A method for optimizing raw materials for aromatic hydrocarbon transalkylation reaction, and an aromatic hydrocarbon transalkylation reaction method and device

By optimizing the processing of raw materials before the aromatic alkyl group transfer reaction, and using a catalyst containing an oxide support and metal active component to remove impurities such as polycyclic aromatic hydrocarbons, the problems of reduced catalyst activity and high energy consumption in the aromatic hydrocarbon combined device are solved. The catalyst life is extended and the production efficiency is improved.

CN114436755BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202011116224.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-19
Publication Date
2024-11-01
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

In the existing aromatic hydrocarbon combined device, the substance and energy consumption of the aromatic hydrocarbon alkyl transfer unit is relatively high, and the catalyst activity is rapidly reduced, resulting in an increase in production costs and increased difficulty in device transformation, especially due to the influence of impurities in reforming oil, the catalyst is caused by the influence of impurities in the reforming oil. Carbon deposits and activity decrease.

Method used

Before the aromatic alkyl transfer reaction, the raw materials are optimized and the raw materials optimization catalysts containing oxide support, Group VIII metal active components and molecular sieve are used to remove polycyclic aromatic hydrocarbons, fused ring aromatic hydrocarbons and unsaturated aromatic hydrocarbons to prolong the catalyst to extend the catalyst Lifespan and reduce energy consumption.

Benefits of technology

Through the optimization of raw material treatment, the life of the alkyl transfer catalyst is significantly extended, material consumption and energy consumption are reduced, carbon deposits and activity of impurities on the catalyst are reduced, and the stability and production efficiency of the device are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114436755B_ABST
    Figure CN114436755B_ABST
Patent Text Reader

Abstract

The invention discloses an optimization method for an aromatic hydrocarbon alkylation feedstock, an aromatic hydrocarbon alkylation method and a device. The optimization method is performed before an aromatic hydrocarbon alkylation reaction, comprising: contacting the aromatic hydrocarbon alkylation feedstock with a feedstock optimization catalyst, and heating the feedstock at 1.0 to 6.0 MPa, 300 to 550° C., a hydrogen-to-hydrocarbon molar ratio of 1 to 20, and a feed weight space velocity of 1.0 to 40 h ‑1 The method for aromatic hydrocarbon transalkylation comprises: first optimizing the raw material by the optimization method, and then reacting in the presence of a transalkylation catalyst. The device comprises a reactor, in which a composite catalyst bed is arranged, and along the raw material feeding direction, the composite catalyst bed comprises a raw material optimization catalyst bed and a transalkylation catalyst bed. The present invention solves the problem of high impurities in the aromatic hydrocarbon transalkylation feed through a single reactor multi-bed fixed bed reaction process, and reduces the influence of impurities on the transalkylation catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to raw material optimization, and in particular to an optimization method for aromatic hydrocarbon alkyl transfer raw materials, an aromatic hydrocarbon alkyl transfer method and a device. Background Art

[0002] The aromatics complex is a core unit that produces paraxylene as the main product. It mainly uses straight-run naphtha as raw material and produces aromatic products such as benzene, paraxylene and o-xylene through catalytic reforming, aromatics extraction, xylene separation, disproportionation and aromatics transalkylation, adsorption separation and xylene isomerization. Among the many processes, catalytic reforming, as the leading unit, undertakes the function of manufacturing aromatics.

[0003] Catalytic reforming refers to the process in which the hydrocarbon molecules of C6-C9 naphtha fraction rearrange their structures under the action of reforming catalysts under certain conditions to produce new molecular structures, that is, to obtain high-octane gasoline and aromatics, and to produce hydrogen and liquefied petroleum gas as by-products. In order to obtain more aromatics and high-octane gasoline to meet market demand, reforming technology has been developed day by day, resulting in an increase in the severity of the reforming reaction and an increase in the content of inferior products in the reformed oil. The inferior products in the reformed oil enter the downstream units as raw material impurities in the aromatics conversion process.

[0004] The impurities in reforming oil are mainly olefins, diolefins, polycyclic aromatic hydrocarbons, and condensed aromatic hydrocarbons. Olefins can undergo polymerization and cyclization reactions on aromatic conversion catalysts to produce more condensed aromatic hydrocarbons. These polymers are adsorbed on the catalyst surface, and the catalyst is eventually deactivated by carbon deposition. In the transalkylation unit, more impurities can cause the rapid deactivation of the transalkylation catalyst and easily contaminate the heat exchange surface of the operating equipment, which will cause scaling in the feed heat exchanger and affect its heat exchange efficiency.

