Method for preparing tungsten on semiconductor wafer
By inserting a thermal annealing operation in the bulk growth stage of chemical vapor deposition, the problems of corrosion and warping on the backside of the semiconductor wafer are solved, the tungsten accumulation stress is reduced, and the product yield is improved.
Patent Information
- Application Number
- CN202111491362.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-08
AI Technical Summary
When tungsten is deposited by chemical vapor phase on a semiconductor wafer, the backside of the wafer will be corroded and flattened, resulting in serious warpage, which will affect the subsequent packaging process and product yield.
Insert at least one thermal annealing operation during the bulk growth stage of chemical vapor deposition, pause the deposition process and keep it warm at a set temperature to reduce tungsten accumulation stress and reduce damage to the backside by reaction gases.
It effectively reduces the risk of warpage of semiconductor wafers, reduces the damage to the backside by chemical vapor deposition process gases, and improves the flatness and product yield of the backside of the wafer.
Smart Images

Figure CN114420533B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for preparing tungsten on a semiconductor wafer. Background Art
[0002] Tungsten chemical vapor deposition has become an important technology in semiconductor processes because the metal tungsten (W) formed has low resistivity, high resistance to electromigration, excellent flatness when filling small through holes, and excellent step coverage compared to tungsten deposited by physical sputtering. In the structure of semiconductor components, tungsten is usually used as a highly conductive interconnect metal, silicon through holes (TSV) between metal layers, vertical contact holes (Contact), and spacers between aluminum and silicon. The main process gases for common tungsten chemical vapor deposition include tungsten hexafluoride (WF6).
[0003] However, when tungsten is deposited on one surface of a semiconductor wafer (called the front surface or the first surface) by chemical vapor deposition, although the other surface of the semiconductor wafer (called the back surface or the second surface) is placed on a base, its morphology will also change, which is specifically reflected in corrosion and deterioration of the flatness of the back of the wafer. In subsequent processes such as planarization of the front surface and cleaning of the back of the wafer, the degree of damage to the back of the wafer will be further aggravated, resulting in color differences and flatness problems on the back of the wafer that are visible to the naked eye, which will in turn affect the subsequent packaging process of semiconductor components and affect the product yield. Summary of the invention
[0004] The inventors of the present application have discovered that the main reason why the back side of a semiconductor wafer is damaged when tungsten is deposited using a chemical vapor deposition process is that during the deposition of metal tungsten onto the front side of the semiconductor wafer, as the amount of tungsten deposited increases, the stress accumulated in the tungsten becomes greater and greater, generating strain, causing the edge of the wafer to warp away from the base, forming a gap between the back side of the wafer and the base, and process gases in the process chamber, such as tungsten hexafluoride (WF6), diffuse to the back side of the wafer and react with the wafer on the back side of the wafer, thereby destroying the back side morphology.
[0005] Based on the above research, the present application proposes a method for preparing tungsten on a semiconductor wafer, which can reduce the warping of the semiconductor wafer during tungsten chemical vapor deposition and reduce the damage of the reaction gas to the back of the wafer.
[0006] The method for preparing tungsten on a semiconductor wafer proposed in this application includes:
[0007] Tungsten is deposited on a first surface of a semiconductor wafer using chemical vapor deposition, and a second surface of the semiconductor wafer opposite to the first surface is attached to a base. The deposition process of the chemical vapor deposition includes a nucleation stage and a bulk growth stage, wherein at least one thermal annealing operation is inserted in the bulk growth stage.
[0008] Optionally, before performing the thermal annealing operation, the deposition process of the chemical vapor deposition is suspended; after pausing the deposition process of the chemical vapor deposition, the thermal annealing operation is performed, and the semiconductor wafer is kept at a set annealing temperature for a set time; after the insulation is completed, the thermal annealing operation is terminated, and the remaining deposition process of the body growth stage is continued.
[0009] Optionally, the set annealing temperature is 350°C to 400°C.
[0010] Optionally, during the thermal annealing operation, the semiconductor wafer is kept at a set annealing temperature for 1 min to 6 min.
[0011] Optionally, the thermal annealing operation is inserted only once in the bulk growth stage.
[0012] Optionally, after the bulk growth phase begins, when the deposition time reaches 30% to 65% of the total duration of the bulk growth phase, the thermal annealing operation is performed.
[0013] Optionally, before performing the thermal annealing operation, the proportion of tungsten-containing gas in the chamber where the semiconductor wafer is located is reduced to below a set content.
