Physical crosslinking type transparent nylon and preparation method thereof

By introducing urea groups and fatty cyclodiamines into transparent nylon, a physical crosslinking point is formed, the problem of low glass transition temperature of transparent nylon materials is solved, the mechanical properties and transparency are improved, and the high temperature stability of the material is achieved and reprocessability.

CN119039581APending Publication Date: 2024-11-29SHANDONG GUANGYIN NEW MATERIALS
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411172389.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The glass transition temperature of transparent nylon materials is generally lower than 150°C, which limits its application in high temperature environments. Chemical crosslinking can easily lead to gelation and the reaction end point is difficult to control.

Method used

The urea group is introduced by reacting isocyanate with amino groups to form a physical crosslinking point, combined with fatty cyclodiamine as the preparation monomer, and a simple process method is used to prepare physical crosslinked transparent nylon to improve the glass transition temperature and transparency of the material.

Benefits of technology

It significantly improves the glass transition temperature and mechanical properties of the material, broadens the scope of high-temperature application, maintains the transparency of the material, and realizes the reprocessability and recycling ability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009679060000021
    Figure BDA0005009679060000021
  • Figure BDA0005009679060000061
    Figure BDA0005009679060000061
  • Figure FDA0005009679050000011
    Figure FDA0005009679050000011
Patent Text Reader

Abstract

The invention belongs to the technical field of polyamide, and particularly relates to physical crosslinking type transparent nylon and a preparation method thereof. The preparation method comprises the following steps: S1, adding diisocyanate and alicyclic diamine into a solvent for reaction to generate an amino-terminated prepolymer; s2, adding the amino-terminated prepolymer and aliphatic dibasic acid into deionized water, and stirring to obtain a salt solution; s3, mixing the salt solution, a catalyst and an antioxidant, and heating for polymerization reaction to obtain the physical crosslinking type transparent nylon. Through the reaction of isocyanate and amino, ureido is successfully introduced into a polyamide system, then physical crosslinking points are constructed, and the crosslinking points effectively limit the free movement of a macromolecular chain, so that the glass-transition temperature of the material is remarkably increased, and the material can be stably applied in a high-temperature environment. Meanwhile, alicyclic diamine is selected as a preparation monomer, so that the prepared material can show excellent transparency while having high-temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyamide, and in particular relates to physically cross-linked transparent nylon and a preparation method thereof. Background Art

[0002] Polyamide, also known as nylon, refers to a class of polymers with an amide bond (-CONH-) in the main chain. Among them, transparent nylon is an amorphous or microcrystalline material with a light transmittance generally greater than 90%. It is widely used in optical instruments, precision parts, food packaging, high-end sports equipment, etc. However, since most transparent nylons are amorphous or microcrystalline, their glass transition temperature is generally lower than 150°C. This feature limits their application to a certain extent in situations where they inevitably need to withstand high temperature environments.

[0003] After moderate crosslinking, linear polymers cross-link molecules through the formation of chemical bonds or physical action to form a three-dimensional network structure, which can improve its mechanical strength, glass transition temperature, dimensional stability, solvent resistance and other properties. Crosslinking is divided into chemical crosslinking and physical crosslinking. Chemical crosslinking generally uses a multifunctional crosslinking agent to connect polymer chains to each other through the formation of chemical bonds, which is prone to gelation and the reaction end point is difficult to control. Physical crosslinking can be crosslinked using supramolecular interactions between molecular chains. This interaction includes van der Waals forces, electrostatic interactions, hydrogen bonds, metal ligand coordination, etc. The advantage of physical crosslinking is its reversibility. Under appropriate conditions, the crosslinking structure can be untied, thereby realizing the reprocessing and reuse of polymer materials. Among them, the hydrogen bond effect is widely used as a physical crosslinking point because it is easy to form and has a strong binding force.