[0005] In a conventional aromatics complex, the aromatics raw materials generated by reforming are divided by a deheptanizer, the top component of the tower is extracted to remove non-aromatics, benzene or toluene, and the bottom component of the tower is separated by a bleaching clay tower and then enters a xylene tower. The C8A extracted from the top of the xylene tower enters a PX adsorption separation unit for separation. This process can effectively suppress the impurity content of the feed in the aromatics transalkylation unit and protect aromatics and transalkylation catalysts. However, due to the increasing requirements for environmental protection in recent years, the waste bleaching clay after the removal of impurities, especially olefins, is identified as hazardous waste, and the disposal volume and disposal fee of enterprises have greatly increased, and the cost remains high. In order to reduce the disposal volume and disposal fee, CN1282733C discloses a reforming oil selective hydrogenation deolefination catalyst, which contains 0.1-1.0wt% of precious metals and 0.05-0.50wt% of alkali metals or alkaline earth metals as additives. Under the conditions of hydrogenation, the reaction temperature is 150-250°C, the pressure is 1.5-3.0MPa, and the volume space velocity is 2.0-4.0h -1Under the above conditions, the olefin content in the product is greatly reduced, and the loss of aromatics is less than 0.5wt%. The deolefination catalyst is designed to ensure that the impurity content of the PX adsorption separation feed is qualified, and only the impurities of the C8 component are removed. Due to the limitations of the catalyst structure, the removal of impurities in components C9 and above and components C7 and below is not thorough, resulting in the subsequent entry of C9 heavy aromatics into the toluene disproportionation and aromatics alkyl transfer units, causing the catalyst to accelerate carbon deposition and rapidly decrease in activity. On the other hand, the presence of the deolefination unit increases energy and material consumption, which affects the production cost of the entire aromatics complex.

[0006] In recent years, with the breakthrough of key issues such as large-scale crystallization separation equipment, PX crystallization separation technology has developed rapidly. Due to the advantages of low energy consumption, simple operation, and stable products, crystallization separation has been more and more widely used and is one of the future development directions of PX separation technology. Since PX crystallization separation technology does not involve the use of adsorbents, it has no strict restrictions on impurities in the raw materials, especially components such as polycyclic aromatic hydrocarbons, olefins, and polycyclic aromatic hydrocarbons. Therefore, it is not necessary to process the reforming oil in the process, which can greatly reduce waste solid emissions. The untreated C9 + The impurity content in component A, especially the high olefin content, will accelerate the carbon deposition and deactivation of the catalyst. The existing major disproportionation catalysts at home and abroad have restrictions on the olefin content in the raw materials and are not suitable for directly treating C9 with high bromine index. + A Raw materials. Summary of the invention

[0007] In order to reduce the material and energy consumption of the aromatics transalkylation unit of an aromatics complex and to reduce the difficulty of transformation of existing devices, an optimization method and device for aromatics transalkylation feedstock are proposed without increasing the complexity of the process, wherein the raw materials are first optimized (impurity removal) before the aromatics transalkylation reaction. The raw material optimization can be used to solve the problem of high content of polycyclic aromatic hydrocarbons, heavy condensed aromatic hydrocarbons, unsaturated aromatic hydrocarbons and other impurities such as moisture and carbon oxides in the feed of the transalkylation reactor.

[0008] Specifically, the present invention mainly solves the problem of poor operating stability and short life of toluene transalkylation catalyst caused by the increased deterioration of raw materials in the transalkylation unit in the existing xylene production process. In the aromatics refining widely used in the latest generation of aromatics units, there is often a problem of high content of polycyclic aromatic hydrocarbons, heavy condensed aromatic hydrocarbons, unsaturated aromatic hydrocarbons and other impurities such as moisture and carbon oxides in the transalkylation raw materials. The material with a high impurity content often causes the catalyst activity to drop rapidly after entering the transalkylation.

[0009] One of the objects of the present invention is to provide a method for optimizing an aromatic transalkylation feedstock, which is carried out before the aromatic transalkylation reaction and comprises: contacting the aromatic transalkylation feedstock with a feedstock optimization catalyst, wherein the feedstock optimization catalyst comprises an oxide carrier, an active component and an optional molecular sieve.

[0010] In a preferred embodiment, the active component includes a first active component and a second active component, wherein the first active component is selected from at least one of Group VIII metals, and the second active component is selected from at least one of Group VIB, Group VB, Group VIIB, Group IIB and Group VA metals.

[0011] Wherein, the first active component and the second active component exist independently in at least one form of a simple substance, an oxide and a complex.

[0012] In a preferred embodiment, in the feedstock optimized catalyst, the first active component is selected from at least one of cobalt, nickel, palladium, platinum, rhodium and iridium.

[0013] In a further preferred embodiment, in the feedstock optimized catalyst, the first active component is selected from cobalt and / or nickel.

[0014] In a preferred embodiment, in the raw material optimized catalyst, the second active component is selected from at least one of zinc, rhenium, molybdenum, bismuth and chromium.

[0015] In a further preferred embodiment, in the raw material optimized catalyst, the second active component is selected from at least one of rhenium, molybdenum and bismuth.

[0016] In a further preferred embodiment, based on the mass of metal elements, the mass ratio of the first active component to the second active component is (0.01-40):1, preferably (0.1-20):1, and more preferably (0.1-10):1.

[0017] For example, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 8:1, 10:1, 15:1, 20:1, 30:1, etc.

[0018] In a preferred embodiment, the molecular sieve contains a maximum of 6-12 circular ring structures, preferably a maximum of 8-12 circular ring structures.