[0014] Optionally, the tungsten-containing gas includes at least one of tungsten hexachloride (WCl6), tungsten hexafluoride (WF6) and tungsten hydroxyl.
[0015] Optionally, the temperature used for the chemical vapor deposition in the bulk growth stage is 350° C. to 550° C.
[0016] Optionally, a through hole is formed on the semiconductor wafer, and after the bulk growth stage is completed, tungsten fills the through hole and is deposited on the exposed surface of the semiconductor wafer outside the through hole.
[0017] In the method for preparing tungsten on a semiconductor wafer provided by the present invention, tungsten is deposited on a first surface of the semiconductor wafer by chemical vapor deposition, a second surface (serving as a back surface) of the semiconductor wafer opposite to the first surface is attached to a base, and at least one thermal annealing operation is inserted in the bulk growth stage. The thermal annealing operation can relieve the stress accumulated by the tungsten deposited on the semiconductor wafer, reduce the risk of warping of the semiconductor wafer, and reduce the damage of the process gas of the chemical vapor deposition to the back surface of the semiconductor wafer, thereby achieving the purpose of protecting the back surface of the wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the warping of a semiconductor wafer during tungsten chemical vapor deposition.
[0019] Figure 2 Schematic diagram of a method for preparing tungsten on a semiconductor wafer according to an embodiment of the present invention.
[0020] Description of reference numerals:
[0021] 10-semiconductor wafer; 20-base. DETAILED DESCRIPTION
[0022] The method for preparing tungsten on a semiconductor wafer of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will become clearer. It should be understood that the drawings in the specification are all in a very simplified form and are not in precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. It should be noted that the order of the steps in the method presented herein is not necessarily the only order for performing these steps, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method.
[0023] Figure 1 Schematic diagram of the warping of a semiconductor wafer during tungsten chemical vapor deposition. Figure 1 When a semiconductor wafer 10 is placed on a chemical vapor deposition base 20 and tungsten is continuously deposited on the semiconductor wafer 10 using a chemical vapor deposition process, the stress accumulated in the tungsten metal film under continuous high temperature conditions cannot be released in time, which will cause the semiconductor wafer 10 to warp. In the warped state, the reaction gas of the chemical vapor deposition will reach the back of the wafer and react, which will adversely affect the yield of semiconductor components manufactured using the semiconductor wafer 10.
[0024] Taking the use of tungsten hexafluoride (WF6) as the main reaction gas for tungsten chemical vapor deposition on silicon semiconductor wafers as an example, when tungsten hexafluoride contacts the silicon on the back of the wafer, the chemical reaction between the two is: WF6+Si——>W+SiF. The products of this reaction, tungsten (W) and silicon fluoride (SiF), are precipitated on the back of the wafer, causing the back of the wafer to be corroded and uneven, affecting subsequent processes and ultimately affecting product yield.
[0025] The following is a description of a method for preparing tungsten on a semiconductor wafer according to an embodiment of the present invention. The method can reduce the warpage of the semiconductor wafer during the tungsten chemical vapor deposition process, reduce the damage of the reaction gas to the back of the wafer, protect the back of the wafer, and improve the product yield.
[0026] Reference Figure 2 The method comprises step S1: depositing tungsten on a first surface of a semiconductor wafer by chemical vapor deposition, wherein a second surface of the semiconductor wafer opposite to the first surface is attached to a base, and the deposition process of the chemical vapor deposition comprises a nucleation phase and a bulk growth phase, wherein at least one thermal annealing operation is inserted in the bulk growth phase.
[0027] The semiconductor wafer may be made of materials known in the art, such as silicon, germanium, silicon germanium, silicon carbide, gallium oxide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide or indium antimonide, etc. It may also be silicon on insulator (SOI) or germanium on insulator (GOI), or other materials, such as GaAsP, AlInAs, AlGaAs, GaInAs, GaInP or GaInAsP, etc., or a combination of the above materials. When chemical vapor deposition is performed to deposit tungsten on the semiconductor wafer, the semiconductor wafer, for example, has completed part of the semiconductor process, and a pixel structure, a storage unit and / or a logic circuit may be formed on the semiconductor wafer, and may also include at least one of MOSFET (metal-oxide-semiconductor field effect transistor), CMOS (complementary metal oxide semiconductor), pFET (p-channel field effect transistor), nFET (n-channel field effect transistor), high-voltage transistor and high-frequency transistor, and may also include other suitable components.
