A method for preparing polystyrene thermal insulation material

Through a one-step polymerization method and preheating, prepolymerization, and multi-step polymerization processes, high-performance polystyrene insulation materials are prepared, which solves the problems of insufficient high temperature resistance and flame retardancy in the existing technology, reduces costs, and improves the material's performance. Practicality.

CN114426746BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011187524.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-29
Publication Date
2024-10-15
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

When existing polystyrene insulation materials achieve high temperature resistance and flame retardant effects, they require secondary processing, which increases costs, and their performance is insufficient to meet the needs of certain applications.

Method used

Using a one-step polymerization method, through preheating, prepolymerization and three-step polymerization process, using styrene, ethylbenzene, initiator and flame retardant, a polyester with good tensile strength, high melt tension and high heat distortion temperature is prepared. Styrene insulation.

Benefits of technology

The high-performance preparation of polystyrene insulation materials is achieved, reducing intermediate links, reducing costs, and improving the practicality of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002751765130000091
    Figure BDA0002751765130000091
Patent Text Reader

Abstract

The present invention provides a method for preparing a polystyrene thermal insulation material, comprising: S1. preheating a raw material containing styrene, ethylbenzene, an initiator and a flame retardant to obtain a first mixed material; S2. subjecting the first mixed material to a prepolymerization reaction to obtain a second mixed material; S3. subjecting the second mixed material to a first polymerization reaction to obtain a third mixed material; S4. subjecting the third mixed material to a second polymerization reaction to obtain a fourth mixed material; S5. subjecting the fourth mixed material to a third polymerization reaction to obtain a fifth mixed material containing a polystyrene thermal insulation material; and optionally, S6. devolatilizing the fifth mixed material to obtain the polystyrene thermal insulation material. The polystyrene thermal insulation material prepared by the preparation method has the characteristics of good tensile strength, high melt tension and high heat deformation temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, and in particular to a method for preparing a polystyrene thermal insulation material. Background Art

[0002] Extruded polystyrene insulation board is a rigid foam insulation board that is continuously extruded and foamed by a special process. Extruded polystyrene insulation board is an environmentally friendly insulation material with beneficial properties such as low thermal conductivity, high pressure resistance, moisture resistance, airtightness, non-water absorption, light weight, corrosion resistance, and long service life. It has been widely used in wall insulation, insulation of flat concrete roofs and steel structure roofs, low-temperature storage, moisture-proof insulation and control of ground expansion in the fields of ground, parking platforms, airport runways, highways, etc. This polystyrene insulation material is required not only to have good mechanical properties and processing properties, but also to have high temperature resistance and flame retardant properties.

[0003] At present, in order to achieve the effects of high temperature resistance and flame retardancy, flame retardants are basically added to ordinary expanded polystyrene. This method involves secondary processing and increases costs.

[0004] In order to solve the above problems, the key issue that needs to be solved in the development of polystyrene products is to obtain extruded polystyrene insulation materials by a one-step polymerization method. Summary of the invention

[0005] In view of the above problems existing in the prior art, one of the objects of the present invention is to provide a method for preparing a polystyrene thermal insulation material. The polystyrene thermal insulation material prepared by the preparation method has the characteristics of good tensile strength, high melt tension and high heat deformation temperature.

[0006] A second object of the present invention is to provide a polystyrene thermal insulation material corresponding to the first object.

[0007] The third object of the present invention is to provide an application of a polystyrene thermal insulation material corresponding to the above-mentioned object.

[0008] To achieve one of the above purposes, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a polystyrene thermal insulation material, comprising:

[0010] S1. Preheating the raw materials comprising styrene, ethylbenzene, an initiator and a flame retardant to obtain a first mixed material;

[0011] S2. subjecting the first mixed material to a prepolymerization reaction to obtain a second mixed material;

[0012] S3. subjecting the second mixed material to a first polymerization reaction to obtain a third mixed material;

[0013] S4. subjecting the third mixed material to a second polymerization reaction to obtain a fourth mixed material;

[0014] S5. subjecting the fourth mixed material to a third polymerization reaction to obtain a fifth mixed material comprising a polystyrene insulation material; and

[0015] Optionally, S6. performing devolatilization treatment on the fifth mixed material to obtain the polystyrene thermal insulation material.

[0016] The inventors of the present application have found in their research that a polystyrene insulation material with good tensile strength, high melt tension and high heat deformation temperature can be obtained by using styrene, ethylbenzene, initiator and flame retardant as raw materials and adopting preheating, prepolymerization and three-step polymerization processes.

[0017] In some preferred embodiments of the present invention, in step S1, the content of styrene in the raw material is 85 wt% to 95 wt%.