[0019] In a further preferred embodiment, in the raw material optimized catalyst, the molecular sieve is selected from at least one of MFI (ZMS-5) molecular sieve, FER molecular sieve, PTY molecular sieve, MEI molecular sieve, MEL molecular sieve (ZMS-11), MOR molecular sieve (mordenite), FAU molecular sieve (faujasite), STF molecular sieve, ITQ molecular sieve, BEA molecular sieve, MTW molecular sieve, MFI / MEL molecular sieve, MOR / MFI molecular sieve, MOR / MEL molecular sieve, MFI / FAU molecular sieve, BEA / MFI molecular sieve, and FAU / MEL molecular sieve.

[0020] In a further preferred embodiment, in the raw material optimized catalyst, the molecular sieve is a mixture of a molecular sieve containing a maximum of 8 to 10 circular ring structures and a molecular sieve containing a maximum of 12 circular ring structures.

[0021] Wherein, the topological structure of the molecular sieve is a single topological structure and / or a mixed topological structure.

[0022] In a further preferred embodiment, the mass ratio of the molecular sieve containing a maximum of 8-10 ring structures to the molecular sieve containing a maximum of 12 ring structures is (0.1-5):1, preferably (0.3-2):1, and more preferably (0.5-1):1.

[0023] In a preferred embodiment, in the feedstock optimized catalyst, the external specific surface area of ​​the molecular sieve is higher than 30 m 2 / g (preferably 50-300m 2 / g), pore volume of 0.15~0.5cm 3 / g, the percentage of micropores in the total pore volume is 50% to 90%, preferably 55 to 85%, and the micropores are 2nm.

[0024] In a preferred embodiment, in the raw material optimized catalyst, the carrier is selected from at least one of α-alumina, γ-alumina, silica, silica gel, and silicon carbide.

[0025] In a further preferred embodiment, the carrier is a calcined carrier.

[0026] In a further preferred embodiment, the calcination temperature is 350-900°C, preferably 500-800°C, more preferably 550-700°C; and / or the calcination time is 2-12h, preferably 2-12h, more preferably 4-10h.

[0027] Among them, pretreatment of the carrier can remove acidity, prevent and reduce carbon deposition, reduce carbon deposition, and extend the life of the carrier.

[0028] In a preferred embodiment, in the raw material optimized catalyst, the weight content of each component is as follows: 5-99% of the carrier, 0-90% of the molecular sieve, 0.05-20% of the first active component, and 0.05-30% of the second active component.

[0029] In a further preferred embodiment, in the raw material optimized catalyst, the weight content of each component is as follows: 10-95% of the carrier, 4-80% of the molecular sieve, 0.08-10% of the first active component, and 0.1-20% of the second active component.

[0030] In a preferred embodiment, the optimization of the aromatic hydrocarbon transalkylation feedstock is that the reaction pressure is 2.0-4.0 MPa, the reaction temperature is 340-450°C, the hydrogen-to-hydrocarbon molar ratio is 3-10, and the feed weight space velocity is 5-20 h -1 Next proceed.

[0031] Among them, in the process of raw material optimization, hydrocracking reaction of polycyclic aromatic hydrocarbons, hydrocracking reaction of condensed-ring heavy aromatic hydrocarbons, hydrocracking and / or cracking reaction of non-aromatic hydrocarbons, hydrogenation reaction of unsaturated aromatic hydrocarbons, etc. can occur simultaneously, which mainly involves the removal of polycyclic aromatic hydrocarbons, condensed-ring heavy aromatic hydrocarbons, non-aromatic hydrocarbons and unsaturated aromatic hydrocarbons, solves the problem of high impurities such as polycyclic aromatic hydrocarbons, condensed-ring heavy aromatic hydrocarbons, non-aromatic hydrocarbons and unsaturated aromatic hydrocarbons in the feed of aromatic alkyl transfer unit, reduces the influence of impurities on alkyl transfer catalyst, and achieves the goal of extending the life of alkyl transfer catalyst.

[0032] The second object of the present invention is to provide a method for aromatic hydrocarbon transalkylation, comprising: first optimizing the raw material using the optimization method described in one of the objects of the present invention, and then reacting in the presence of a transalkylation catalyst.

[0033] In a preferred embodiment, the reaction is carried out as follows: reaction pressure 1.0-6.0 MPa, reaction temperature 300-550°C, hydrogen-to-hydrocarbon molar ratio 1-20, feed weight space velocity 1.0-100 h -1 Next proceed.

[0034] In a further preferred embodiment, the reaction is carried out as follows: the reaction pressure is 2.0-4.0 MPa, the reaction temperature is 340-450°C, the hydrogen-to-hydrocarbon molar ratio is 3-10, and the feed weight space velocity is 5-20 h -1 Next proceed.

[0035] The third object of the present invention is to provide an aromatic hydrocarbon alkyl transfer device for carrying out the method described in the second object of the present invention, wherein the device includes a reactor in which a composite catalyst bed is arranged, wherein along the raw material feed direction, the composite catalyst bed includes a raw material optimized catalyst bed and an alkyl transfer catalyst bed.

[0036] Among them, it is preferred to load the composite catalyst bed in a conventional aromatics transalkylation reactor.

[0037] In a preferred embodiment, the raw material optimized catalyst comprises an oxide support, a first active component, a second active component and an optional molecular sieve, wherein the first active component is selected from at least one of Group VIII metals, and the second active component is selected from at least one of Group VIB, Group VB, Group VIIB, Group IIB and Group VA metals.