[0028] The semiconductor wafer has two opposite surfaces, which are respectively recorded as the first surface and the second surface. The first surface is used as the front surface, that is, the side where tungsten needs to be deposited, and the second surface is used as the back surface. The second surface is the side that avoids reacting with the reaction gas of chemical vapor deposition. When chemical vapor deposition is performed, the semiconductor wafer is placed on a base in the deposition chamber of the chemical vapor deposition equipment, and the first surface is exposed to the reaction gas, while the second surface is attached to the surface of the base when it is not warped. Here, "first" and "second" are only used to distinguish and do not represent any order. In the method for preparing tungsten on a semiconductor wafer of an embodiment of the present invention, before depositing tungsten, a barrier layer (such as a silicon nitride layer and / or a silicon oxide layer) and an adhesion layer (such as a composite layer of metal titanium and titanium nitride) may be formed on the first surface of the semiconductor wafer.
[0029] By utilizing the excellent hole-filling property of chemical vapor deposition tungsten, in the embodiment of the present invention, a through hole may be formed on the semiconductor wafer, and the first surface on which tungsten is to be deposited includes the inner surface of the through hole and the surface of the semiconductor wafer outside the through hole. The tungsten attached to the first surface of the semiconductor wafer by chemical vapor deposition fills the through hole and covers the exposed surface of the wafer outside the through hole. The amount of tungsten deposited can be set according to specific needs, for example, the thickness of the tungsten covering the upper surface of the semiconductor wafer outside the through hole reaches 100%.
[0030] In an embodiment of the present invention, the process gas used for tungsten chemical vapor deposition may include one or more of hydrogen (H2), borane (B2H6), monosilane (SiH4), and argon (Ar) as auxiliary gases, and also includes at least one tungsten-containing gas selected from tungsten hexachloride (WCl6), tungsten hexafluoride (WF6), and hydroxyl tungsten. The tungsten-containing gas is the main reaction gas for tungsten chemical vapor deposition.
[0031] The tungsten deposition process by chemical vapor deposition includes a nucleation stage and a bulk growth stage. In the nucleation stage, a tungsten-containing gas reacts with hydrogen (or borane, monosilane) to generate a thin layer of tungsten, which serves as the growth point of the subsequent tungsten layer. In the bulk growth stage, the process parameters of chemical vapor deposition (such as pressure, gas flow, etc.) are different from those in the nucleation stage. Compared with the nucleation stage, the deposition rate, deposition time and deposition amount of the bulk growth stage are relatively large. The tungsten deposited in the bulk growth stage is about 90% of the total tungsten deposition amount in the same chemical vapor deposition process. The deposition temperature used in the chemical vapor deposition should avoid affecting the structure formed on the semiconductor wafer. In the embodiment of the present invention, the process temperature used in the bulk growth stage is set at 350°C to 550°C, and more specifically, at about 400°C to 500°C.
[0032] In the embodiment of the present invention, in order to relieve and release the stress accumulated as the amount of tungsten deposition increases and reduce the risk of warping of the semiconductor wafer, at least one thermal annealing operation is inserted in the body growth stage. The thermal annealing operation is during the body growth stage, and the body growth process of chemical vapor deposition is performed for a period of time before and after the thermal annealing operation. During the entire body growth stage, the number of times the thermal annealing operation is inserted is specifically set according to the thickness of the tungsten to be deposited and the time of the thermal annealing.
[0033] Before performing the thermal annealing operation, the deposition process of the chemical vapor deposition is suspended. The suspension here can be achieved by setting the parameters of the chemical vapor deposition. After the suspension, the chemical reaction of generating tungsten on the semiconductor wafer gradually slows down to basically stop, so that the tungsten deposition is basically stopped. Specifically, before performing the thermal annealing operation, the proportion of tungsten-containing gas in the chamber where the semiconductor wafer is located can be reduced to below the set content to achieve the purpose of suppressing the deposition rate of tungsten. For example, at the pause node, the intake flow rate of the tungsten-containing gas is set to 0, and the flow rate of other process gases used in the tungsten chemical vapor deposition and other parameters can be left unchanged. The thermal annealing operation can allow the semiconductor wafer to be directly performed on a chemical vapor deposition reaction base with a heating function. In this case, the semiconductor substrate does not need to be transferred. The thermal annealing operation can also be performed after the semiconductor substrate is transferred from the chemical vapor deposition reaction base to another heating base. After the thermal annealing operation is completed, the semiconductor substrate is transferred back to the chemical vapor deposition reaction base.