[0018] According to some embodiments of the present invention, in step S1, the content of styrene in the raw material is 88 wt% to 95 wt%.

[0019] According to some embodiments of the present invention, in step S1, the content of styrene in the raw material is 88 wt% to 92 wt%.

[0020] In some preferred embodiments of the present invention, in step S1, the ethylbenzene content in the raw material is 1 wt% to 15 wt%.

[0021] In some preferred embodiments of the present invention, in step S1, the ethylbenzene content in the raw material is 5 wt% to 15 wt%.

[0022] In some preferred embodiments of the present invention, in step S1, the ethylbenzene content in the raw material is 6 wt% to 15 wt%.

[0023] In some preferred embodiments of the present invention, in step S1, the ethylbenzene content in the raw material is 6 wt% to 12 wt%.

[0024] In some preferred embodiments of the present invention, in step S1, the ethylbenzene content in the raw material is 6 wt% to 10 wt%.

[0025] In some preferred embodiments of the present invention, in step S1, the content of the initiator in the raw material is 100 ppm to 500 ppm.

[0026] In some preferred embodiments of the present invention, in step S1, the content of the initiator in the raw material is 200 ppm to 400 ppm.

[0027] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 100 ppm to 2000 ppm.

[0028] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 500ppm to 2000ppm.

[0029] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 800ppm to 2000ppm.

[0030] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 1000ppm to 2000ppm.

[0031] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 1100ppm to 2000ppm.

[0032] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 1100ppm to 1800ppm.

[0033] In some preferred embodiments of the present invention, in step S1, the content of the flame retardant in the raw material is 1100 ppm to 1600 ppm.

[0034] In some preferred embodiments of the present invention, in step S1, the initiator is dicumyl peroxide.

[0035] According to the present invention, in the system of the present invention, the use of dicumyl peroxide as an initiator can achieve the best initiation effect compared with other types of initiators.

[0036] In some preferred embodiments of the present invention, in step S1, the flame retardant is cage-type silsesquioxane.

[0037] According to the present invention, in the system of the present invention, compared with other types of flame retardants, the use of cage silsesquioxane as a flame retardant can obtain the best flame retardant effect.

[0038] According to the present invention, the cage-type silsesquioxane is a product commonly sold in the market.

[0039] In some preferred embodiments of the present invention, in step S1, the temperature of the preheat treatment is 80°C to 90°C, preferably 82°C to 88°C.

[0040] In some preferred embodiments of the present invention, in step S1, the preheating treatment time is 1 min to 60 min, preferably 10 min to 15 min.

[0041] In some preferred embodiments of the present invention, in step S2, the temperature of the prepolymerization reaction is 110°C to 120°C, preferably 112°C to 118°C.

[0042] In some preferred embodiments of the present invention, in step S2, the prepolymerization reaction time is 1 min to 60 min, preferably 10 min to 15 min.

[0043] In some preferred embodiments of the present invention, in step S2, the liquid level is controlled to be 70% to 80%.

[0044] In some preferred embodiments of the present invention, in step S3, the temperature of the first polymerization reaction is 120°C to 130°C, preferably 122°C to 128°C.

[0045] In some preferred embodiments of the present invention, in step S3, the time of the first polymerization reaction is 10 min to 90 min, preferably 45 min to 60 min.

[0046] In some preferred embodiments of the present invention, in step S4, the temperature of the second polymerization reaction is 140°C to 150°C, preferably 142°C to 148°C.

[0047] In some preferred embodiments of the present invention, in step S4, the time of the second polymerization reaction is 10 min to 90 min, preferably 45 min to 60 min.

[0048] In some preferred embodiments of the present invention, in step S5, the temperature of the third polymerization reaction is 150°C to 160°C, preferably 162°C to 168°C.

[0049] In some preferred embodiments of the present invention, in step S5, the duration of the third polymerization reaction is 10 min to 90 min, preferably 45 min to 60 min.

[0050] In some preferred embodiments of the present invention, the temperature of the first polymerization reaction is lower than the temperature of the second polymerization reaction. Preferably, the temperature of the first polymerization reaction is 18°C ​​to 30°C lower than the temperature of the second polymerization reaction, and preferably 20°C to 25°C lower.

[0051] In some preferred embodiments of the present invention, the temperature of the second polymerization reaction is lower than the temperature of the third polymerization reaction. Preferably, the temperature of the second polymerization reaction is 5°C to 15°C lower than the temperature of the third polymerization reaction, and preferably 8°C to 12°C lower.

[0052] In some preferred embodiments of the present invention, in step S6, the pressure of the devolatilization treatment is -10 KPa to 0 KPa, preferably -8 KPa to -2 KPa.