[0038] Wherein, the first active component and the second active component exist independently in at least one form of a simple substance, an oxide and a complex.

[0039] In a preferred embodiment, in the feedstock optimized catalyst, the first active component is selected from at least one of cobalt, nickel, palladium, platinum, rhodium and iridium.

[0040] In a further preferred embodiment, in the feedstock optimized catalyst, the first active component is selected from cobalt and / or nickel.

[0041] In a preferred embodiment, in the raw material optimized catalyst, the second active component is selected from at least one of zinc, rhenium, molybdenum, bismuth and chromium.

[0042] In a further preferred embodiment, in the raw material optimized catalyst, the second active component is selected from at least one of rhenium, molybdenum and bismuth.

[0043] In a preferred embodiment, the mass ratio of the first active component to the second active component is (0.01-40):1, preferably (0.1-20):1, more preferably (0.1-10):1, where the mass ratio is based on the mass of the metal.

[0044] In a preferred embodiment, in the raw material optimized catalyst, the molecular sieve is selected from at least one of MFI (ZMS-5) molecular sieve, FER molecular sieve, PTY molecular sieve, MEI molecular sieve, MEL molecular sieve (ZMS-11), MOR molecular sieve (mordenite), FAU molecular sieve (faujasite), STF molecular sieve, ITQ molecular sieve, BEA molecular sieve, MTW molecular sieve, MFI / MEL molecular sieve, MOR / MFI molecular sieve, MOR / MEL molecular sieve, MFI / FAU molecular sieve, BEA / MFI molecular sieve, and FAU / MEL molecular sieve.

[0045] In a further preferred embodiment, in the raw material optimized catalyst, the molecular sieve is a mixture of a molecular sieve containing a maximum of 8 to 10 circular ring structures and a molecular sieve containing a maximum of 12 circular ring structures.

[0046] Wherein, the topological structure of the molecular sieve is a single topological structure and / or a mixed topological structure.

[0047] In a further preferred embodiment, the mass ratio of the molecular sieve containing a maximum of 8-10 ring structures to the molecular sieve containing a maximum of 12 ring structures is (0.1-5):1, preferably (0.3-2):1, and more preferably (0.5-1):1.

[0048] In a preferred embodiment, in the feedstock optimized catalyst, the external specific surface area of ​​the molecular sieve is higher than 30 m 2 / g (preferably 50-300m 2 / g), pore volume of 0.15~0.5cm 3 / g, the percentage of micropores in the total pore volume is 50% to 90%, preferably 55 to 85%, and the micropores are 2nm.

[0049] In a preferred embodiment, in the raw material optimized catalyst, the carrier is selected from at least one of alumina, silica, α-alumina, γ-alumina, silica, silica gel, and silicon carbide.

[0050] In a further preferred embodiment, the carrier is a calcined carrier.

[0051] In a further preferred embodiment, the calcination temperature is 350-900°C, preferably 500-800°C, more preferably 550-700°C; and / or the calcination time is 2-12h, preferably 2-12h, more preferably 4-10h.

[0052] In a preferred embodiment, in the raw material optimized catalyst, the weight content of each component is as follows:

[0053] Carrier 5-99%;

[0054] Molecular sieve 0~90%;

[0055] The first active component 0.05-20%;

[0056] The second active component is 0.05-30%.

[0057] In a further preferred embodiment, in the raw material optimized catalyst, the weight content of each component is as follows:

[0058] Carrier 10-95%;

[0059] Molecular sieve 4~80%;

[0060] The first active component 0.08-10%;

[0061] The second active component is 0.1-20%.

[0062] Among them, when preparing the protected catalyst described in the present invention, the active components in the raw materials can basically be loaded onto the carrier and the molecular sieve. Therefore, the above content can be calculated based on the amount of raw materials used. Preferably, the above content is calculated based on the sum of the weight of the carrier + molecular sieve + active components as 100%.

[0063] The raw material optimized catalyst of the present invention can be prepared by using the catalyst preparation method disclosed in the prior art.

[0064] In a preferred embodiment, the composite catalyst bed comprises at least one feedstock optimized catalyst bed and at least one transalkylation catalyst bed.

[0065] The feedstock optimized catalyst bed refers to a bed filled with a feedstock optimized catalyst, and the transalkylation catalyst bed refers to a bed filled with a transalkylation catalyst.

[0066] In a further preferred embodiment, when the composite catalyst bed includes multiple feedstock optimized catalyst beds and multiple alkyl transalkylation catalyst beds, the feedstock optimized catalyst beds and the alkyl transalkylation catalyst beds are alternately arranged along the feedstock flow direction, and preferably the first bed is the feedstock optimized catalyst bed and the last bed is the alkyl transalkylation catalyst bed.

[0067] In this way, a feedstock optimized catalyst bed - an alkylation catalyst bed - a feedstock optimized catalyst bed - an alkylation catalyst bed ... are formed and this process is repeated.

[0068] Among them, the inventors found through a large number of experiments that when multiple beds are alternately arranged, the data reaction effect is better than that of a simple double-bed compound. This is because a small amount of impurities such as olefins will be produced during the main reaction (disproportionation). After multiple beds are alternately compounded, the impact is reduced, but the filling is complicated and not easy to be excessive. When side reactions are easily increased (such as benzene ring hydrogenation saturation), it is preferably a 4-6 bed compound (A+C+A+C+A+C) or (A+C+A+C).