[0034] After pausing the deposition process of the chemical vapor deposition, the thermal annealing operation is performed. In an embodiment of the present invention, the thermal annealing operation is completed by keeping the semiconductor wafer at a set annealing temperature for a set period of time. The set annealing temperature is, for example, less than the temperature used for the chemical vapor deposition, for example, in the range of 350°C to 400°C. The semiconductor wafer is kept at a set annealing temperature of 350°C to 400°C for, for example, 1min to 6min; more preferably, kept at a set annealing temperature of 350°C to 400°C for 70s to 6min. After the insulation is completed, the semiconductor wafer can be placed on a reaction base for chemical vapor deposition, the chemical vapor deposition process is restarted, and the remaining deposition process of the body growth stage is continued. It can be specifically carried out through the parameter setting of chemical vapor deposition.
[0035] In one embodiment, the thermal annealing operation is inserted only once in the bulk growth phase of tungsten, and the thermal annealing operation is performed for about half of the bulk growth phase. Specifically, in the method, after the bulk growth phase begins, when the deposition time reaches 30% to 65% of the total duration of the bulk growth phase, the thermal annealing operation is performed.
[0036] In the method for preparing tungsten on a semiconductor wafer described in an embodiment of the present invention, tungsten is deposited on the first surface of the semiconductor wafer by chemical vapor deposition, the second surface (as the back side) of the semiconductor wafer opposite to the first surface is attached to a base, and at least one thermal annealing operation is inserted in the bulk growth stage. The thermal annealing operation can relieve the stress accumulated by the tungsten deposited on the semiconductor wafer, reduce the risk of warping of the semiconductor wafer, reduce the damage of the process gas of chemical vapor deposition to the back side of the semiconductor wafer, and achieve the purpose of protecting the back side of the wafer, which helps to improve the product yield. In addition, the method does not require additional film-forming etching and other processes, is easy to operate, has low cost, and has high application value.
[0037] The above description is only a description of the preferred embodiment of the present invention, and is not any limitation on the scope of rights of the present invention. Any technical personnel in this field can make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing tungsten on a semiconductor wafer, It is characterized in that include: Tungsten is deposited on a first surface of a semiconductor wafer by chemical vapor deposition, and a second surface of the semiconductor wafer opposite to the first surface is attached to a base. The deposition process of the chemical vapor deposition includes a nucleation stage and a body growth stage, wherein at least one thermal annealing operation is inserted in the body growth stage, and the thermal annealing operation is located during the body growth stage. The body growth process of chemical vapor deposition is performed for a period of time before and after the thermal annealing operation. Before the thermal annealing operation is performed, the deposition process of the chemical vapor deposition is suspended, and the set annealing temperature of the thermal annealing operation is 350°C~400°C.
2. The method for preparing tungsten on a semiconductor wafer as claimed in claim 1, It is characterized in that After pausing the deposition process of the chemical vapor deposition, performing the thermal annealing operation, keeping the semiconductor wafer at a set annealing temperature for a set time; After the heat preservation is completed, the thermal annealing operation is terminated and the remaining deposition process of the bulk growth stage is continued.
3. The method for preparing tungsten on a semiconductor wafer as claimed in claim 2, It is characterized in that When performing the thermal annealing operation, the semiconductor wafer is kept at the set annealing temperature for 1 min to 6 min.
4. The method for preparing tungsten on a semiconductor wafer as claimed in claim 1, It is characterized in that The thermal annealing operation is inserted only once in the bulk growth stage.
5. The method for preparing tungsten on a semiconductor wafer as claimed in claim 4, It is characterized in that After the bulk growth phase begins, the thermal annealing operation is performed when the deposition time reaches 30% to 65% of the total duration of the bulk growth phase.
6. The method for preparing tungsten on a semiconductor wafer as claimed in claim 1, It is characterized in that Before performing the thermal annealing operation, the proportion of tungsten-containing gas in the chamber where the semiconductor wafer is located is reduced to below a set content.
7. The method for preparing tungsten on a semiconductor wafer as claimed in claim 6, It is characterized in that The tungsten-containing gas includes at least one of tungsten hexachloride, tungsten hexafluoride and tungsten hydroxyl.
8. A method for preparing tungsten on a semiconductor wafer according to any one of claims 1 to 7, It is characterized in that The temperature used by the chemical vapor deposition in the bulk growth stage is 350° C. to 550° C.
9. A method for preparing tungsten on a semiconductor wafer according to any one of claims 1 to 7, It is characterized in that A through hole is formed on the semiconductor wafer. After the bulk growth stage is completed, tungsten fills the through hole and is deposited on the exposed surface of the semiconductor wafer outside the through hole.
Citation Information
Patent Citations
Metal tungsten deposition method and structure
CN110714189A