[0004] Amide bonds can also form hydrogen bonding effects, but there is only one hydrogen bond, which is easier to break. The urea group can form two hydrogen bonds due to its special structure, which is relatively stable and has strong hydrogen bonding properties. Therefore, introducing the special hydrogen bonding properties of the urea group into the modification of transparent nylon materials to improve its overall performance is of great significance for the promotion of high-temperature resistant transparent nylon. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a physically cross-linked transparent nylon, which successfully introduces urea groups into the polyamide system through the reaction of isocyanate and amino groups, thereby constructing physical cross-linking points. These cross-linking points effectively restrict the free movement of the polymer chain, thereby significantly improving the glass transition temperature of the material, so that it can be stably used in high temperature environments. At the same time, the use of aliphatic cyclic diamine as a preparation monomer ensures that the prepared material has high temperature stability and excellent transparency;

[0006] Another object of the present invention is to provide a method for preparing physically cross-linked transparent nylon, which has a simple process and is easy for large-scale production.

[0007] The technical solution adopted by the present invention is as follows:

[0008] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0009] S1, adding a diisocyanate and an alicyclic diamine in a molar ratio of (0.05-0.25):1 into a solvent for reaction to generate an amino-terminated prepolymer;

[0010] S2, adding the amino-terminated prepolymer and the aliphatic dibasic acid into deionized water, stirring to obtain a salt solution;

[0011] S3, mixing the salt solution, the catalyst and the antioxidant, raising the temperature to carry out polymerization reaction, and after the reaction is completed, cooling the obtained polymer melt and pelletizing to obtain physically cross-linked transparent nylon.

[0012] The diisocyanate is one or more of hexamethylene diisocyanate, 4,4-diisocyanate dicyclohexylmethane, 4,4'-diphenylmethane diisocyanate, isophorone diisocyanate or naphthalene diisocyanate.

[0013] The alicyclic diamine is one or more of 4,4'-diaminodicyclohexylmethane (PACM), isophoronediamine (IPDA), 3,3'-dimethyl-4,4-diaminodicyclohexylmethane (MACM) or 1-methyl-2,4-cyclohexanediamine (HTDA).

[0014] The solvent is one or more of DMF, DMSO, DMAC or NMP.

[0015] The aliphatic dibasic acid is one or more of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid or octadecanedioic acid.

[0016] The total number of moles of the diisocyanate is a, the total number of moles of the alicyclic diamine is b, the total number of moles of the aliphatic dibasic acid is c, and the parameter r is defined as:

[0017]

[0018] The value range of r is 0.95~1.05.

[0019] The catalyst is one or more of dibutyl phosphate, sodium hypophosphite, hypophosphorous acid, trimethyl phosphate, triphenyl phosphite or dibutyltin dilaurate; the amount of the catalyst is 0.05-0.2wt.‰ of the total weight of the polymerization monomer.

[0020] The antioxidant is one or more of antioxidant 1098, antioxidant 1096, antioxidant 1010, antioxidant 168, antioxidant BHT or phosphite; the amount of the antioxidant is 0.05-0.2wt.% of the total weight of the polymerized monomers.

[0021] In the step S1, the reaction temperature is 50-200° C. and the reaction time is 0.5-5 h; in the step S2, the stirring temperature is 50-100° C.; in the step S3, the polymerization temperature is 230-275° C. and the pressure is normal pressure.

[0022] The physically cross-linked transparent nylon is prepared by using the above-mentioned method for preparing physically cross-linked transparent nylon.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The physically cross-linked transparent nylon described in the present invention significantly enhances the interaction between molecules by introducing urea groups into the polyamide chain and utilizing the unique double hydrogen bonding effect of the urea groups, effectively restricting the thermal motion of the polymer chain, thereby greatly increasing the glass transition temperature of the material. This feature enables the material to maintain structural stability and mechanical properties at higher temperatures, broadening its application range in the high-temperature industrial field;

[0025] (2) The physically cross-linked transparent nylon of the present invention not only improves the heat resistance of the material through the formation of a physically cross-linked network, but also enhances the mechanical properties of the material such as tensile strength, modulus and toughness by restricting the movement of chain segments, so that the transparent nylon material exhibits better comprehensive performance when subjected to mechanical loads; by selecting aliphatic cyclic diamine as a preparation monomer, its unique cyclic structure hinders the crystallization of the material, so that the material can maintain a high degree of transparency;