[0069] In a preferred embodiment, the weight ratio of the feedstock optimized catalyst bed to the transalkylation catalyst bed is 1:50 to 10:1.

[0070] In a further preferred embodiment, the weight ratio of the feedstock optimized catalyst bed to the transalkylation catalyst bed is 1:20 to 1:1, preferably 1:20 to 1:5.

[0071] Among them, the amount of raw material optimization catalyst used is too much, the hydrogenation reaction is violent, and it is easy to cause excessive hydrogenation of the benzene ring, resulting in the main product of the alkyl transfer unit - benzene - The purity of the product does not meet the requirements. Therefore, the most preferred range is 1:20-1:5.

[0072] The weight of the feedstock optimized catalyst bed is calculated based on the total weight of the feedstock optimized catalyst in the composite catalyst bed, and the weight of the transalkylation catalyst bed is calculated based on the total weight of the transalkylation catalyst in the composite catalyst bed.

[0073] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0074] Compared with the prior art, the present invention has the following beneficial effects: the present invention solves the problem of high levels of impurities such as polycyclic aromatic hydrocarbons, condensed-ring heavy aromatic hydrocarbons, non-aromatic hydrocarbons and unsaturated aromatic hydrocarbons in the feed of the aromatic hydrocarbon alkyl transfer unit through a single-reactor multi-bed fixed bed reaction process, reduces the influence of impurities on the alkyl transfer catalyst, and achieves the goal of extending the life of the alkyl transfer catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 A schematic diagram showing the reaction device used in Example 3 (mainly showing the structure of the composite catalyst bed);

[0076] Figure 2 A schematic diagram of the reaction device used in Example 4 is shown (mainly showing the structure of the composite catalyst bed);

[0077] Figure 3 A schematic diagram showing the reaction device used in Example 5 (mainly showing the structure of the composite catalyst bed);

[0078] Figure 4 A schematic diagram showing the reaction device used in Example 6 (mainly showing the structure of the composite catalyst bed);

[0079] Figure 5 A schematic diagram of the reaction apparatus used in Example 7 is shown (mainly showing the structure of the composite catalyst bed therein).

[0080] A1 represents catalyst A1 obtained in Example 1; A2 represents catalyst A2 obtained in Example 1; A3 represents catalyst A3 obtained in Example 1; A4 represents catalyst A4 obtained in Example 1; A5 represents catalyst A5 obtained in Example 1; A6 represents catalyst A6 obtained in Example 1; C1 represents catalyst obtained in Example 2. DETAILED DESCRIPTION

[0081] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0082] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0083] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0084] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0085] The present invention analyzes the composition of the catalyst by ICP (inductively coupled plasma) and XRF (X-ray fluorescence) methods. The ICP test conditions are: Varian 700-ES series XPS instrument. The XRF test conditions are: Rigaku ZSX 100e XRF instrument.

[0086] The composition of the reaction raw materials and products of the present invention is determined by gas chromatography. The chromatographic model is Agilent 7890A, equipped with a FID detector with a hydrogen ion flame, and a FFAP capillary chromatographic column for separation. The chromatographic column adopts a programmed temperature increase, with an initial temperature of 90°C, maintained for 15 minutes, and then heated to 220°C at a rate of 15°C / min, and maintained for 45 minutes.

[0087] [Example 1] Preparation of raw material optimized catalyst

[0088] 1. After 41 g of alumina (calcined at 500° C. for 6 h) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 0.2) were uniformly mixed, 7.20 g of zinc chloride and 57.22 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding, calcining at 500° C. for 3 h, and reducing at 400° C. and 3 MPa for 4 h to obtain catalyst A1. The physical properties of the molecular sieve used are shown in Table 1, and the physical properties of the obtained catalyst are shown in Table 2.

[0089] 2. Add 25 g of aluminum oxide (calcined at 350°C for 12 h) and 70 g of silicon oxide, dissolve 11.21 g of nickel nitrate and 1.88 g of rhenium trichloride in a small amount of distilled water and add to the mixed powder, then add 5 g of sesbania powder and 10 mL of nitric acid solution, knead thoroughly and extrude into strips, calcine at 500°C for 3 hours, and then reduce at 400°C and 3 MPa for 4 hours to obtain catalyst A2. The catalyst properties are shown in Table 2.

[0090] 3. After 7 g of silicon oxide (calcined at 500° C. for 8 h) and 88 g of ammonium-type MOR / ZSM-11 (MOR / MEL structure, mass ratio 1 / 6) were mixed evenly, 0.50 g of palladium chloride and 9.20 g of ammonium heptamolybdate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding into strips, calcined at 500° C. for 3 h, and reduced at 400° C. and 3 MPa for 4 h to obtain catalyst A3. The physical properties of the molecular sieve used are shown in Table 1, and the physical properties of the obtained catalyst are shown in Table 2.

[0091] 4. Dissolve 1.33 g of chloroplatinic acid hexahydrate and 2.83 g of bismuth nitrate in a small amount of distilled water and add them to 98 g of alumina (calcined at 750°C for 2 h). Then add 5 g of sesbania powder and 10 mL of nitric acid solution, knead thoroughly and squeeze into strips. After calcining at 500°C for 3 hours, reduce at 400°C and 3 MPa for 4 hours to obtain catalyst A4. The catalyst properties are shown in Table 2.