[0053] In some preferred embodiments of the present invention, in step S6, the temperature of the devolatilization treatment is 230°C to 250°C, preferably 235°C to 245°C.

[0054] In some preferred embodiments of the present invention, in step S6, the time of the devolatilization treatment is 10 min to 90 min, preferably 45 min to 60 min.

[0055] To achieve the second purpose above, the technical solution adopted by the present invention is as follows:

[0056] A polystyrene thermal insulation material prepared according to the above preparation method.

[0057] In some preferred embodiments of the present invention, the heat deformation temperature of the polystyrene thermal insulation material is above 100°C, preferably 100°C to 120°C.

[0058] To achieve the third purpose above, the technical solution adopted by the present invention is as follows:

[0059] A polystyrene thermal insulation material prepared according to the above preparation method or use of the above polystyrene thermal insulation material as a raw material for preparing an extruded polystyrene thermal insulation board.

[0060] The beneficial effects of the present invention are at least that: due to the use of the optimal component ratio and process production conditions in the production process, the obtained polystyrene insulation material has good tensile strength and high heat deformation temperature, the heat deformation temperature is as high as 104°C, and can be directly used for extrusion molding polystyrene insulation boards, reducing intermediate links, saving costs, and having strong practicality. DETAILED DESCRIPTION

[0061] The present invention is described in detail below by way of examples, but the protection scope of the present invention is not limited to the following description.

[0062] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be obtained through commercial channels.

[0063] In the following embodiments:

[0064] Melt flow index is determined according to ASTM D1238;

[0065] The tensile yield strength is measured according to ASTM D638;

[0066] The unnotched cantilever beam impact strength is measured according to ASTM D256.

[0067] The heat distortion temperature is measured according to ASTM D648.

[0068] In the following embodiments, unless otherwise specified, the initiator used is dicumyl peroxide, and the flame retardant used is amino-substituted cage silsesquioxane (OAPS).

[0069] Example 1

[0070] Step 1: Feed raw materials including styrene, ethylbenzene, initiator and flame retardant (wherein the content of ethylbenzene is 8%, the content of initiator is 300ppm, the content of flame retardant is 1500ppm, and the balance is styrene) into a preheater at a flow rate of 15t / h, control the temperature of the preheater to 82°C and the residence time of the raw materials in the preheater to about 13min, and obtain a first mixed material from the outlet of the preheater.

[0071] Step 2: Pass the first mixed material obtained in step 1 into a prepolymerization reactor, control the temperature of the prepolymerization reactor to 112° C. and the residence time of the first mixed material in the prepolymerization reactor to about 10 minutes, control the liquid level in the prepolymerization reactor to 73%, and obtain a second mixed material from the outlet of the prepolymerization reactor.

[0072] Step 3: Pass the second mixed material obtained in step 2 into the first reactor, control the temperature of the first reactor to 125° C. and the residence time of the second mixed material in the first reactor to about 45 minutes, and obtain the third mixed material from the outlet of the first reactor.

[0073] Step 4: Pass the third mixed material obtained in step 3 into the second reactor, control the temperature of the second reactor to 145° C. and the residence time of the third mixed material in the second reactor to about 45 minutes, and obtain the fourth mixed material from the outlet of the second reactor.

[0074] Step 5: Pass the fourth mixed material obtained in step 4 into the third reactor, control the temperature of the third reactor to 155° C. and the residence time of the fourth mixed material in the third reactor to about 45 minutes, and obtain the fifth mixed material from the outlet of the third reactor.

[0075] Step six: Pass the fifth mixed material obtained in step five into a de-recovery device to remove unreacted raw materials and then extrude and pelletize to obtain a polystyrene thermal insulation material, wherein the pressure of the de-recovery device is controlled to be -5 KPa and the temperature is 235°C, and the residence time of the fifth mixed material in the de-recovery device is about 45 minutes.

[0076] The prepared polystyrene thermal insulation material was tested, and its melt flow index, tensile yield strength, IZOD unnotched impact strength, heat deformation temperature and melt tension are listed in Table 1.

[0077] Example 2

[0078] Step 1: The raw materials including styrene, ethylbenzene, initiator and flame retardant (wherein the content of ethylbenzene is 8%, the content of initiator is 350ppm, the content of flame retardant is 1200ppm, and the balance is styrene) are passed into the preheater at a flow rate of 15t / h, the temperature of the preheater is controlled to be 86°C and the residence time of the raw materials in the preheater is about 13min, and the first mixed material is obtained from the outlet of the preheater.