[0026] (3) The physically cross-linked transparent nylon described in the present invention can achieve de-cross-linking of polymer chains by regulating the cross-linking structure, thereby giving the material good reprocessability and recycling capabilities, which is green and environmentally friendly;

[0027] (4) The preparation method of physically cross-linked transparent nylon described in the present invention has mild reaction conditions, is easy to control, and is convenient for industrial production. DETAILED DESCRIPTION

[0028] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0029] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.

[0030] Example 1

[0031] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0032] S1. In a nitrogen-protected glove box, 262.4 g (1 mol) of 4,4-diisocyanate dicyclohexylmethane, 2.1 kg (10 mol) of 4,4'-diaminodicyclohexylmethane and 500 mL of DMF were added to a reaction apparatus, and reacted at 150° C. for 3 h to generate an amino-terminated prepolymer;

[0033] S2, adding the amino-terminated prepolymer and 2.07 kg (9 mol) of dodecanedioic acid to 4.5 kg of deionized water, stirring at 80° C. to form a salt, to obtain a salt solution;

[0034] S3. Mix the salt solution, 0.44g of sodium hypophosphite and 4.4g of antioxidant 1098, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5MPa, maintain the pressure for 1h, then slowly release the pressure for 1.5h. After the pressure release is completed, further raise the temperature to 250°C, and react at normal pressure for 1h to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0035] Example 2

[0036] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0037] S1. In a nitrogen-protected glove box, 524.7 g (2 mol) of 4,4-diisocyanate dicyclohexylmethane, 2.1 kg (10 mol) of 4,4'-diaminodicyclohexylmethane and 600 mL of DMF were added to a reaction apparatus, and reacted at 180° C. for 4 h to generate an amino-terminated prepolymer;

[0038] S2, adding the amino-terminated prepolymer and 1.618 kg (8 mol) of sebacic acid to 4.2 kg of deionized water, stirring at 100° C. to form a salt to obtain a salt solution;

[0039] S3. Mix the salt solution, 0.4g hypophosphorous acid, 4.4g antioxidant 1098 and 1.46g antioxidant 168, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5MPa, maintain the pressure for 2h, then slowly release the pressure for 1.6h. After the pressure release is completed, further raise the temperature to 260°C, and carry out polymerization reaction at normal pressure for 1h to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0040] Example 3

[0041] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0042] S1. In a nitrogen-protected glove box, 250.3 g (1 mol) of 4,4'-diphenylmethane diisocyanate, 2.1 kg (10 mol) of 4,4'-diaminodicyclohexylmethane and 500 mL of DMAC were added to a reaction device, and reacted at 150° C. for 3 h to generate an amino-terminated prepolymer;

[0043] S2, adding the amino-terminated prepolymer and 2.325 kg (9 mol) of tetradecanedioic acid to 4.5 kg of deionized water, stirring at 50° C. to form a salt, to obtain a salt solution;

[0044] S3. Mix the salt solution, 0.44g of sodium hypophosphite and 4.4g of antioxidant 1098, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5MPa, maintain the pressure for 1h, then slowly release the pressure for 1.5h. After the pressure release is completed, further raise the temperature to 255°C, and carry out polymerization reaction at normal pressure for 50min to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0045] Example 4

[0046] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0047] S1. In a nitrogen-protected glove box, 336.38 g (2 mol) of hexamethylene diisocyanate, 2.1 kg (10 mol) of 4,4'-diaminodicyclohexylmethane and 700 mL of NMP were added to a reaction device, and reacted at 200° C. for 1 h to generate an amino-terminated prepolymer;

[0048] S2, adding the amino-terminated prepolymer and 1.84 kg (8 mol) of dodecanedioic acid to 4.3 kg of deionized water, stirring at 80° C. to form a salt, to obtain a salt solution;