[0092] 5. After 79.9 g of alumina (calcined at 600° C. for 3 h) and 10 g of ammonium ZSM-11 molecular sieve (MEL structure) were uniformly mixed, 18.39 g of ammonium heptamolybdate and 2.55 g of rhodium chloride were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution to fully knead and extrude strips. After calcination at 500° C. for 3 hours, the mixture was reduced at 400° C. and 3 MPa for 4 hours to obtain catalyst A5. The physical properties of the molecular sieve used are shown in Table 1, and the physical properties of the obtained catalyst are shown in Table 2.

[0093] 6. After 51 g of alumina (calcined at 550° C. for 3 h) and 45 g of ammonium FER / MTW molecular sieve (mass ratio 1 / 2) were uniformly mixed, 4.66 g of iridium chloride and 0.69 g of chromium nitrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding. After calcining at 500° C. for 3 h, the mixture was reduced at 400° C. and 3 MPa for 4 h to obtain catalyst A6. The physical properties of the molecular sieve used are shown in Table 1, and the physical properties of the obtained catalyst are shown in Table 2.

[0094] [Example 2] Preparation of transalkylation catalyst

[0095] After 45g of ammonium-type MOR molecular sieve and 60g of pseudo-boehmite are evenly mixed, 7g of ammonium heptamolybdate and 1g of nickel nitrate are dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 3g of sesbania powder and 10mL of nitric acid solution, kneading and extruding into strips, and calcining at 550°C for 4 hours to obtain catalyst number C1.

[0096] [Example 3]

[0097] Catalyst A1 obtained in Example 1 and catalyst C1 obtained in Example 2 were mixed according to Figure 1 The catalyst obtained in Example 1 is in the upper layer, and the catalyst obtained in Example 2 is in the lower layer. The amount of each catalyst is shown in Table 2.

[0098] Introducing the aromatic transalkylation feedstock Figure 1 The device with a composite catalyst bed is shown in the figure, and the reaction conditions are shown in Table 2. The reaction performance is shown in Table 3 and Table 4.

[0099] [Example 4]

[0100] Catalyst A2 obtained in Example 1 and catalyst C1 obtained in Example 2 were mixed according to Figure 2 The catalyst obtained in Example 1 is in the upper layer, and the catalyst obtained in Example 2 is in the lower layer. The amount of each catalyst is shown in Table 2.

[0101] Introducing the aromatic transalkylation feedstock Figure 2 The composite catalyst bed of the structure shown was used for the reaction, the conditions were as shown in Table 2, and the reaction performance was shown in Table 3 and Table 4.

[0102] [Example 5]

[0103] Catalyst A3 obtained in Example 1 and catalyst C1 obtained in Example 2 were mixed according to Figure 3 The catalyst obtained in Example 1 is in the upper layer, and the catalyst obtained in Example 2 is in the lower layer. The amount of each catalyst is shown in Table 2.

[0104] Introducing the aromatic transalkylation feedstock Figure 3 The composite catalyst bed of the structure shown was used for the reaction, the conditions were as shown in Table 2, and the reaction performance was shown in Table 3 and Table 4.

[0105] [Example 6]

[0106] Catalysts A4 and A5 obtained in Example 1 and catalyst C1 obtained in Example 2 were mixed according to Figure 4 The catalyst bed is filled in a structure of , wherein the catalyst bed has 4 layers, which are alternately filled in the order of A4, C1, A5, and C1. The amount of each catalyst is shown in Table 2.

[0107] Introducing the aromatic transalkylation feedstock Figure 4 The composite catalyst bed of the structure shown was used for the reaction, the conditions were as shown in Table 2, and the reaction performance was shown in Table 3 and Table 4.

[0108] [Example 7]

[0109] Catalysts A6, A5, A4, A3 obtained in Example 1 and catalyst C1 obtained in Example 2 were mixed according to Figure 5 The catalyst bed has 8 layers in total, which are alternately loaded in the order of A6, C1, A5, C1, A4, C1, A3, and C1. The amount of each catalyst is shown in Table 2.

[0110] Introducing the aromatic transalkylation feedstock Figure 5 The composite catalyst bed of the structure shown was used for the reaction, the conditions were as shown in Table 2, and the reaction performance was shown in Table 3 and Table 4.

[0111] [Comparative Example 1] Preparation of raw material optimized catalyst

[0112] 1. Inert alumina pellets were calcined at 500°C in air atmosphere for 6 h and then reduced at 400°C and 3 MPa for 4 h to obtain catalyst B1.

[0113] 2. After 41g of alumina (calcined at 500℃ for 6h) and 39g of ammonium-type SFN molecular sieve (mass ratio 0.2) were mixed evenly, 7.20g of zinc chloride and 57.22g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5g of sesbania powder and 10mL of nitric acid solution, kneading and extruding. After calcining at 500℃ for 3 hours, the mixture was reduced at 400℃ and 3MPa for 4 hours to obtain catalyst B2. The catalyst properties are shown in Table 2.

