passing the sheared solution through multiple cores to simulate the long-term migration of the oil displacement polymer in the formation, evaluating the performance of the effluent from each core, and thus evaluating and determining the performance of the oil displacement polymer in the long-term migration process of the formation is: Step S31: comparing the permeability K1 of the near-wellbore zone and the permeability K2 of the target formation, and selecting a moderate permeability gradient ΔK; Step S32: Select a certain length L and a certain diameter The core with permeability equal to the near-wellbore zone permeability K1 is placed in the core holder, connected to the intermediate container, pipeline and saturated with water, the sheared polymer is added to the intermediate container and the injection pump is started; Step S33: measuring the viscosity of the polymer output liquid at the core outlet, and collecting the polymer output liquid for standby use after the viscosity stabilizes; Step S34: Replace the core with a permeability of K=K1+△K, and repeat steps S32 and S33 until the last core has a permeability of K=K2. The polymer output liquid collected before each core replacement is the target polymer test liquid; In the step S34, the number of cores is changed: Actual polymer migration distance L 实 =L*n, where n is the number of cores with actual polymer migration and L is the core length.

2. A method for evaluating the long-term migration performance of an oil displacement polymer in a formation as claimed in claim 1, characterized in that: The shear simulation device in step S1 includes: an injection pump, a sand filling pipe or a core, a core holder, an intermediate container, a liquid storage tank, a pipeline and an oven.

3. A method for evaluating the long-term migration performance of an oil displacement polymer in a formation as claimed in claim 1, characterized in that: In step S12, the injection pump flow rate is determined according to the actual polymer shear rate.

4. A method for evaluating the long-term migration performance of an oil displacement polymer in a formation as claimed in claim 1 or 2, characterized in that: Either method can be selected to evaluate the long-term migration performance of oil recovery polymers in formations, or both methods can be used simultaneously for verification and evaluation.

Citation Information

Patent Citations

  • Two-stage shearing method for testing property parameter of polymer solution for expelling oil

    CN104792659A

  • System and method for testing tensile property of polymer solution in porous medium

    CN107843522A

  • Simulation method for evaluating deep migration characteristics of polymer microspheres in porous medium

    CN110927026A

  • Device and method for measuring reservoir salt deposition damage and evaluating effect of salt dissolving agent

    CN113504171A

  • Core displacement experimental device

    CN212134441U