[0049] S3. Mix the salt solution, 0.44 g of trimethyl phosphate and 4.4 g of antioxidant 1096, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5 MPa, maintain the pressure for 1 hour, then slowly release the pressure for 1.5 hours. After the pressure release is completed, further raise the temperature to 270°C, and carry out polymerization reaction at normal pressure for 1 hour to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0050] Example 5

[0051] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0052] S1. In a nitrogen-protected glove box, 250.3 g (1 mol) of 4,4'-diphenylmethane diisocyanate, 2.38 kg (10 mol) of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane and 600 mL of DMF were added to a reaction device, and reacted at 150° C. for 3 h to generate an amino-terminated prepolymer;

[0053] S2, adding the amino-terminated prepolymer and 2.07 kg (9 mol) of dodecanedioic acid to 4.5 kg of deionized water, stirring at 80° C. to form a salt, to obtain a salt solution;

[0054] S3. Mix the salt solution, 0.46g of dibutyl phosphate and 4.6g of antioxidant 1010, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5MPa, maintain the pressure for 1h, then slowly release the pressure for 1.5h. After the pressure release is completed, further raise the temperature to 265°C, and carry out polymerization reaction at normal pressure for 1.2h to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0055] Example 6

[0056] The preparation method of the physically cross-linked transparent nylon comprises the following steps:

[0057] S1. In a nitrogen-protected glove box, 500.5 g (2 mol) of 4,4'-diphenylmethane diisocyanate, 2.38 kg (10 mol) of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane and 700 mL of DMF were added to a reaction apparatus, and reacted at 165° C. for 3.5 h to generate an amino-terminated prepolymer;

[0058] S2, adding the amino-terminated prepolymer and 1.84 kg (8 mol) of dodecanedioic acid to 4.5 kg of deionized water, stirring at 80° C. to form a salt, to obtain a salt solution;

[0059] S3. Mix the salt solution, 0.47g of sodium hypophosphite and 4.7g of antioxidant 1098, and convey them to a polymerization kettle. Use inert gas to flush and exhaust for multiple times to evacuate the air in the polymerization kettle. Heat the polymerization kettle and start stirring. Raise the temperature to 220°C. When the pressure reaches 1.5MPa, maintain the pressure for 1h, then slowly release the pressure for 1.5h. After the pressure release is completed, further raise the temperature to 260°C, and carry out polymerization reaction at normal pressure for 1.1h to obtain a polymer melt. Cool the obtained polymer melt and cut it into pellets to obtain physically cross-linked transparent nylon.

[0060] Comparative Example 1

[0061] The difference from Example 1 is that there is no step S1, and step S2 is: add 2.1 kg (10 mol) of 4,4'-diaminodicyclohexylmethane and 2.3 kg (10 mol) of dodecanedioic acid into 4.4 kg of deionized water, stir at 80°C to form salt, and obtain a salt solution; the rest is the same as Example 1.

[0062] Comparative Example 2

[0063] The difference from Example 5 is that there is no step S1, and step S2 is: add 2.38 kg (10 mol) of 3,3'-dimethyl-4,4-diaminodicyclohexylmethane and 2.3 kg (10 mol) of dodecanedioic acid to 4.5 kg of deionized water, stir at 80° C. to form salt, and obtain a salt solution; the rest is the same as Example 5.

[0064] The performance tests were performed on the nylon prepared in Examples 1 to 6 and Comparative Examples 1 to 2, respectively, and the test methods were as follows:

[0065] Glass transition temperature (℃): The glass transition temperature (Tg) of nylon was tested using differential scanning calorimetry, where the heating and cooling rates were both 10℃ / min, and the purge gas and protective gas during the test were both nitrogen, with a purge gas rate of 20mL / min;

[0066] Tensile strength (MPa): Tested in accordance with GB / T 1040.1-2018;

[0067] Tensile modulus (MPa): Tested in accordance with GB / T 1040.1-2018;

[0068] Light transmittance (%): The sample to be tested was made into a disk with a diameter of 40 mm and a thickness of 2 mm, and its light transmittance was tested using a light transmittance tester.