[0114] 3. After 41 g of alumina (untreated) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 0.2) were mixed evenly, 7.20 g of zinc chloride and 57.22 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding, calcining at 500 ° C for 3 hours, and then reducing at 400 ° C and 3 MPa for 4 hours to obtain catalyst B3. The catalyst properties are shown in Table 2.

[0115] 4. After 41 g of alumina (calcined at 500°C for 6 h) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 0.2) were mixed evenly, 7.20 g of zinc chloride and 0.95 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding into strips, calcined at 500°C for 3 h, and reduced at 400°C and 3 MPa for 4 h to obtain catalyst B4. The catalyst properties are shown in Table 2.

[0116] 5. After 41 g of alumina (calcined at 500°C for 6 h) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 0.2) were mixed evenly, 0.42 g of zinc chloride and 57.22 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding into strips, calcined at 500°C for 3 h, and reduced at 400°C and 3 MPa for 4 h to obtain catalyst B5. The catalyst properties are shown in Table 2.

[0117] 6. After 41 g of alumina (calcined at 500°C for 6 h) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 10) were mixed evenly, 7.20 g of zinc chloride and 57.22 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder, followed by adding 5 g of sesbania powder and 10 mL of nitric acid solution, kneading and extruding into strips, calcining at 500°C for 3 h, and reducing at 400°C and 3 MPa for 4 h to obtain catalyst B6. The catalyst properties are shown in Table 2.

[0118] 7. After uniformly mixing 41 g of alumina (calcined at 500° C. for 6 h) and 39 g of ammonium ZSM-5 / FAU molecular sieve (mass ratio 0.2, micropores accounting for 95% of total pores), 7.20 g of zinc chloride and 57.22 g of cobalt sulfate heptahydrate were dissolved in a small amount of distilled water and added to the mixed powder. Subsequently, 5 g of sesbania powder and 10 mL of nitric acid solution were added, kneaded thoroughly and extruded into strips. After calcining at 500° C. for 3 h, the catalyst B7 was reduced at 400° C. and 3 MPa for 4 h. The catalyst properties are shown in Table 2.

[0119] [Comparative Example 2]

[0120] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B1 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0121] [Comparative Example 3]

[0122] The process of Example 4 was repeated, except that the raw material optimized catalyst A2 was replaced by the catalyst B1 prepared in Comparative Example 1, the catalyst dosage and reaction conditions were shown in Table 2, and the reaction performance was shown in Tables 3 and 4.

[0123] [Comparative Example 4]

[0124] The process of Example 5 was repeated, except that the raw material optimized catalyst A3 was replaced by the catalyst B1 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0125] [Comparative Example 5]

[0126] The process of Example 6 was repeated, except that the raw material optimized catalysts A4 and A5 were replaced by the catalyst B1 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0127] [Comparative Example 6]

[0128] The process of Example 7 was repeated, except that the raw material optimized catalysts A6, A5, A4, and A3 were replaced by the catalyst B1 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0129] [Comparative Example 7]

[0130] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B2 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0131] [Comparative Example 8]

[0132] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B3 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0133] [Comparative Example 9]

[0134] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B4 prepared in Comparative Example 1, the catalyst dosage and reaction conditions were shown in Table 2, and the reaction performance was shown in Table 3 and Table 4.

[0135] [Comparative Example 10]

[0136] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B5 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0137] [Comparative Example 11]

[0138] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B6 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0139] [Comparative Example 12]

[0140] The process of Example 3 was repeated, except that the raw material optimized catalyst A1 was replaced by the catalyst B7 prepared in Comparative Example 1. The catalyst dosage and reaction conditions are shown in Table 2, and the reaction performance is shown in Table 3 and Table 4.

[0141] Table 1: Performance of molecular sieves used in various catalysts

[0142]

[0143]

[0144] Table 3:

[0145]

[0146]

[0147] Table 4: Catalyst performance at different sampling times

[0148]

[0149]

[0150] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A method for optimizing an aromatic transalkylation feedstock, the optimization method being performed before an aromatic transalkylation reaction, include: The aromatic hydrocarbon transalkylation feedstock is contacted with a feedstock optimization catalyst, wherein the feedstock optimization catalyst comprises an oxide carrier, an active component and a molecular sieve; the carrier is a calcined carrier; the molecular sieve is a mixture of a molecular sieve containing a maximum of 10-membered ring structure and a molecular sieve containing a maximum of 12-membered ring structure, and the mass ratio of the molecular sieve containing a maximum of 10-membered ring structure to the molecular sieve containing a maximum of 12-membered ring structure is (0.1-0.2):1; the external specific surface area of ​​the molecular sieve is higher than 30 m 2 / g, pore volume is 0.15~0.5 cm 3 / g, the percentage of micropores in the total pore volume is 50%~90%, and the micropores are 2nm; the active components include a first active component and a second active component, and the mass ratio of the first active component to the second active component is (0.1-40):1 in terms of the mass of the metal elements, the first active component is selected from at least one of cobalt, nickel, palladium, platinum, rhodium and iridium, and the second active component is selected from at least one of zinc, rhenium, molybdenum, bismuth and chromium; the carrier is selected from at least one of α-alumina, γ-alumina and silica.