[0079] Step 2: Pass the first mixed material obtained in step 1 into a prepolymerization reactor, control the temperature of the prepolymerization reactor to 118°C and the residence time of the first mixed material in the prepolymerization reactor to about 12 minutes, control the liquid level in the prepolymerization reactor to 72%, and obtain a second mixed material from the outlet of the prepolymerization reactor.

[0080] Step 3: Pass the second mixed material obtained in step 2 into the first reactor, control the temperature of the first reactor to 123° C. and the residence time of the second mixed material in the first reactor to about 45 minutes, and obtain the third mixed material from the outlet of the first reactor.

[0081] Step 4: Pass the third mixed material obtained in step 3 into the second reactor, control the temperature of the second reactor to 146° C. and the residence time of the third mixed material in the second reactor to about 50 minutes, and obtain the fourth mixed material from the outlet of the second reactor.

[0082] Step 5: Pass the fourth mixed material obtained in step 4 into the third reactor, control the temperature of the third reactor to 155° C. and the residence time of the fourth mixed material in the third reactor to about 50 minutes, and obtain the fifth mixed material from the outlet of the third reactor.

[0083] Step six: Pass the fifth mixed material obtained in step five into a de-recovery device to remove unreacted raw materials and then extrude and pelletize to obtain a polystyrene thermal insulation material, wherein the pressure of the de-recovery device is controlled to be -3 KPa and the temperature is 237°C, and the residence time of the fifth mixed material in the de-recovery device is about 45 minutes.

[0084] The prepared polystyrene thermal insulation material was tested, and its melt flow index, tensile yield strength, IZOD unnotched impact strength, heat deformation temperature and melt tension are listed in Table 1.

[0085] Example 3

[0086] Step 1: The raw materials including styrene, ethylbenzene, initiator and flame retardant (wherein the content of ethylbenzene is 10%, the content of initiator is 250ppm, the content of flame retardant is 1300ppm, and the balance is styrene) are passed into the preheater at a flow rate of 16t / h, the temperature of the preheater is controlled to be 85°C and the residence time of the raw materials in the preheater is about 13min, and the first mixed material is obtained from the outlet of the preheater.

[0087] Step 2: Pass the first mixed material obtained in step 1 into a prepolymerization reactor, control the temperature of the prepolymerization reactor to 114°C and the residence time of the first mixed material in the prepolymerization reactor to about 12 minutes, control the liquid level in the prepolymerization reactor to 74%, and obtain a second mixed material from the outlet of the prepolymerization reactor.

[0088] Step 3: Pass the second mixed material obtained in step 2 into the first reactor, control the temperature of the first reactor to 123° C. and the residence time of the second mixed material in the first reactor to about 48 minutes, and obtain the third mixed material from the outlet of the first reactor.

[0089] Step 4: Pass the third mixed material obtained in step 3 into the second reactor, control the temperature of the second reactor to 148° C. and the residence time of the third mixed material in the second reactor to about 55 minutes, and obtain the fourth mixed material from the outlet of the second reactor.

[0090] Step 5: Pass the fourth mixed material obtained in step 4 into the third reactor, control the temperature of the third reactor to 152° C. and the residence time of the fourth mixed material in the third reactor to about 55 minutes, and obtain the fifth mixed material from the outlet of the third reactor.

[0091] Step six: Pass the fifth mixed material obtained in step five into a de-recovery device to remove unreacted raw materials and then extrude and pelletize to obtain a polystyrene thermal insulation material, wherein the pressure of the de-recovery device is controlled to be -6 KPa and the temperature is 240°C, and the residence time of the fifth mixed material in the de-recovery device is about 50 minutes.

[0092] The prepared polystyrene thermal insulation material was tested, and its melt flow index, tensile yield strength, IZOD unnotched impact strength, heat deformation temperature and melt tension are listed in Table 1.

[0093] Example 4

[0094] Example 4 is configured to be substantially the same as Example 1, except that the flame retardant in Example 1 is replaced by magnesium hydroxide.

[0095] The obtained polystyrene material was tested and the results are shown in Table 1.

[0096] Example 5

[0097] Example 5 is configured to be substantially the same as Example 1, except that the flame retardant in Example 1 is replaced by antimony trioxide.

[0098] The obtained polystyrene material was tested and the results are shown in Table 1.

[0099] Example 6

[0100] Example 6 is configured to be substantially the same as Example 1, except that the initiator in Example 1 is replaced by tert-butyl peroxide.

[0101] The obtained polystyrene material was tested and the results are shown in Table 1.

[0102] Example 7

[0103] Example 7 is configured substantially the same as Example 1, except that benzoyl peroxide is used to replace the initiator in Example 1.