[0069] The test results are shown in Table 1.

[0070] Table 1 Performance test results

[0071]

[0072] It can be seen from the test data in Table 1 that compared with Comparative Examples 1 and 2, the glass transition temperature of the nylon prepared in Examples 1 to 6 will be increased due to the addition of urea groups. This is because the physical crosslinking points formed by the double hydrogen bonding effect of the urea groups limit the movement of the molecular chain, and the more physical crosslinking points there are, the higher the glass transition temperature. In addition, the glass transition temperature of Example 3 is higher than that of Examples 1 and 2. This is because in addition to the hydrogen bonding effect, there is also a π-π conjugation effect of the benzene ring in Example 3, but this strong intermolecular force is easier to form crystals, so the transparency of the material will decrease. Since Examples 5 to 6 use 3,3'-dimethyl-4,4-diaminodicyclohexylmethane as a polymerization monomer, it has two more methyl groups than 4,4-diaminodicyclohexylmethane, and the presence of methyl side groups will further limit the movement of the aliphatic ring structure, so Examples 5 to 6 have a higher glass transition temperature than Examples 1 to 4.

Claims

1. A method for preparing physically cross-linked transparent nylon, characterized in that: The following steps are involved: S1, adding a diisocyanate and an alicyclic diamine in a molar ratio of (0.05-0.25):1 into a solvent for reaction to generate an amino-terminated prepolymer; S2, adding the amino-terminated prepolymer and the aliphatic dibasic acid into deionized water, stirring to obtain a salt solution; S3, mixing the salt solution, the catalyst and the antioxidant, raising the temperature to carry out polymerization reaction, and after the reaction is completed, cooling the obtained polymer melt and pelletizing to obtain physically cross-linked transparent nylon.

2. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The diisocyanate is one or more of hexamethylene diisocyanate, 4,4-diisocyanate dicyclohexylmethane, 4,4'-diphenylmethane diisocyanate, isophorone diisocyanate or naphthalene diisocyanate.

3. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The alicyclic diamine is one or more of 4,4'-diaminodicyclohexylmethane, isophoronediamine, 3,3'-dimethyl-4,4-diaminodicyclohexylmethane or 1-methyl-2,4-cyclohexanediamine.

4. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The solvent is one or more of DMF, DMSO, DMAC or NMP.

5. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The aliphatic dibasic acid is one or more of sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid or octadecanedioic acid.

6. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The total number of moles of the diisocyanate is a, the total number of moles of the alicyclic diamine is b, the total number of moles of the aliphatic dibasic acid is c, and the parameter r is defined as: The value range of r is 0.95~1.

05.

7. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The catalyst is one or more of dibutyl phosphate, sodium hypophosphite, hypophosphorous acid, trimethyl phosphate, triphenyl phosphite or dibutyltin dilaurate; the amount of the catalyst is 0.05-0.2wt.‰ of the total weight of the polymerization monomer.

8. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1098, antioxidant 1096, antioxidant 1010, antioxidant 168, antioxidant BHT or phosphite; the amount of the antioxidant is 0.05-0.2wt.% of the total weight of the polymerized monomers.

9. The method for preparing physically cross-linked transparent nylon according to claim 1, characterized in that: In the step S1, the reaction temperature is 50-200° C. and the reaction time is 0.5-5 h; in the step S2, the stirring temperature is 50-100° C.; in the step S3, the polymerization temperature is 230-275° C. and the pressure is normal pressure.

10. A physically cross-linked transparent nylon, characterized in that: The physically cross-linked transparent nylon is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Cited By

  • Polyamide-imide composite nanofiber and preparation method thereof

    CN119824566A

  • A polyamide-imide composite nanofiber and its preparation method

    CN119824566B

  • Resin composition, film, polarizing sheet, and sunglasses

    JP2026116283A

  • Resin composition, film, polarizing sheet, and sunglasses