2. The optimization method according to claim 1, It is characterized in that Calculated by the mass of metal elements, the mass ratio of the first active component to the second active component is (0.1-20):

1.

3. The optimization method according to claim 1, It is characterized in that In the feedstock optimized catalyst, The molecular sieve is at least one selected from MFI molecular sieve, MEI molecular sieve, MEL molecular sieve, MOR molecular sieve, FAU molecular sieve, STF molecular sieve, ITQ molecular sieve, BEA molecular sieve, MTW molecular sieve, MFI / MEL molecular sieve, MOR / MFI molecular sieve, MOR / MEL molecular sieve, MFI / FAU molecular sieve, BEA / MFI molecular sieve, and FAU / MEL molecular sieve.

4. The optimization method according to claim 1, It is characterized in that The calcination temperature is 350-900°C.

5. The optimization method according to claim 4, It is characterized in that The calcination temperature is 500-800°C.

6. The optimization method according to claim 1, It is characterized in that In the raw material optimized catalyst, the weight content of each component is as follows: 10-95% of the carrier, 4-80% of the molecular sieve, 0.08-10% of the first active component, and 0.1-20% of the second active component.

7. The optimization method according to any one of claims 1 to 6, It is characterized in that The optimization of the aromatic hydrocarbon transalkylation feedstock is that the reaction pressure is 2.0-4.0 MPa, the reaction temperature is 340-450°C, the hydrogen-to-hydrocarbon molar ratio is 3-10, and the feed weight space velocity is 5-20h -1 Next proceed.

8. A method for aromatic hydrocarbon transalkylation, include: The raw material is first optimized using the optimization method described in any one of claims 1 to 7, and then the reaction is carried out in the presence of a transalkylation catalyst.

9. The aromatic hydrocarbon transalkylation method according to claim 8, It is characterized in that The reaction is carried out as follows: reaction pressure 1.0-6.0 MPa, reaction temperature 300-550°C, hydrogen-to-hydrocarbon molar ratio 1-20, feed weight space velocity 1.0-100 h -1 The reaction was carried out below.

10. An aromatic hydrocarbon transalkylation device for carrying out the aromatic hydrocarbon transalkylation method according to claim 8 or 9, the device comprising a reactor, a composite catalyst bed being arranged in the reactor, in, Along the raw material feeding direction, the composite catalyst bed comprises a raw material optimized catalyst bed and an alkyl transfer catalyst bed; the raw material optimized catalyst comprises an oxide carrier, an active component and a molecular sieve; the carrier is a calcined carrier; the molecular sieve is a mixture of a molecular sieve containing a maximum of 10 circular ring structures and a molecular sieve containing a maximum of 12 circular ring structures, and the mass ratio of the molecular sieve containing a maximum of 10 circular ring structures to the molecular sieve containing a maximum of 12 circular ring structures is (0.1-0.2):1; the external specific surface area of ​​the molecular sieve is higher than 30 m 2 / g, pore volume is 0.15~0.5 cm 3 / g, the percentage of micropores in the total pore volume is 50%~90%, and the micropores are 2nm; the active components include a first active component and a second active component, and the mass ratio of the first active component to the second active component is (0.1-40):1 in terms of the mass of the metal elements, the first active component is selected from at least one of cobalt, nickel, palladium, platinum, rhodium and iridium, and the second active component is selected from at least one of zinc, rhenium, molybdenum, bismuth and chromium; the carrier is selected from at least one of α-alumina, γ-alumina and silica.

11. The aromatic hydrocarbon transalkylation unit according to claim 10, It is characterized in that The composite catalyst bed includes at least one feedstock optimized catalyst bed and at least one transalkylation catalyst bed.

12. The aromatic hydrocarbon transalkylation unit according to claim 11, It is characterized in that When the composite catalyst bed includes a plurality of feedstock optimized catalyst beds and a plurality of transalkylation catalyst beds, the feedstock optimized catalyst beds and the transalkylation catalyst beds are alternately arranged along the feedstock flow direction.

13. The aromatic hydrocarbon transalkylation unit according to claim 12, It is characterized in that The first bed is a feedstock optimized catalyst bed, and the last bed is a transalkylation catalyst bed.

14. The aromatic hydrocarbon transalkylation unit according to any one of claims 10 to 13, It is characterized in that The total weight usage ratio of the raw material optimized catalyst bed layer to the alkyl transfer catalyst bed layer is 1:50-10:

1.

15. The aromatic hydrocarbon transalkylation unit according to claim 14, It is characterized in that The total weight usage ratio of the raw material optimized catalyst bed layer to the alkyl transfer catalyst bed layer is 1:20 to 1:1.

Citation Information

Patent Citations

  • Cytalyst for reformed formation oil selective hydrogen removing olefin

    CN1282733C

  • Method for purifying supply flows containing aromates by means of zeolites

    CN101023049A

  • Catalyst for converting polycyclic aromatic hydrocarbons into monocyclic aromatic hydrocarbons to produce more dimethylbenzene and preparation method thereof

    CN103120956A

  • Method for converting polycyclic aromatic hydrocarbons into monocyclic aromatic hydrocarbons to produce more dimethylbenzene

    CN103121907A

  • Heavy aromatics light catalyst for high-yield production of xylene and preparation method of catalyst

    CN104549465A