[0104] The obtained polystyrene material was tested and the results are shown in Table 1.

[0105] Example 8

[0106] Example 8 was configured substantially the same as Example 1, except that the amount of flame retardant used was 500 ppm.

[0107] The obtained polystyrene material was tested and the results are shown in Table 1.

[0108] Example 9

[0109] Example 9 was configured substantially the same as Example 1, except that the amount of flame retardant used was 3000 ppm.

[0110] The obtained polystyrene material was tested and the results are shown in Table 1.

[0111] Table 1

[0112]

[0113] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A method for preparing a polystyrene thermal insulation material, comprising: S1. Preheating the raw materials comprising styrene, ethylbenzene, an initiator and a flame retardant to obtain a first mixed material; the preheating temperature is 80 ℃ ~ 90 ℃; S2. The first mixed material is subjected to a prepolymerization reaction to obtain a second mixed material; the prepolymerization reaction temperature is 110 ℃ ~ 120 ℃; S3. subjecting the second mixed material to a first polymerization reaction to obtain a third mixed material; the temperature of the first polymerization reaction is 120 ℃ ~ 130 ℃; S4. subjecting the third mixed material to a second polymerization reaction to obtain a fourth mixed material; the temperature of the second polymerization reaction is 140 ℃ ~ 150 ℃; S5. subjecting the fourth mixed material to a third polymerization reaction to obtain a fifth mixed material comprising a polystyrene insulation material; the temperature of the third polymerization reaction is 150 ℃ ~ 160 ℃; and S6. Devolatilizing the fifth mixed material to obtain the polystyrene insulation material; The initiator is dicumyl peroxide; the flame retardant is cage-type silsesquioxane; In step S1, in the raw materials, the content of styrene is 85wt%~95wt%; the content of ethylbenzene is 1wt%~15wt%; the content of the initiator is 100ppm~500ppm; and the content of the flame retardant is 100ppm~2000ppm.

2. The preparation method according to claim 1, characterized in that In step S1, the preheating treatment time is 1 min to 60 min.

3. The preparation method according to claim 2, characterized in that The preheating treatment temperature is 82° C. to 88° C.; and / or the preheating treatment time is 10 min to 15 min.

4. The preparation method according to any one of claims 1 to 3, characterized in that In step S2, the prepolymerization reaction time is 1 min to 60 min; and / or the liquid level is controlled to be 70% to 80%.

5. The preparation method according to claim 4, characterized in that The temperature of the prepolymerization reaction is 112° C. to 118° C.; and / or the time of the prepolymerization reaction is 10 min to 15 min.

6. The preparation method according to any one of claims 1 to 3, characterized in that In step S3, the first polymerization reaction time is 10 min to 90 min.

7. The preparation method according to claim 6, characterized in that The temperature of the first polymerization reaction is 122° C. to 128° C.; and / or the time of the first polymerization reaction is 45 min to 60 min.

8. The preparation method according to any one of claims 1 to 3, characterized in that In step S4, the second polymerization reaction time is 10 min to 90 min.

9. The preparation method according to claim 8, characterized in that The temperature of the second polymerization reaction is 142° C. to 148° C.; and / or the time of the second polymerization reaction is 45 min to 60 min.

10. The preparation method according to any one of claims 1 to 3, characterized in that: In step S5, the third polymerization reaction time is 10 min to 90 min.

11. The preparation method according to claim 10, characterized in that The temperature of the third polymerization reaction is 162° C. to 168° C.; and / or the time of the third polymerization reaction is 45 min to 60 min.

12. The preparation method according to any one of claims 1 to 3, characterized in that In step S6, the pressure of the devolatilization treatment is -10 KPa to 0 KPa; and / or the temperature of the devolatilization treatment is 230° C. to 250° C.; and / or the time of the devolatilization treatment is 10 min to 90 min.

13. The preparation method according to claim 12, characterized in that The pressure of the devolatilization treatment is -8KPa to -2KPa; and / or the temperature of the devolatilization treatment is 235°C to 245°C; and / or the time of the devolatilization treatment is 45min to 60min.

14. A polystyrene thermal insulation material obtained by the preparation method according to any one of claims 1 to 13, wherein the heat deformation temperature of the polystyrene thermal insulation material is above 100°C.

15. The preparation method according to claim 14, characterized in that: The heat deformation temperature of the polystyrene thermal insulation material is 100°C to 120°C.

16. Use of the polystyrene thermal insulation material obtained by the preparation method according to any one of claims 1 to 13 or the polystyrene thermal insulation material according to claim 14 or 15 as a raw material for preparing an extruded polystyrene thermal insulation board.